Sodium-free negative pole piece, preparation method of sodium-free negative pole piece, solid-state sodium battery and assembly method of solid-state sodium battery
Through the combination of acid treatment and sodium ion active layer, the problems of high cost and low safety of negative electrode materials in solid sodium batteries are solved, and higher cycle life and safety are achieved. Combined with the solid electrolyte design, the overall performance of the battery is improved .
Patent Information
- Application Number
- CN202411101344.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-22
AI Technical Summary
Existing solid-state sodium batteries face difficulties in selecting negative electrode materials and electrolyte design. Hard carbon negative electrodes have high cost and low cycle life. Sodium metal negative electrodes have safety hazards, and liquid sodium batteries have low energy density and poor safety.
Using copper or aluminum-based current collector after acid treatment as the negative electrode material, the sodium ion active layer is coated, which contains highly active sodium ion deposition sites and mesh electron conduction channel materials, combined with solid electrolyte design, and is formed by plasma surface treatment. Stable interface layer.
It reduces battery manufacturing costs, improves safety and cycle life, avoids safety hazards of sodium metals, and improves high and low temperature stability and electrochemical performance.
Smart Images

Figure BDA0004989458250000091 
Figure BDA0004989458250000101
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solid-state sodium batteries, and in particular to a sodium-free negative electrode sheet and a preparation method thereof, a solid-state sodium battery and an assembly method thereof. Background Art
[0002] In recent years, with the growing demand for energy and the urgent need for environmentally friendly energy storage solutions, solid-state sodium battery technology has attracted much attention. Compared with traditional lithium-ion batteries, solid-state sodium batteries have many advantages, including cost-effectiveness, higher safety, and excellent high and low temperature performance. At the same time, solid-state sodium batteries also have better safety and higher energy density than liquid sodium batteries. Liquid sodium-ion batteries have low energy density, liquid sodium metal batteries have poor safety, and conventional sodium metal solid-state batteries have insufficient cycle life; however, despite the many advantages of solid-state sodium batteries, their realization still faces some challenges. Among them, the selection of negative electrode materials and the design of electrolytes are technical difficulties. In contrast, sodium batteries using hard carbon negative electrodes still face the problem of high cost, which is mainly due to the complex production process of hard carbon materials and the high cost of raw materials. Hard carbon negative electrodes will continue to produce gas in long cycles, which brings about low cycle life and safety issues. In addition, sodium metal, as a highly active metal, is directly used as the negative electrode of sodium batteries. There are a series of safety hazards when used in batteries, such as the easy generation of sodium dendrites and internal short circuits of batteries. On the other hand, repeated expansion and contraction of sodium metal can also damage the interface between the negative electrode and the electrolyte, resulting in a poor cycle life of the battery. Summary of the invention
[0003] The present invention aims to solve the technical problems in the prior art such as high cost, low safety and poor high and low temperature performance of lithium ion batteries, low energy density of liquid sodium ion batteries, poor safety of liquid sodium metal batteries and insufficient cycle life of conventional sodium metal solid-state batteries, and provides a sodium-free negative electrode sheet and a preparation method thereof, a solid-state sodium battery and an assembly method thereof.
[0004] To achieve the above object, the present invention adopts the following technical solutions:
[0005] In a first aspect, the present invention provides a sodium-free negative electrode plate, comprising:
[0006] (1) Acid-treated current collector;
[0007] (2) The acid-treated current collector is coated with a sodium ion active layer, which comprises an active component of highly active sodium ion deposition, a mesh-like conductive electron channel material, and a binder.
[0008] The thickness of the current collector is 4 to 12 microns, preferably 8 to 10 microns;
[0009] Optionally, the thickness of the sodium ion active layer is 1 to 30 microns; preferably 10 to 20 microns;
[0010] Optionally, the mass ratio of the active component of the highly active sodium ion deposition, the mesh-shaped conductive electron channel material and the binder is 25-75:24-70:1.0-10.
[0011] The current collector is a copper-based current collector or an aluminum-based current collector;
[0012] Optionally, the current collector is in the form of at least one of a foil, a metal foam, or a metal mesh;
[0013] Optionally, the concentration of the acid used to treat the current collector is 0.01M to 1.0M, and the treatment time is 1 to 60 min; preferably, the acid is at least one of CH3COOH, HCl, HNO3, and H2SO4.
[0014] The active component of the highly active sodium ion deposition is at least one of the oxides of Zr, Ge and La;
[0015] Optionally, the mesh-shaped conductive electron channel material is a carbon material; preferably, the carbon material is at least one of graphite, hard carbon, acetylene black, carbon nanotubes, graphene, nitrogen-doped carbon materials, and sulfur-doped carbon materials;
[0016] Optionally, the binder is at least one of PVDF, PTFE, CMC, SBR, PAA, and PAA-Na.
