ZnO / CdS heterojunction ultraviolet photoelectric detector and preparation method thereof
By growing ZnO/CdS heterojunction on the traditional ultraviolet detector substrate, the responsiveness and stability of the detector are improved by using hydrothermal method, solving the performance and cost of traditional detectors, and achieving efficient and environmentally friendly Ultraviolet light detection effect.
Patent Information
- Application Number
- CN202410875337.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-11-22
AI Technical Summary
Traditional ultraviolet detectors have problems such as small bandwidth, high cost, low sensitivity, large size and high energy consumption in terms of functions and performance, and it is difficult to meet the application needs in intelligent, multifunctional and harsh environments.
The ZnO seed crystal layer was grown on the substrate surface by hydrothermal method, and ZnO nanorods were formed by immersing a mixed solution containing zinc acetate, NaOH and PEG-1000, and then CdS particles were grown there to form ZnO/CdS heterojunction ultraviolet photoelectric detector.
It achieves high responsiveness, high sensitivity, rapid response and recovery time to ultraviolet light, with good stability and repeatability, while reducing the preparation cost and being highly environmentally friendly.
Smart Images

Figure CN119008766A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of detectors, and in particular relates to a ZnO / CdS heterojunction ultraviolet photoelectric detector and a preparation method thereof. Background Art
[0002] Ultraviolet detectors are electronic devices based on the photoelectric effect that can convert ultraviolet radiation into electrical signals, thereby realizing the detection of ultraviolet rays. At present, as a typical application of ultraviolet detection technology, ultraviolet detectors have shown market potential in the above-mentioned fields. With the growing demand of users, the functions and performance indicators of traditional ultraviolet detectors can no longer meet their application scenarios. In practical applications, new ultraviolet detectors with certain special functions or multi-functions are in increasing demand. For example, medical health, industrial facilities, environmental monitoring, and unmanned base stations are in urgent need of intelligent ultraviolet detectors that can work in harsh environments. Therefore, from the perspective of basic research and technological application, it is necessary to develop ultraviolet detectors with the characteristics of high stability, low cost, high sensitivity, high responsiveness, and short response time.
[0003] Traditional ultraviolet detectors are mainly made of Si and other conventional III-IV compounds. For example, the Chinese invention patent with application number 200910028977.3 discloses an Ag / silicon composite structure ultraviolet detector, which consists of an Ag film layer, a single crystal silicon substrate, and an ohmic contact metal electrode from top to bottom. The optical properties of the Ag film are combined with the Si single crystal substrate to achieve the photoelectric response of ultraviolet light. However, traditional ultraviolet detectors have the disadvantages of small bandgap, high cost, low detection sensitivity, large device size, and high energy consumption. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a ZnO / CdS heterojunction ultraviolet photodetector which exhibits excellent and stable photoelectric performance in the ultraviolet region and a preparation method thereof.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a ZnO / CdS (zinc oxide / cadmium sulfide) heterojunction ultraviolet photodetector, comprising the following steps:
[0006] S1: growing a ZnO seed layer on the substrate surface by a hydrothermal method;
[0007] S2: immersing the substrate on which the ZnO seed crystal layer is grown into a mixed solution containing zinc acetate, NaOH (sodium hydroxide) and PEG-1000 (polyethylene glycol 1000) for reaction to obtain a substrate on which ZnO nanorods are grown;
[0008] S3: placing the substrate on which the ZnO nanorods are grown into a mixed solution containing Cd(NO3)2 (cadmium nitrate), thiourea and CTAB (cetyltrimethylammonium bromide) for hydrothermal reaction to obtain a substrate on which a ZnO / CdS heterojunction is grown;
[0009] S4: Using the ZnO / CdS heterojunction as the working electrode, a ZnO / CdS heterojunction ultraviolet photodetector was prepared.
[0010] Another technical solution adopted by the present invention is: a ZnO / CdS heterojunction ultraviolet photodetector is prepared by adopting the above-mentioned preparation method of the ZnO / CdS heterojunction ultraviolet photodetector.