[0017] The present invention also provides a method for preparing the sodium-free negative electrode sheet, comprising immersing the acid-treated current collector in the slurry of the sodium ion active layer; drying; rolling the current collector into a sheet, and performing surface treatment using a plasma jet machine to obtain the sodium-free negative electrode sheet;
[0018] Preferably, the thickness of the current collector is 4 to 12 microns, more preferably 8 to 10 microns; and / or
[0019] The immersion conditions are: temperature of 25-80°C, time of 5-240 min; and / or
[0020] The drying conditions are: placing in a vacuum oven or a blast oven at a temperature of 60 to 120° C. for 10 to 30 hours; and / or
[0021] The thickness of the sodium ion active layer is 1 to 30 micrometers, more preferably 10 to 20 micrometers.
[0022] The acid treatment steps are: immersing the current collector in an acid solution, then washing the current collector with deionized water; and drying;
[0023] Preferably, the H of the acid solution+ The concentration is 0.01M to 1.0M, and the soaking time is 1 to 60 minutes; more preferably, the acid is at least one of CH3COOH, HCl, HNO3, and H2SO4; and / or
[0024] The current collector is a copper-based current collector or an aluminum-based current collector; more preferably, the current collector is in the form of at least one of a foil, a metal foam, or a metal mesh; and / or
[0025] The drying conditions are: drying in a vacuum oven or a blast oven at a temperature of 50 to 120° C. for 6 to 20 hours;
[0026] Optionally, the preparation steps of the slurry of the sodium ion active layer are: mixing the active components of the highly active sodium ion deposition and the mesh-shaped conductive electron channel material in a solid state to obtain a mixture; then adding a mixed solution of a binder to the obtained mixture, homogenizing, and obtaining a slurry of the sodium ion active layer;
[0027] Preferably, the mass ratio of the active component of the highly active sodium ion deposition, the mesh-shaped conductive electron channel material and the binder is 25-75:24-70:1.0-10; and / or
[0028] The active component of the highly active sodium ion deposition is at least one of oxides of Zr, Ge and La; and / or
[0029] The mesh-shaped conductive electron channel material is a carbon material; more preferably, the mesh-shaped conductive electron channel material is at least one of graphite, hard carbon, acetylene black, carbon nanotubes, graphene, nitrogen-doped carbon materials, and sulfur-doped carbon materials; and / or
[0030] The binder is at least one of PVDF, PTFE, CMC, SBR, PAA, and PAA-Na; more preferably, the solvent of the binder mixed solution is at least one of ethanol, acetonitrile, NMP, triethylamine, and acetone; and / or the mass fraction of the binder in the binder mixed solution is 1% to 10%; and / or the binder mixed solution is added to the obtained mixture for homogenization for 10 to 30 hours.
[0031] In a second aspect, the present invention provides a solid-state sodium battery, comprising the sodium-free negative electrode plate.
[0032] The solid-state sodium battery further comprises a positive electrode plate, a separator and a solid electrolyte; the solid electrolyte is a polymer precursor solution formed by mixing an unsaturated monomer, an alkali metal sodium salt, an initiator, a functional additive and a cross-linking agent, and solidifying to form a solid polymer electrolyte;
[0033] Preferably, the unsaturated ester monomer is at least one of vinylene carbonate, vinyl ethylene carbonate, trimethylolpropane triacrylate, pentaerythritol triacrylate, polyethylene glycol diacrylate, tripropylene glycol diacrylate, butyl acrylate and derivatives thereof; and / or
[0034] The alkali metal sodium salt is at least one of NaDFOB, NaBOB, NaTFSI, NaCF3SO3, NaN(CF3SO2)2, NaN(C2F5SO2)2, NaPF6, NaN(CF3SO2)(C4F9SO2), NaTDI, NaC(CF3SO2)3, NaBF4, NaC(C2F5SO2)3, and NaClO4; and / or
[0035] The functional additive is at least one of LLZTO, LLZO, LATP, Al2O3, silicon compounds and amide small molecule monomers; and / or
[0036] The cross-linking agent is at least one of pentaerythritol tetrathioglycolate, trimethylolpropane tris(2-thioglycolate) and derivatives thereof; more preferably, the amount of the cross-linking agent added is 0.1 to 25% of the mass of the unsaturated ester monomer; and / or
[0037] The curing conditions are 50-90° C., more preferably 60-80° C.; and the curing time is 2-30 hours, more preferably 3-20 hours.
[0038] The material of the positive electrode plate is at least one of layered oxide or modified products thereof, sodium iron phosphate or modified products thereof, sodium iron sulfate or modified products thereof, and sodium vanadium phosphate or modified products thereof.