[0011] The beneficial effects of the present invention are as follows: the present invention synthesizes a ZnO / CdS heterojunction by a low-cost, green and environmentally friendly hydrothermal method, and prepares a ZnO / CdS heterojunction ultraviolet photodetector. In the ZnO / CdS heterojunction ultraviolet photodetector, granular CdS is coated on the surface of ZnO nanorods, which improves the performance of ZnO, achieves high responsiveness, high sensitivity, fast response and recovery time to ultraviolet light, and has good stability and repeatability. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 Shown is a flow chart of a method for preparing a ZnO / CdS heterojunction ultraviolet photodetector according to a specific embodiment of the present invention;
[0013] Figure 2 Shown are XRD patterns of ZnO NRAs and ZnO / CdS heterojunction in Example 1 of the present invention;
[0014] Figure 3 Shown is a SEM top view image of a ZnO / CdS heterojunction in Example 1 of the present invention;
[0015] Figure 4 Shown is a SEM cross-sectional image of a ZnO / CdS heterojunction in Example 1 of the present invention;
[0016] Figure 5 Shown is a histogram of the SEM top view image of the ZnO / CdS heterojunction in Example 1 of the present invention;
[0017] Figure 6 Shown is the EDX spectrum of the ZnO / CdS heterojunction in Example 1 of the present invention;
[0018] Figure 7 Shown is a TEM image of a ZnO / CdS heterojunction in Example 1 of the present invention;
[0019] Figure 8Shown is a HRTEM image of a ZnO / CdS heterojunction in Example 1 of the present invention;
[0020] Fig. 9 Shown is the full XPS spectrum of the ZnO / CdS heterojunction in Example 1 of the present invention;
[0021] Fig.10 Shown is a Zn 2p XPS spectrum of a ZnO / CdS heterojunction in Example 1 of the present invention;
[0022] Fig.11 Shown is the O1s XPS spectrum of the ZnO / CdS heterojunction in Example 1 of the present invention;
[0023] Fig.12 Shown is a Cd 3d XPS spectrum of a ZnO / CdS heterojunction in Example 1 of the present invention;
[0024] Fig.13 Shown is the S2p XPS spectrum of the ZnO / CdS heterojunction in Example 1 of the present invention;
[0025] Fig.14 Shown is the FTIR spectra of ZnO NRAs and ZnO / CdS nanocomposite materials in Example 1 of the present invention;
[0026] Fig.15 Shown is the UV-visible absorption spectrum of the ZnO / CdS heterojunction and ZnO NRAs in Example 1 of the present invention;
[0027] Fig.16 Shown is the Raman scattering spectrum of ZnO NRAs in Example 1 of the present invention;
[0028] Fig.17 Shown is the Raman scattering spectrum of the ZnO / CdS heterojunction in Example 1 of the present invention;
[0029] Fig.18 The figure shows the light efficiency test of ZnO NRAs UV photodetector, where (a) is 1.0~3.0mW / cm at 0V bias. 2 It curve within the range of light intensity, (b) is the relationship between light intensity and photocurrent, (c) is the relationship between light intensity and responsivity, and (d) is the relationship between light intensity and quantum efficiency;
[0030] Fig.19 The photoelectric efficiency test diagram of CdS NPs UV photodetector is shown in Figure 1, where (a) is 1.0-3.0 mW / cm at 0 V bias. 2It curve within the range of light intensity, (b) is the relationship between light intensity and photocurrent, (c) is the relationship between light intensity and responsivity, and (d) is the relationship between light intensity and quantum efficiency;
[0031] Fig. 20 The figure shows the light efficiency test diagram of the ZnO / CdS heterojunction ultraviolet photodetector in the first embodiment of the present invention, wherein (a) is 1.0-3.0 mW / cm at 0 V bias voltage. 2 It curve within the range of light intensity, (b) is the relationship between light intensity and photocurrent, (c) is the relationship between light intensity and responsivity, and (d) is the relationship between light intensity and quantum efficiency;
[0032] Fig.21 FIG. 1 is an IV curve diagram of the ZnO / CdS heterojunction ultraviolet photodetector in Example 1 of the present invention;
[0033] Fig. 22 It is a graph showing the It curve of the ZnO / CdS heterojunction ultraviolet photodetector under 365nm illumination at different bias voltages in Example 1 of the present invention;
[0034] Fig.23 The figure shows the rise and decay time of the ZnO / CdS heterojunction ultraviolet photodetector under 365nm light without bias according to the first embodiment of the present invention;
[0035] Fig.24 The figure shows the working mechanism of the ZnO / CdS heterojunction photodetector in the first embodiment of the present invention. DETAILED DESCRIPTION
[0036] In order to explain the technical content, achieved objectives and effects of the present invention in detail, the following is an explanation in combination with the implementation modes and the accompanying drawings.
[0037] Please refer to Figure 1 , a method for preparing a ZnO / CdS heterojunction ultraviolet photodetector, comprising the following steps:
[0038] S1: growing a ZnO seed layer on the substrate surface by a hydrothermal method;
[0039] S2: immersing the substrate on which the ZnO seed crystal layer is grown into a mixed solution containing zinc acetate, NaOH and PEG-1000 for reaction to obtain a substrate on which ZnO nanorods are grown;
[0040] S3: placing the substrate on which the ZnO nanorods are grown into a mixed solution containing Cd(NO3)2, thiourea and CTAB for hydrothermal reaction to obtain a substrate on which a ZnO / CdS heterojunction is grown;
[0041] S4: Using the ZnO / CdS heterojunction as the working electrode, a ZnO / CdS heterojunction ultraviolet photodetector was prepared.
[0042] From the above description, it can be seen that the beneficial effects of the present invention are: ZnO, as a typical wide bandgap semiconductor (Eg=3.37eV), has a large exciton binding energy, and has the advantages of being non-toxic and harmless, high thermal stability, high electron mobility, and low cost. It has a low growth temperature, does not require a complex preparation process, has strong radiation resistance, less pollution, and exhibits excellent and stable photoelectric properties in the ultraviolet light region.
[0043] The present invention forms a ZnO / CdS heterojunction by coating granular CdS on the surface of ZnO nanorods and growing them on a substrate, which has the following advantages: ① This heterojunction can effectively improve the band structure matching of ZnO materials, enhance the separation and transmission capabilities of carriers, and thus improve the photoelectric conversion efficiency; ② The coating of CdS particles can effectively reduce the defects and dangling bonds on the surface of ZnO nanorods, and reduce the interface recombination rate, which helps to reduce the loss of carriers, improve the photoelectric conversion efficiency and the stability of the detector; ③ Under illumination conditions, the ZnO / CdS heterojunction will generate photogenerated electrons and holes; due to the presence of the heterojunction, the separation and transmission efficiency of photogenerated electrons and holes is improved, thereby enhancing the photoconductivity effect. This helps to improve the sensitivity and response speed of the detector. The ultraviolet photodetector prepared by the present invention can work without the need for an external power supply, and achieves high responsiveness, high sensitivity, fast response and recovery time to ultraviolet light, and has good stability and repeatability.
[0044] The present invention adopts a hydrothermal method to prepare a ZnO / CdS heterojunction, which has the following advantages: (1) The hydrothermal method can prepare ZnO / CdS at a lower temperature, saving energy. (2) During the hydrothermal reaction, the material fully reacts under high pressure and high temperature conditions, which is conducive to the uniform mixing and crystallization of atoms or molecules, thereby obtaining a high-purity, high-crystallinity ZnO / CdS material with good physical and chemical properties. (3) The hydrothermal method can accurately control the crystal structure and morphology of ZnO / CdS by adjusting reaction conditions, such as temperature, reaction time, etc., to achieve optimization of material properties. (4) The equipment required for the hydrothermal method is relatively simple and the operation is relatively convenient. (5) The hydrothermal method usually uses an aqueous solution as a reaction medium, which reduces the use of organic solvents, thereby reducing the risk of environmental pollution; in addition, the reaction process of the hydrothermal method is relatively mild, and does not generate a large amount of waste gas, wastewater and solid waste, which is beneficial to environmental protection.
[0045] The present invention uses polyethylene glycol (PEG-1000) with a specific molecular weight to prepare ZnO nanorods. Polyethylene glycols with other molecular weights cannot grow the desired ZnO nanorods: ZnO cannot be grown on FTO using PEG-600, and ZnO grown on FTO using PEG-2000 is too thick, resulting in very low or no photoelectric performance.
[0046] Further, S1 is specifically as follows: dripping zinc acetate-ethanol solution on the surface of the substrate, rinsing it with anhydrous ethanol after 8 to 12 seconds, and then blowing away the anhydrous ethanol with nitrogen to complete a cycle; after repeating the cycle 8 to 10 times, drying the substrate to obtain a substrate with a ZnO seed crystal layer grown thereon.
[0047] Furthermore, the substrate is a FTO (highly conductive fluorine-doped tin oxide) substrate.
[0048] Furthermore, before growing the ZnO seed crystal layer, the substrate needs to be ultrasonically cleaned using acetone, anhydrous ethanol and deionized water in sequence.
[0049] Furthermore, the concentration of the zinc acetate-ethanol solution is 0.01-0.03M.
[0050] From the above description, it can be seen that changes in the concentration of raw materials will lead to different thicknesses of the materials grown on FTO, which will also affect various parameters of the optoelectronic performance.
[0051] Furthermore, the drying step is specifically as follows: keeping the temperature at 220-270° C. for 25-35 minutes, cooling to room temperature and then drying naturally in the air.
[0052] From the above description, it can be seen that the drying step of the present invention can promote the crystallization and growth of ZnO, remove residual moisture and impurities, enhance the bonding force between the seed layer and the substrate, optimize the performance of the seed layer, and ensure the stability of the cooling process. It is helpful to improve the quality of the ZnO seed layer, and then improve the performance of the constructed optoelectronic device.
[0053] Furthermore, the mixed solution in S2 is prepared by dissolving 0.01-0.03M zinc acetate, 0.2-0.4M NaOH and 0.01-0.03M PEG-1000 in deionized water, and stirring for 25-35 minutes to form a mixed solution.
[0054] Furthermore, the reaction conditions in S2 are: keeping warm at 150-170° C. for 8-12 hours under sealed conditions.
[0055] Furthermore, the mixed solution in S3 is prepared by dissolving 0.01-0.03M cadmium nitrate, 0.03-0.04M thiourea and 0.01-0.03M CTAB in deionized water, and stirring for 25-35 minutes to form a mixed solution.
[0056] Furthermore, the reaction conditions of the hydrothermal reaction in S3 are: keeping warm at 150-170° C. for 8-12 hours.
[0057] Furthermore, S4 is specifically as follows: placing the substrate on which the ZnO / CdS heterojunction is grown in an electrolyte, and adopting a three-electrode system of a working electrode, a counter electrode, and a reference electrode to prepare a ZnO / CdS heterojunction ultraviolet photodetector.
[0058] Furthermore, the counter electrode is a Pt mesh electrode, the reference electrode is a calomel electrode, and the electrolyte is a Na2SO4 aqueous solution.
[0059] From the above description, we can know that the Pt mesh electrode: has excellent conductivity, which enables the platinum mesh electrode to provide a stable electrical signal to ensure the stability of the electrochemical reaction; it also has high corrosion resistance and a long service life, reducing maintenance costs. Calomel reference electrode: has high electrochemical activity and can catalyze many electrochemical reactions. Na2SO4 aqueous solution: mainly plays the role of conducting ions, participates in various chemical reactions in the battery, and promotes the redox reaction on the positive and negative electrodes.