[0039] The present invention further provides a method for assembling the solid-state sodium battery, comprising the following steps:
[0040] The button battery assembly method comprises stacking the positive electrode sheet, the separator and the sodium-free negative electrode sheet in order, and adding a solid electrolyte solution to assemble the button battery; or
[0041] The positive electrode plate, the separator, and the sodium-free negative electrode plate are stacked in sequence to form a dry battery cell with an injection hole, a solid electrolyte solution is added to the injection hole, and then the hole is sealed and solidified to obtain a soft-pack battery.
[0042] The present invention uses low-concentration acid to treat the surface of the current collector, which can effectively remove stains and oxides on the surface of the current collector. At the same time, a high-low surface layer is formed on the surface of the current collector, so that the current collector has a larger specific surface area and stronger adhesion to the slurry. The current collector after acid treatment is coated with a sodium ion active layer. The slurry of the sodium ion active layer uses Zr, Ge, and La oxides as high-activity deposition sites for sodium ions, so that sodium ions are uniformly deposited, dendrite growth is avoided, and dendrite formation is effectively inhibited. Adding carbon materials (such as graphite, hard carbon, acetylene black, carbon nanotubes, graphene, etc.) as mesh conductive electron channel materials in the sodium ion active layer can construct an electron transmission network. The addition of a binder (such as PVDF, PTFE, CMC, SBR, PAA, PAA-Na, etc.) makes the slurry and the current collector more closely combined. When configuring the binder mixed solution, an organic solvent (such as ethanol, acetonitrile, NMP, triethylamine, acetone, etc.) is used, and ultrasound or stirring is performed to achieve uniform mixing and dispersion of the slurry. After drying and rolling, the treated negative electrode plate is subjected to plasma surface treatment, which can form a highly active surface on the outer surface of the electrode and increase the contact with the solid electrolyte.
[0043] The slurry of the sodium-free negative electrode plate of the present invention has good adhesion to the current collector. During the operation of the battery, there will be no delamination or peeling, which helps to maintain the integrity and stability of the electrode. At the same time, the attachments on the current collector have highly active sites for sodium ions, which promote the uniform deposition of sodium ions. In addition, these attachments also have good electronic conductivity to ensure the effective transmission of current; at the same time, they also have a highly active outer surface to match the corresponding solid electrolyte to form a stable solid-electrolyte interface layer.
[0044] The present invention adopts a sodium-free negative electrode combined with a solid electrolyte design to assemble a solid-state sodium battery. Not only can the battery manufacturing cost be reduced, but the safety and electrochemical performance of the battery can also be improved. By adopting a sodium-free negative electrode plate, the present invention can avoid the direct use of sodium metal, thereby eliminating the safety hazards caused by sodium metal. At the same time, the use of a matching solid electrolyte can improve the cycle life and high and low temperature stability of the battery, so that the battery can perform well in various application scenarios.
[0045] The present invention can further achieve good contact between the solid electrolyte and the sodium-free negative electrode through an in-situ curing process, thereby improving the cycle performance of the battery, and matching the current mature battery technology, without the need for major changes to the production line, which is conducive to the efficient use of the original production line. DETAILED DESCRIPTION
[0046] Embodiments of the present invention are described in detail below, and the examples of the embodiments are intended to be used to explain the present invention, but should not be construed as limiting the present invention. In the embodiments, if specific techniques or conditions are not specified, they are carried out according to the techniques or conditions described in the literature in this area or according to the product specification. If the manufacturer is not specified for reagents or instruments used, they are all conventional products that can be obtained commercially.
[0047] Example 1: Preparation method of sodium-free negative electrode sheet:
[0048] The active components of the highly active sodium ion deposition are a mixture of GeO2 and La2O3 with a mass ratio of 1:1;
[0049] The mesh conductive channel material is a mixture of hard carbon, acetylene black and carbon nanotubes, with a mass ratio of 1:1:0.05;
[0050] Mixed solution of binder: PVDF is dissolved in NMP solvent to obtain a mixed solution of binder; the mass fraction of the binder is 2%.
[0051] Preparation of the slurry of the sodium ion active layer used below:
[0052] Solid material mixing: The active components of highly active sodium ion deposition and the mesh conductive channel material are mixed evenly in a solid state.
[0053] Slurry preparation: Add the mixed solution of the binder to the above mixture and homogenize for 24 hours to obtain the slurry of the sodium ion active layer.
[0054] The mass ratio of the active components of high-activity sodium ion deposition, the mesh conductive channel material and the binder is 30:68:2.