[0060] Another technical solution adopted by the present invention is: a ZnO / CdS heterojunction ultraviolet photodetector is prepared by adopting the above-mentioned preparation method of the ZnO / CdS heterojunction ultraviolet photodetector.
[0061] From the above description, it can be seen that the ZnO / CdS heterojunction ultraviolet photodetector made by the present invention has a good response to ultraviolet light. Under the condition of 365nm ultraviolet irradiation and 0V bias voltage, when the light intensity is 3mW / cm 2 When the ZnO / CdS heterojunction UV detector is used, the Iphoto / Idark ratio is 17.17, the photoresponsivity is 33.35 mA / W, the external quantum efficiency is 11.33%, the response speed rise time is 0.12 s, the decay time is 0.15 s, and the response time is short.
[0062] Please refer to Figure 1 Embodiment 1 of the present invention is: a method for preparing a ZnO / CdS heterojunction ultraviolet photodetector, comprising the following steps:
[0063] S1: The FTO substrate was ultrasonically cleaned with acetone, anhydrous ethanol and deionized water for 10 min in sequence, and then dried with nitrogen.
[0064] S2: Use a dropper to drop 0.02M zinc acetate-ethanol solution on the surface of the FTO substrate, rinse it with anhydrous ethanol after 10 seconds, and then blow away the anhydrous ethanol with nitrogen to complete a cycle; after repeating 9 cycles, put the substrate into a drying oven, keep it at 250°C for 30 minutes, cool it to room temperature and dry it naturally in the air to obtain a FTO substrate with a ZnO seed layer grown on it.
[0065] S3: 0.02M zinc acetate, 0.3M NaOH and 0.02M PEG-1000 were dissolved in deionized water and magnetically stirred for 30 minutes to form a mixed solution; the mixed solution was poured into the inner lining of a 100mL stainless steel autoclave, and then the FTO substrate with the ZnO seed layer grown was vertically placed therein, the autoclave was sealed and kept warm at 160°C for 10 hours, and then naturally dried after being taken out to obtain the FTO substrate with ZnO nanorods grown thereon.
[0066] S4: 0.02M cadmium nitrate, 0.032M thiourea and 0.02M CTAB were dissolved in deionized water and magnetically stirred for 30 minutes to form a mixed solution; the FTO substrate grown with ZnO nanorods was placed in a reactor containing the mixed solution, and the mixture was kept at 160°C for 10 hours for hydrothermal reaction. After cooling to room temperature, the mixture was naturally dried in air to obtain a FTO substrate grown with a ZnO / CdS heterojunction.
[0067] S5: The FTO substrate with the ZnO / CdS heterojunction grown thereon is placed in an electrolyte, and a ZnO / CdS heterojunction ultraviolet photodetector is prepared using a three-electrode system of a working electrode, a counter electrode, and a reference electrode; the counter electrode is a Pt mesh electrode, the reference electrode is a calomel electrode, and the electrolyte is a 0.5 mol / L Na2SO4 aqueous solution.
[0068] The FTO substrate with ZnO NRAs (zinc oxide nanorod arrays), the FTO substrate with ZnO / CdS heterojunction, and the ZnO / CdS heterojunction ultraviolet photodetector sample prepared in Example 1 were tested, and the test results are as follows:
[0069] 1. Detect the XRD patterns of ZnO NRAs (zinc oxide nanorod arrays) and ZnO / CdS heterojunctions at 160°C for 10 h. Figure 2 . Figure 2The presence of CdS can be observed at the two diffraction peaks of 44.1° and 51.9°, which correspond to the (102) and (110) crystal planes respectively; the diffraction peak of ZnO (-210) crystal plane disappears at 22.2°, and the diffraction peaks of ZnO (100), (002) and (101) crystal planes at 31.7°, 34.4° and 36.2° are all weakened, which indicates that the ZnO content is low and the crystallization quality of the ZnO / CdS heterojunction is good.
[0070] 2. Use SEM to detect the morphological characteristics of the samples. The test results are shown in Figures 3 to 5 . Figure 3 and Figure 4 The SEM top view and SEM cross-sectional view of the ZnO / CdS heterojunction are shown, which clearly shows that CdS NPs (cadmium sulfide nanoparticles) are densely grown on ZnO NRAs, where the average diameter length and thickness of CdS NPs are 182.18±48.74nm and 1.765μm, respectively. ZnO NRAs are densely grown on the FTO glass substrate, and CdS NPs and ZnO NRAs have good contact. Figure 5 Reflects the average diameter length of CdS NPs.
[0071] 3. Study on the elemental composition of ZnO / CdS heterojunction using EDX spectrometer Figure 6 . Figure 6 Strong peaks of Cd and S elements are shown. The relative atomic mass of Cd is 69.723, and the relative atomic mass of O is 16. The weight percentages of Cd and S in the sample are 79.1% and 18.4%, respectively. The result is close to the standard ratio Cd:S=1:1, further confirming the successful synthesis of ZnO / CdSNRAs. Through the above material characterization, it can be confirmed that after a hydrothermal reaction at 160°C for 10h, CdS NPs can be successfully grown on ZnO NRAs to obtain a ZnO / CdS heterojunction.