[0055] Preparation of sodium-free negative electrode sheet:
[0056] (1) Acid treatment of current collector: Immerse the copper foil current collector in a hydrochloric acid solution (H + The concentration was 0.05 M) and the treatment time was 5 min. The copper foil current collector was then washed with deionized water.
[0057] (2) The cleaned current collector is dried in a vacuum oven at 80° C. for 10 h.
[0058] (3) Preparation of sodium-free negative electrode sheet:
[0059] a. Immerse the dried current collector in the prepared sodium ion active layer slurry for 30 min at a slurry temperature of 25°C.
[0060] b. Dry in a vacuum oven at 100°C for 15 hours.
[0061] c. Roll the dried current collector with the sodium ion active layer active slurry to form a pole piece, wherein the current collector thickness is 10 microns and the sodium ion active layer thickness is 10 microns.
[0062] d. Plasma surface treatment: Use a jet plasma machine to perform surface treatment on the obtained electrode sheet, thereby obtaining the sodium-free negative electrode sheet.
[0063] Example 2: Preparation method of sodium-free negative electrode sheet:
[0064] The active components of the highly active sodium ion deposition are a mixture of GeO2, La2O3 and ZrO4 with a mass ratio of 1:1:0.2;
[0065] The mesh conductive channel material is a mixture of hard carbon, graphite, acetylene black and carbon nanotubes, with a mass ratio of 1:1:1:0.05;
[0066] Mixed solution of binder: PVDF is dissolved in NMP solvent; the mass fraction of the binder is 2%.
[0067] Preparation of the slurry of the sodium ion active layer used below:
[0068] Solid material mixing: The active components of highly active sodium ion deposition and the mesh conductive channel material are mixed evenly in a solid state.
[0069] Slurry preparation: Add the mixed solution of the binder to the above mixture and homogenize for 24 hours to obtain the slurry of the sodium ion active layer.
[0070] The mass ratio of the active components of high-activity sodium ion deposition, the mesh conductive channel material and the binder is 40:57:3.
[0071] Preparation of sodium-free negative electrode sheet:
[0072] (1) Acid treatment of current collector: prepare acid solution, the acid is CH3COOH, H + The concentration is 0.02M; the aluminum foil current collector is immersed in the above acid solution for 20 minutes, and then the aluminum foil current collector is washed with deionized water.
[0073] (2) The above current collector is dried in a vacuum oven at 60° C. for 10 h.
[0074] (3) Preparation of sodium-free negative electrode sheet:
[0075] a. The current collector obtained in (2) was immersed in the prepared sodium ion active layer slurry for 40 min at a slurry temperature of 30°C.
[0076] b. Take out the current collector with the active slurry of the sodium ion active layer obtained in a and dry it in a vacuum oven at a temperature of 100°C for 10 hours.
[0077] c. The current collector with the sodium ion active layer active slurry dried in b is rolled into a pole piece, wherein the current collector thickness is 10 microns; the thickness of the sodium ion active layer is 20 microns.
[0078] d. Plasma surface treatment: Use a jet plasma machine to perform surface treatment on the electrode obtained in c, so as to obtain the sodium-free negative electrode.
[0079] Example 3: Preparation method of sodium-free negative electrode sheet:
[0080] The active components of the highly active sodium ion deposition are a mixture of GeO2, La2O3 and ZrO4 with a mass ratio of 1:1:0.2;
[0081] The mesh conductive channel material is a mixture of hard carbon, graphite, acetylene black and carbon nanotubes, with a mass ratio of 1:1:1:0.05;
[0082] Mixed solution of binder: PVDF is dissolved in NMP solvent; the mass fraction of the binder is 10%.
[0083] Preparation of the slurry of the sodium ion active layer used below:
[0084] Solid material mixing: The active components of highly active sodium ion deposition and the mesh conductive channel material are mixed evenly in a solid state.
[0085] Slurry preparation: Add the mixed solution of the binder to the above mixture and homogenize for 24 hours to obtain the slurry of the sodium ion active layer.
[0086] The mass ratio of the active components of high-activity sodium ion deposition, the mesh conductive channel material and the binder is 45:52:3.
[0087] Preparation of sodium-free negative electrode sheet:
[0088] (1) Acid treatment of current collector: prepare acid solution, the acid is H2SO4, H + The concentration is 1.0M; the copper foil current collector is immersed in the above acid solution for 60 minutes, and then the copper foil current collector is washed with deionized water.
[0089] (2) The above current collector is dried in a vacuum oven at a temperature of 120° C. for 6 h.
[0090] (3) Preparation of sodium-free negative electrode sheet:
[0091] a. The current collector obtained in (2) was immersed in the prepared sodium ion active layer slurry for 240 min at a slurry temperature of 80°C.
[0092] b. Take out the current collector with the active slurry of the sodium ion active layer obtained in a and dry it in a vacuum oven at a temperature of 100°C for 20h.
[0093] c. The current collector with the active slurry of the sodium ion active layer dried in b is rolled into a pole piece, wherein the current collector thickness is 8 microns; the thickness of the sodium ion active layer is 10 microns.
[0094] d. Plasma surface treatment: Use a jet plasma machine to perform surface treatment on the electrode obtained in c, so as to obtain the sodium-free negative electrode.
[0095] Example 4: Preparation method of sodium-free negative electrode sheet:
[0096] The active components of the highly active sodium ion deposition are a mixture of GeO2, La2O3 and ZrO4 with a mass ratio of 1:1:0.2;
[0097] The mesh conductive channel material is a mixture of hard carbon, graphite, acetylene black and carbon nanotubes, with a mass ratio of 1:1:1:0.05;
[0098] Mixed solution of binder: PVDF is dissolved in NMP solvent; the mass fraction of the binder is 1%.
[0099] Preparation of the slurry of the sodium ion active layer used below:
[0100] Solid material mixing: The active components of highly active sodium ion deposition and the mesh conductive channel material are mixed evenly in a solid state.
[0101] Slurry preparation: Add the binder mixed solution to the above mixture and homogenize for 24 hours to obtain the slurry of the sodium ion active layer.
[0102] The mass ratio of the active component of high-activity sodium ion deposition, the mesh conductive channel material and the binder is 50:40:10.
[0103] Preparation of sodium-free negative electrode sheet:
[0104] (1) Acid treatment of current collector: prepare acid solution, the acid is HNO3, H + The concentration is 0.8M; the copper foil current collector is immersed in the above acid solution for 60 minutes, and then the copper foil current collector is washed with deionized water.
[0105] (2) The above current collector is dried in a vacuum oven at 120° C. for 20 h.
[0106] (3) Preparation of sodium-free negative electrode sheet:
[0107] a. The current collector obtained in (2) was immersed in the prepared sodium ion active layer slurry for 240 min at a slurry temperature of 80°C.
[0108] b. Take out the current collector with the active slurry of the sodium ion active layer obtained in a and dry it in a vacuum oven at a temperature of 100°C for 20h.
[0109] c. The current collector with the sodium ion active layer active slurry dried in b is rolled into a pole piece, wherein the current collector thickness is 12 microns; the thickness of the sodium ion active layer is 20 microns.
[0110] d. Plasma surface treatment: Use a jet plasma machine to perform surface treatment on the electrode obtained in c, so as to obtain the sodium-free negative electrode.
[0111] Example 5: Preparation method of sodium-free negative electrode sheet:
[0112] The difference from Example 3 is that the active components of high-activity sodium ion deposition, the mesh conductive path material and the binder are weighed in a mass ratio of 25:70:5. The thickness of the current collector is 10 microns. The thickness of the sodium ion active layer is 1 micron.
[0113] Example 6: Preparation method of sodium-free negative electrode sheet:
[0114] The difference from Example 3 is that the active components of high-activity sodium ion deposition, the mesh conductive path material and the binder are weighed at a mass ratio of 75:24:1. The thickness of the current collector is 4 microns. The thickness of the sodium ion active layer is 30 microns.
[0115] The current collectors used in the above-mentioned embodiments 3-6 are not limited to foil, metal foam or metal mesh. The concentration of the acid used to treat the current collector is 0.01M to 1.0M, not limited to 0.01M, 0.02M, 0.05M, 0.1M, 0.2M, 0.3M, 0.4M, 0.5M, 0.6M, 0.7M, 0.8M, 0.9M, 1.0M. The treatment time is 1 to 60min, not limited to 1min, 2min, 5min, 10min, 20min, 30min, 40min, 50min, 60min.
[0116] The mesh conductive electron channel material used in Examples 3-6 can be replaced by graphite, hard carbon, acetylene black, carbon nanotubes, graphene, nitrogen-doped carbon materials, and sulfur-doped carbon materials; the PVDF binder used can be replaced by PTFE, CMC, SBR, PAA, and PAA-Na. The NMP solvent used can be replaced by ethanol, acetonitrile, triethylamine, and acetone.