[0072] 4. TEM was used to study the ZnO / CdS heterojunction, see Figure 7 . Figure 7 The complete morphology of a single ZnO / CdS heterojunction is shown, further confirming the formation of the ZnO / CdS heterojunction, which is consistent with the SEM image results.
[0073] 5. HRTEM was used to study the ZnO / CdS heterojunction, see Figure 8 , Figure 8It shows that the lattice fringe spacing of ZnO is 0.260nm, which can correspond to the (002) crystal plane of ZnO; the lattice fringe spacing of CdS is 0.354nm, which can correspond to the (110) crystal plane of CdS; the above results further confirm the successful synthesis of ZnO / CdS heterojunction.
[0074] 6. XPS spectrum test of ZnO / CdS heterojunction is carried out. The test results are shown in Figures 9 to 13 ,in Fig. 9 This is the full spectrum of the ZnO / CdS heterojunction. Fig.10 is the Zn 2p spectrum of ZnO / CdS heterojunction, Fig.11 This is the O1s spectrum of the ZnO / CdS heterojunction. Fig.12 Cd 3d spectrum of ZnO / CdS heterojunction. Fig.13 This is the S2p spectrum of the ZnO / CdS heterojunction. Fig. 9 It can be seen that the samples prepared in the experiment contain four elements: Zn, O, Cd and S. Fig.10 The positions of the middle signal peaks are 1021.2eV and 1044.5eV, corresponding to Zn3 / 2 and Zn1 / 2, respectively, indicating that Zn exists in a positive divalent state. Fig.11 The O1s signal peak is 532.5 eV, which is consistent with the lattice oxygen O 2- correspond. Fig.12 The signal peaks are located at 404.95 eV and 411.65 eV, which are consistent with the Cd 2+ Very consistent. Fig.13 The signal peak of S2p is 161.8eV, corresponding to S2-. The above results show that the ZnO / CdS sample is composed of Zn 2+ , O 2- 、Cd 2+ and S 2- The composition, namely containing ZnO and CdS, further proves that the ZnO / CdS heterojunction has been prepared.
[0075] 7. The ZnO / CdS heterojunction and ZnO NRAs were analyzed by infrared spectrometer. The analysis results are shown in Fig.14 .Depend on Fig.14 It can be seen that the ZnO / CdS heterojunction has a good correspondence with the ZnO absorption peak, indicating that the ZnO / CdS heterojunction sample contains ZnO components. At the same time, a new absorption peak is formed in the infrared spectrum of the ZnO / CdS heterojunction at 755.39 cm -1 、871.42cm -1 、2923.14cm -1The absorption peak caused by the stretching vibration of hydroxyl groups appeared at the ZnO / CdS heterojunction. The research shows that the above phenomena are closely related to the CdS component. Infrared analysis shows that there are ZnO and CdS with complete phase structures in the ZnO / CdS heterojunction, and there is an obvious chemical interaction between the two.
[0076] 8. Fig.15 UV-visible absorption spectra of ZnO / CdS heterojunction and ZnO NRAs. Fig.15 The absorption edge of the ZnO / CdS heterojunction is at about 537nm. Fig.15 The illustration in the figure uses the formula (αhv)2=A(hv-Eg) to calculate the optical band gap of the ZnO / CdS heterojunction. It can be seen that the absorption edge of the ZnO / CdS heterojunction is about 537nm, the band gap is about 2.31eV, and the ZnO / CdS composite broadens the wavelength range.
[0077] 9. The resonant Raman scattering spectra of ZnO NRAs and ZnO / CdS heterojunctions were analyzed at an excitation wavelength of 325 nm. Fig.16 and 17 .from Fig.17 It can be seen that the prepared ZnO / CdS heterojunctions are all at 294.68 cm -1 、1591.05cm -1 、2836.74cm -1 The resonant Raman vibration peaks observed at 368.45 cm-1 and 368.45 cm-2 can be observed from the figure, and the peak spacing is almost equal. These Raman peaks originate from the first, second, and third order longitudinal optical phonon (LO) vibration modes of CdS. In addition, it can be observed from the figure that the sample has a resonant Raman vibration peak at 368.45 cm-1. -1 There is a weak 1LO phonon peak of ZnO at the reaction time, indicating that the ZnO / CdS heterojunction at this reaction time has the resonant Raman phonon peaks of both ZnO and CdS. These Raman peaks are significantly resonantly enhanced under 325nm excitation, which comes from the electron phonon Interaction. The lattice mismatch and strain between ZnO and CdS lead to quantum confinement and binding of electrons and holes at the interface. This quantum confinement and binding may lead to the existence of a local band structure at the interface, resulting in bound states, affecting the interaction between phonons and carriers, and thus affecting the lifetime and intensity of phonons.
[0078] 10. Use ZnO NRAs and CdS NPs as working electrodes to prepare ZnO NRAs UV photodetectors and CdS NPs UV photodetectors respectively; test the ZnO NRAs UV photodetector at 0V bias voltage of 1.0-3.0mW / cm 2It curve within the light intensity range (a), the relationship between light intensity and photocurrent (b), the relationship between light intensity and responsivity (c), and the relationship between light intensity and quantum efficiency (d). The test results are shown in Fig.18 ; Test CdS NPs UV photodetector at 0V bias 1.0~3.0mW / cm 2 The It curve within the light intensity range (a), the relationship between light intensity and photocurrent (b), the relationship between light intensity and responsivity (c), and the relationship between light intensity and quantum efficiency (d) are shown in the test results. Fig.19 ; Test the ZnO / CdS heterojunction UV photodetector of Example 1 at 0V bias 1.0~3.0mW / cm 2 The It curve within the light intensity range (a), the relationship between light intensity and photocurrent (b), the relationship between light intensity and responsivity (c), and the relationship between light intensity and quantum efficiency (d) are shown in the test results. Fig. 20 .
[0079] Fig.18 The photocurrent density of ZnO NRAs increases with the increase of power intensity. 2 When the photocurrent density reaches 27.3μA / cm 2 , the dark current density at this time is -2.77μA / cm 2 ;exist Fig.19 In the experiment, the photocurrent density of CdS NPs increased with the increase of power intensity. 2 When the photocurrent density reaches 79.4μA / cm 2 , the dark current density at this time is -0.39μA / cm 2 ;exist Fig. 20 In the ZnO / CdS heterojunction, the photocurrent density increases with the increase of power intensity. 2 When the photocurrent density reaches 101μA / cm 2 , the dark current density at this time is -0.06μA / cm 2 According to the photogenerated process, this increase in photoresponse is due to the increase in light power generating more photogenerated electron-hole pairs, thereby generating a larger photocurrent. The above results show that the material prepared by the present invention can immediately respond to the optical switch transition and generate a corresponding current, showing that the device has good sensitivity and repeatability.
[0080] In addition, two basic indicators for measuring performance are photoresponsivity (R) and external quantum efficiency (EQE). R is the photocurrent generated by unit power incident light on the effective area, and EQE is the ratio of electron-hole pair conversion efficiency. R is defined as R = (Iphoto-Idark) / (PS), where Iphoto is the photocurrent, Idark is the dark current, P is the light intensity, and S is the effective irradiated area. The equation EQE = (Rhc) / eλ is used to define EQE, where R is the responsivity, h is Planck's constant, c is the speed of light, e is the electron charge, and λ is the wavelength of the irradiated light. By Figures 18 to 20 It can be seen that at a wavelength of 365nm and a light intensity of 3mW / cm 2 Under ultraviolet light irradiation with a bias voltage of 0 V, the R and EQE of ZnO NRAs were calculated to be 9.92 mA / W and 3.37%, respectively, the R and EQE of CdS NPs were calculated to be 26.80 mA / W and 9.10%, respectively, and the R and EQE of ZnO / CdS heterojunction were calculated to be 33.35 mA / W and 11.33%, respectively, showing excellent detection capabilities.
[0081] 11. Fig.21 The IV curve of the ZnO / CdS heterojunction UV photodetector shows that the light intensity increases from 1.0 to 3.0 mW / cm at a bias voltage of 0 V. 2 , the photocurrent density of the ZnO / CdS heterojunction photodetector increased from -46.71 to 92.89μA / cm2. The dark current density of the ZnO / CdS heterojunction photodetector at 0V bias is 21.4μA / cm 2 . Under 365nm illumination and 3.0mW / cm 2 Under high light intensity, the photocurrent / dark current ratio (Iphoto / Idark) of the ZnO / CdS heterojunction photodetector is 7.25, which indicates that the ZnO / CdS heterojunction photodetector has high sensitivity to ultraviolet light and good signal recognition ability, and not only has a strong photoresponse, but also has obvious rectification characteristics.
[0082] 12. In addition to strong light, the photoresponse is also affected by the applied bias voltage. The It curves of the ZnO / CdS heterojunction UV photodetector under 365nm light with different applied bias voltages are tested, such as Fig. 22 shown. Fig. 22 At a wavelength of 365nm and a light intensity of 1mW / cm 2 When the bias voltage increases from -0.4V to 0.4V under ultraviolet light, the photocurrent density increases from 12.42μA / cm 2 Increased to 28.6μA / cm 2The photocurrent density at 0.4 V is 2.30 times that at -0.4 V, which is due to the enhanced drift velocity of photogenerated carriers and the increased probability of electron-hole pair separation and acceleration.
[0083] 13. Test the rise and decay time of the ZnO / CdS heterojunction UV photodetector without bias under 365nm illumination. See the test results. Fig.23 . Fig.23 At a wavelength of 365nm and a light intensity of 1mW / cm 2 The response speed of the ZnO / CdS heterojunction photodetector was measured under ultraviolet light irradiation with a bias voltage of 0V. The rise time is defined as the time for the maximum photocurrent to increase from 10% to 90%, and the decay time is defined as the time for the maximum photocurrent to decrease from 90% to 10%. Fig.23 As shown, under 365nm UV irradiation, the rise time is 0.12s and the decay time is 0.15s. This remarkable performance may be due to the increase in the contact area between the semiconductor material and the electrolyte environment, which leads to the expansion of the solid / liquid heterojunction interface, resulting in the accelerated separation of photogenerated carriers. In addition, the nanorod array with high crystal quality provides a fast photogenerated carrier transmission channel to improve the light collection efficiency.