[0117] Example 7: Preparation method of solid electrolyte solution:
[0118] (1) adding alkali metal sodium salt (NaPF6 and NaTFSI) to unsaturated ester monomer (polyethylene glycol diacrylate) to form a mixed solution with a concentration of 1 M, wherein the mass ratio of the two salts is 1:0.5, and stirring fully under a protective gas atmosphere to completely dissolve the alkali metal sodium salt, and then adding a crosslinking agent (pentaerythritol tetrathioglycolate), stirring evenly to obtain liquid A; the amount of the crosslinking agent added is 2% of the mass of the unsaturated ester monomer;
[0119] (2) mixing the functional additive (LLZTO) with liquid A and stirring them fully under a protective gas atmosphere to obtain liquid B; the content of the functional additive is 1% of the mass of liquid A;
[0120] (3) Add the initiator (AIBN) to the B solution, stir evenly at low temperature in a protective gas atmosphere away from light to obtain a precursor solution, i.e., a solid electrolyte solution; AIBN is 0.2% of the unsaturated monomer.
[0121] (4) Curing the precursor solution to obtain a solid electrolyte at 50° C. and heating for 20 h.
[0122] Example 8: Preparation method of solid electrolyte solution:
[0123] (1) adding alkali metal sodium salts NaPF6, NaTFSI and NaDFOB to two unsaturated ester monomers (polyethylene glycol diacrylate and vinyl ethylene carbonate, in a volume ratio of 1:1) to form a mixed solution with a concentration of 1 M, wherein the mass ratio of the three salts is 1:0.5:0.2, and stirring is performed under a protective gas atmosphere to completely dissolve the alkali metal sodium salt, and then adding a crosslinking agent pentaerythritol tetrathioglycolate and stirring uniformly to obtain a solution A; the amount of the crosslinking agent added is 2.5% of the mass of the unsaturated ester monomer;
[0124] (2) Mixing the functional additives LZTO and LATP with liquid A, and stirring them thoroughly under a protective gas atmosphere to obtain liquid B; the content of the functional additives is 1.5% by mass of liquid A;
[0125] (3) Add initiator AIBN to liquid B, stir evenly at low temperature in a protective gas atmosphere away from light to obtain a precursor solution, i.e., a solid electrolyte solution; AIBN is 0.25% of the unsaturated monomer.
[0126] (4) The precursor solution is cured to obtain a solid electrolyte at 90° C. and heated for 3 h.
[0127] Example 9-16: Assembly method of solid-state sodium battery
[0128] 1. Assembly method of button battery:
[0129] The diaphragm, commercial electrolyte, and positive electrode are commercial products, purchased from Duoduo Reagent Network or through the Lithium Battery Alliance President (official account). The commercial electrolyte purchased is NaClO4 electrolyte (NC-004) with the formula: 1M NaClO4 inEC:PC=1:1Vol%+5%FEC.
[0130] The positive electrode plate, the separator and the prepared sodium-free negative electrode plate are stacked in order, and the above commercial electrolyte or the solid electrolyte solution prepared in Example 7 or 8 is added to assemble into a button battery.
[0131] 2. Assembly method of soft pack battery:
[0132] Dry cell preparation:
[0133] (1) The positive electrode sheet, separator, and sodium-free negative electrode sheet are stacked in sequence.
[0134] (2) The dry battery cell includes the electrode sheets stacked in step (1) and has a liquid injection hole, and is in the shape of a soft package.
[0135] The diaphragm, commercial electrolyte, and positive electrode are commercial products and can be purchased from Duoduo Reagent Network or through the agent of the President of the Lithium Battery Alliance (official account).
[0136] The above commercial electrolyte or the solid electrolyte solution prepared in Example 7 or 8 is added to the dry cell to assemble into a soft pack battery. For the cell injected with the solid electrolyte solution prepared in Example 7 or 8, it is necessary to cure at 70° C. for 10 hours after sealing.
[0137] The solid-state sodium battery assembled in the present invention is one of a button battery, a soft pack, a hard shell or a cylindrical battery. The material of the positive electrode plate used is at least one of a layered oxide positive electrode or a modified product thereof, sodium iron phosphate or a modified product thereof, sodium iron sulfate or a modified product thereof, sodium vanadium phosphate or a modified product thereof. The diaphragm used is at least one of a PP diaphragm, a PE diaphragm, a non-woven fabric diaphragm, a glass fiber diaphragm, a PTFE diaphragm or a PVDF diaphragm.
[0138] Examples 9-16 and Comparative Examples 1-16 were assembled according to the battery components shown in Table 1.
[0139] Performance test method of solid-state sodium battery:
[0140] At 30°C, the batteries prepared in the examples and comparative examples were activated at a rate of 0.1C for the first cycle, and then fully charged and discharged in the corresponding window at a rate of 1C until the capacity of the battery was less than 90% of the 1C first cycle discharge capacity. The number of cycles was recorded. The specific data is shown in Table 1.