[0084] 14. Fig.24 The working mechanism diagram of the ZnO / CdS heterojunction photodetector is shown to explain its self-powered characteristics and superior photoelectric performance. Under ultraviolet light irradiation, the electrons in the valence bands of ZnO and CdS absorb the energy of the corresponding photons and transition to the valence band, generating photogenerated electron-hole pairs in both ZnO and CdS. The conduction band and valence band potentials of CdS are lower than those of ZnO. After the two combine to form a type II band structure, the electrons in the conduction band of CdS will migrate to the conduction band of ZnO, and the holes in the valence band of ZnO will migrate to the valence band of CdS, achieving rapid separation of photogenerated electrons and holes. The holes accumulated in the valence band of CdS migrate to the surface of CdS, oxidizing S2- in the polysulfide electrolyte to S element, which then further reacts with S to generate S (where x = 2, 3, 4, 5).
[0085] The electrons in the conduction band of ZnO diffuse to the FTO substrate and reach the S reaction of the counter electrode through the external circuit to generate S2- and S again. In this cycle, the S2- / S redox pair in the polysulfide electrolyte can be repeatedly consumed and regenerated and reused. At the same time, since the electrons transmitted to the counter electrode are consumed without aggregation, the photogenerated electrons can continue to reach the counter electrode through the external circuit, so that a photocurrent will be generated in the external circuit. When the ultraviolet light is turned off, neither ZnO nor CdS can generate photogenerated electrons and holes, and the previously generated electrons and holes will react with the electrolyte and be gradually consumed, that is, the photocurrent decreases rapidly and returns to the initial state, and then re-enters the next cycle after the light is restored.
[0086] The second embodiment of the present invention is: a ZnO / CdS heterojunction ultraviolet photodetector, which is prepared by the preparation method of the ZnO / CdS heterojunction ultraviolet photodetector of the first embodiment.
[0087] Embodiment 3 of the present invention is: a method for preparing a ZnO / CdS heterojunction ultraviolet photodetector, comprising the following steps:
[0088] S1: The FTO substrate was ultrasonically cleaned with acetone, anhydrous ethanol and deionized water for 10 min in sequence, and then dried with nitrogen.
[0089] S2: Use a dropper to drop 0.01M zinc acetate-ethanol solution on the surface of the FTO substrate, rinse it with anhydrous ethanol after 8 seconds, and then blow away the anhydrous ethanol with nitrogen to complete a cycle; after repeating 8 cycles, put the substrate into a drying oven, keep it at 220°C for 35 minutes, cool it to room temperature and dry it naturally in the air to obtain a FTO substrate with a ZnO seed layer grown on it.
[0090] S3: 0.01M zinc acetate, 0.2M NaOH and 0.01M PEG-1000 were dissolved in deionized water and magnetically stirred for 25 minutes to form a mixed solution; the mixed solution was poured into the lining of a 100mL stainless steel autoclave, and then the FTO substrate with the ZnO seed layer grown was vertically placed therein, the autoclave was sealed and kept warm at 150°C for 12 hours, and then naturally dried after being taken out to obtain the FTO substrate with ZnO nanorods grown thereon.
[0091] S4: 0.01M cadmium nitrate, 0.03M thiourea and 0.01M CTAB were dissolved in deionized water and magnetically stirred for 25 minutes to form a mixed solution; the FTO substrate grown with ZnO nanorods was placed in a reactor containing the mixed solution, and the mixture was kept at 150°C for 12 hours for hydrothermal reaction. After cooling to room temperature, the mixture was naturally dried in air to obtain a FTO substrate grown with a ZnO / CdS heterojunction.
[0092] S5: The FTO substrate with the ZnO / CdS heterojunction grown thereon is placed in an electrolyte, and a ZnO / CdS heterojunction ultraviolet photodetector is prepared using a three-electrode system of a working electrode, a counter electrode, and a reference electrode; the counter electrode is a Pt mesh electrode, the reference electrode is a calomel electrode, and the electrolyte is a 0.5 mol / L Na2SO4 aqueous solution.
[0093] Embodiment 4 of the present invention is: a method for preparing a ZnO / CdS heterojunction ultraviolet photodetector, comprising the following steps:
[0094] S1: The FTO substrate was ultrasonically cleaned with acetone, anhydrous ethanol and deionized water for 10 min in sequence, and then dried with nitrogen.
[0095] S2: Use a dropper to drop 0.03M zinc acetate-ethanol solution on the surface of the FTO substrate, rinse it with anhydrous ethanol after 12 seconds, and then blow away the anhydrous ethanol with nitrogen to complete a cycle; after repeating 8 to 10 cycles, put the substrate in a drying oven, keep it at 270°C for 25 minutes, cool it to room temperature and dry it naturally in the air to obtain a FTO substrate with a ZnO seed layer grown on it.
[0096] S3: 0.03M zinc acetate, 0.4M NaOH and 0.03M PEG-1000 were dissolved in deionized water and magnetically stirred for 35 minutes to form a mixed solution; the mixed solution was poured into the inner lining of a 100mL stainless steel autoclave, and then the FTO substrate with the ZnO seed layer grown was vertically placed therein, the autoclave was sealed and kept warm at 170°C for 8 hours, and then naturally dried after being taken out to obtain the FTO substrate with ZnO nanorods grown thereon.
[0097] S4: 0.03M cadmium nitrate, 0.04M thiourea and 0.03M CTAB were dissolved in deionized water and magnetically stirred for 35 minutes to form a mixed solution; the FTO substrate grown with ZnO nanorods was placed in a reactor containing the mixed solution and kept at 170°C for 8 hours for hydrothermal reaction. After cooling to room temperature, it was naturally dried in the air to obtain a FTO substrate grown with a ZnO / CdS heterojunction.
[0098] S5: The FTO substrate with the ZnO / CdS heterojunction grown thereon is placed in an electrolyte, and a ZnO / CdS heterojunction ultraviolet photodetector is prepared using a three-electrode system of a working electrode, a counter electrode, and a reference electrode; the counter electrode is a Pt mesh electrode, the reference electrode is a calomel electrode, and the electrolyte is a 0.5 mol / L Na2SO4 aqueous solution.
[0099] In summary, the ZnO / CdS heterojunction ultraviolet photodetector and the preparation method thereof provided by the present invention can improve the photoelectric performance of ZnO by coating granular CdS on the surface of ZnO nanorods and growing them on a substrate; the ultraviolet photodetector prepared with the ZnO / CdS heterojunction as the working electrode has an Iphoto / Idark ratio of 17.17, a photoresponsivity of 33.35 mA / W, an external quantum efficiency of 11.33%, a response speed rise time of 0.12 s, a decay time of 0.15 s, a short response time, high responsiveness, high sensitivity, fast response and recovery time, and good stability and repeatability.
[0100] The present invention adopts a hydrothermal method to prepare a high-purity, high-crystallinity ZnO / CdS heterojunction, which is conducive to accurately controlling the crystal structure and morphology of ZnO / CdS, optimizing material properties, saving energy, and reducing environmental pollution.
[0101] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent transformations made using the contents of the present invention's specification and drawings, or directly or indirectly applied in related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing a ZnO / CdS heterojunction ultraviolet photodetector, characterized in that: The following steps are involved: S1: growing a ZnO seed layer on the substrate surface by a hydrothermal method; S2: immersing the substrate on which the ZnO seed crystal layer is grown into a mixed solution containing zinc acetate, NaOH and PEG-1000 for reaction to obtain a substrate on which ZnO nanorods are grown; S3: placing the substrate on which the ZnO nanorods are grown into a mixed solution containing Cd(NO3)2, thiourea and CTAB for hydrothermal reaction to obtain a substrate on which a ZnO / CdS heterojunction is grown; S4: Using the ZnO / CdS heterojunction as the working electrode, a ZnO / CdS heterojunction ultraviolet photodetector was prepared.
2. The method for preparing the ZnO / CdS heterojunction ultraviolet photodetector according to claim 1, characterized in that: The S1 is specifically as follows: dripping zinc acetate-ethanol solution on the surface of the substrate, then rinsing it with anhydrous ethanol, and then blowing away the anhydrous ethanol with nitrogen to complete a cycle; after repeating the cycle 8 to 10 times, drying the substrate to obtain a substrate with a ZnO seed crystal layer grown thereon.
3. The method for preparing the ZnO / CdS heterojunction ultraviolet photodetector according to claim 2, characterized in that: The concentration of the zinc acetate-ethanol solution is 0.01-0.03M.
4. The method for preparing the ZnO / CdS heterojunction ultraviolet photodetector according to claim 2, characterized in that: The drying step is specifically: keeping the temperature at 220-270° C. for 25-35 minutes, cooling to room temperature, and then drying naturally in the air.
5. The method for preparing the ZnO / CdS heterojunction ultraviolet photodetector according to claim 1, characterized in that: The preparation method of the mixed solution in S2 is: dissolving 0.01-0.03M zinc acetate, 0.2-0.4M NaOH and 0.01-0.03M MPEG-1000 in deionized water, and stirring for 25-35 minutes to form a mixed solution.
6. The method for preparing the ZnO / CdS heterojunction ultraviolet photodetector according to claim 1, characterized in that: The reaction conditions in S2 are: keeping the temperature at 150-170° C. for 8-12 hours under sealed conditions.
7. The method for preparing the ZnO / CdS heterojunction ultraviolet photodetector according to claim 1, characterized in that: The preparation method of the mixed solution in S3 is: dissolving 0.01-0.03M cadmium nitrate, 0.03-0.04M thiourea and 0.01-0.03M CTAB in deionized water, and stirring for 25-35 minutes to form a mixed solution.
8. The method for preparing the ZnO / CdS heterojunction ultraviolet photodetector according to claim 1, characterized in that: The reaction conditions of the hydrothermal reaction in S3 are: keeping warm at 150-170° C. for 8-12 hours.
9. The method for preparing the ZnO / CdS heterojunction ultraviolet photodetector according to claim 1, characterized in that: The S4 is specifically as follows: placing a substrate on which a ZnO / CdS heterojunction is grown in an electrolyte, and adopting a three-electrode system of a working electrode, a counter electrode, and a reference electrode to prepare a ZnO / CdS heterojunction ultraviolet photodetector.
10. A ZnO / CdS heterojunction ultraviolet photodetector prepared by the method for preparing a ZnO / CdS heterojunction ultraviolet photodetector according to any one of claims 1 to 9.