[0141] Table 1 Battery composition and cycle performance test results
[0142]
[0143]
[0144] Note: The diaphragm materials in the table are all Celgard. The negative electrode sheet prepared in Example 1 is referred to as sheet 1. The negative electrode sheet prepared in Example 2 is referred to as sheet 2. The solid electrolyte solution prepared in Example 7 is referred to as solution 7; the solid electrolyte solution prepared in Example 8 is referred to as solution 8.
[0145] From the data results in Table 1, it can be seen that the button-type sodium battery is assembled using the negative electrode plate and the solid electrolyte solution of the present invention. The test results show that when the discharge capacity of the sodium battery decays to 90% of the 1C first-cycle capacity, the number of cycles is 120-130 times. Compared with the use of copper foil or aluminum foil as the negative electrode plate and the use of commercial electrolyte as the electrolyte, the number of cycles of the battery is greatly increased. The soft-pack sodium battery is assembled using the sodium-free negative electrode plate and the solid electrolyte solution of the present invention, and the battery cycle life is also improved. By assembling a solid-state sodium battery using the present invention, the battery cycle life is improved, the battery safety is high, and the cost is low.
[0146] It can also be seen that when copper foil or aluminum foil is directly used as the negative electrode, in a buckle battery or soft pack, whether in a liquid sodium battery or a solid sodium battery, the battery decays rapidly after two or three cycles. The main reason is that in liquid batteries, after the sodium ions are deposited on the aluminum foil, the highly active metallic sodium atoms are quickly consumed by the electrolyte, resulting in irreversible loss of active sodium; while in the solid state, the deposited sodium layer and the solid electrolyte layer have poor contact, resulting in irreversible back embedding of active sodium.
[0147] In liquid batteries, in buckle batteries or soft packs, the sodium-free negative electrode plate of the present invention is directly used as the negative electrode, and the battery can cycle relatively well, but decays faster, mainly because the negative electrode electrolyte cannot be well adapted to the sodium-free negative electrode plate, and gas production is serious.
[0148] In contrast, the solid-state sodium battery composed of the sodium-free negative electrode plate and the in-situ solidified solid electrolyte of the present invention performs excellently. This is mainly due to the innovative electrode design: by treating the surface of the current collector with low-concentration acid, the stains and oxides on the surface of the current collector can be effectively removed, and at the same time, a high and low undulating surface layer is formed on the surface of the current collector, so that the current collector has a larger specific surface area and stronger adhesion to the slurry. In terms of slurry selection, the oxides of Zr, Ge, and La can be used as highly active deposition sites for sodium ions, so that sodium ions are uniformly deposited to avoid dendrite growth; the addition of carbon materials (such as graphite, hard carbon, acetylene black, carbon nanotubes, graphene, etc.) can construct an electron transport network; ultrasonic or stirring in an organic solvent (such as triethylamine, acetone, ethanol, NMP, etc.) can achieve uniform mixing and dispersion of the slurry; the addition of a binder (such as PVDF, PTFE, CMC, SBR, PAA, PAA-Na, etc.) can make the slurry and the current collector more closely bonded. After drying and rolling, the treated negative electrode is subjected to plasma surface treatment, which can form a highly active surface on the outer surface of the electrode and increase contact with the solid electrolyte. The sodium-free negative electrode sheet obtained in this way allows the sodium metal to be uniformly deposited, effectively inhibiting the formation of dendrites; at the same time, the separation of the sodium-free negative electrode sheet coating and the current collector is avoided; the in-situ curing process can further achieve good contact between the solid electrolyte and the sodium-free negative electrode sheet, thereby improving the cycle performance of the battery, and matching the current mature battery process, without major changes in the production line, which is conducive to the efficient use of the original production line.
[0149] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention without departing from the principles and intent of the present invention.
Claims
1. A sodium-free negative electrode plate, characterized in that: Include: (1) Acid-treated current collector; (2) A sodium ion active layer coated on the current collector after acid treatment, wherein the sodium ion active layer comprises an active component of high-activity sodium ion deposition, a network-shaped conductive electron channel material and a binder.
2. The sodium-free negative electrode sheet according to claim 1, characterized in that: The concentration of the acid in the acid treatment is 0.01M to 1.0M, and the time of the acid treatment is 1 to 60 minutes; preferably, the acid is at least one of CH3COOH, HCl, HNO3, and H2SO4; Optionally, the thickness of the current collector is 4 to 12 microns; preferably 8 to 10 microns; Optionally, the current collector is a copper-based current collector or an aluminum-based current collector; Optionally, the current collector is in the form of at least one of foil, metal foam, or metal mesh.
3. The sodium-free negative electrode sheet according to claim 1, characterized in that: The thickness of the sodium ion active layer is 1 to 30 microns, preferably 10 to 20 microns; Optionally, the mass ratio of the active component of the highly active sodium ion deposition, the mesh-shaped conductive electron channel material and the binder is 25-75:24-70:1-10.
4. The sodium-free negative electrode sheet according to claim 1, characterized in that: The active component of the highly active sodium ion deposition is at least one of the oxides of Zr, Ge and La; Optionally, the mesh-shaped conductive electron channel material is a carbon material; preferably, the carbon material is at least one of graphite, hard carbon, acetylene black, carbon nanotubes, graphene, nitrogen-doped carbon materials, and sulfur-doped carbon materials; Optionally, the binder is at least one of PVDF, PTFE, CMC, SBR, PAA, and PAA-Na.
5. A method for preparing a sodium-free negative electrode sheet according to any one of claims 1 to 4, characterized in that: The acid-treated current collector is immersed in the slurry of the sodium ion active layer; dried; rolled into a pole piece, and finally surface treated with a plasma jet machine to obtain a sodium-free negative pole piece; Preferably, the immersion conditions are: temperature of 25-80°C, time of 5-240 min; and / or The drying conditions are: temperature 60-120° C., time 10-30 h.
6. The method for preparing a sodium-free negative electrode sheet according to claim 5, characterized in that: The acid-treated current collector is obtained by immersing the current collector in acid, then washing it, and drying it; Preferably, the acid H + The concentration is 0.01M to 1.0M, and the soaking time is 1 to 60min; more preferably, the acid is at least one of CH3COOH, HCl, HNO3, and H2SO4; and / or The drying conditions are: temperature 50-120°C, time 6-20h; Optionally, the preparation steps of the slurry of the sodium ion active layer are: mixing the active components of the highly active sodium ion deposition and the mesh-shaped conductive electron channel material in a solid state to obtain a mixture; then adding a mixed solution of a binder to the obtained mixture, homogenizing, and obtaining a slurry of the sodium ion active layer; Preferably, the solvent of the mixed solution of the binder is at least one of ethanol, acetonitrile, NMP, triethylamine and acetone; and / or The mass fraction of the binder in the mixed solution of the binder is 1% to 10%.
7. A solid-state sodium battery, characterized in that: It comprises the sodium-free negative electrode sheet as described in any one of claims 1 to 4, or the sodium-free negative electrode sheet prepared by the preparation method as described in claim 5 or 6.
8. The solid-state sodium battery according to claim 7, characterized in that: It also includes a positive electrode plate, a separator and a solid electrolyte; the solid electrolyte is a precursor solution formed by mixing an unsaturated ester monomer, an alkali metal sodium salt, an initiator, a functional additive and a cross-linking agent, and then solidified to form a solid polymer electrolyte; Preferably, the unsaturated ester monomer is at least one of vinylene carbonate, vinyl ethylene carbonate, trimethylolpropane triacrylate, pentaerythritol triacrylate, polyethylene glycol diacrylate, tripropylene glycol diacrylate, butyl acrylate and derivatives thereof; and / or The alkali metal sodium salt is at least one of NaDFOB, NaBOB, NaTFSI, NaCF3SO3, NaN(CF3SO2)2, NaN(C2F5SO2)2, NaPF6, NaN(CF3SO2)(C4F9SO2), NaTDI, NaC(CF3SO2)3, NaBF4, NaC(C2F5SO2)3, and NaClO4; and / or The functional additive is at least one of LLZTO, LLZO, LATP, Al2O3, silicon compounds and amide small molecule monomers; and / or The cross-linking agent is at least one of pentaerythritol tetrathioglycolate, trimethylolpropane tris(2-thioglycolate) and derivatives thereof; more preferably, the amount of the cross-linking agent added is 0.1 to 25% of the mass of the unsaturated ester monomer; and / or The curing conditions are 50-90° C., more preferably 60-80° C.; and the curing time is 2-30 hours, more preferably 3-20 hours.
9. The solid-state sodium battery according to claim 8, characterized in that: The material of the positive electrode plate is at least one of layered oxide or modified products thereof, sodium iron phosphate or modified products thereof, sodium iron sulfate or modified products thereof, and sodium vanadium phosphate or modified products thereof.
10. An assembly method of a solid-state sodium battery according to any one of claims 7 to 9, characterized in that: The steps include: A button battery assembly method: stacking a positive electrode sheet, a separator and a sodium-free negative electrode sheet according to any one of claims 1 to 4 in order, adding a solid electrolyte solution to assemble the button battery; or The positive electrode plate, the separator, and the sodium-free negative electrode plate according to any one of claims 1 to 4 are stacked in sequence to form a dry battery cell with an injection hole, a solid electrolyte solution is added to the injection hole, and then the hole is sealed and solidified to obtain a soft-pack battery.