Positive electrode active material, secondary battery, and electronic device

By combining lithium iron phosphate material and lithium-rich manganese-based material in lithium-ion batteries as composite particles in high proportions, and combining carbon layer coating and doping elements, the problem of difficulty in improving the magnification and cycling performance in the prior art is solved. , achieving high energy density and cycle stability of lithium-ion batteries.

CN119008867APending Publication Date: 2024-11-22ENVISION DYNAMICS TECH (JIANGSU) CO LTD +3
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310553660.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The prior art is difficult to simultaneously improve the rate performance and circulation performance of lithium manganese iron phosphate and lithium-rich manganese-based materials in lithium-ion batteries, and the composite process is complex and costly.

Method used

By combining lithium iron phosphate material and lithium-rich manganese-based material into composite particles at a ratio of 66%-99%, a composite positive electrode active material is formed, and the high rate performance of lithium iron phosphate material and the high cycle of lithium-rich manganese-based material is utilized. Performance advantages, combining carbon layer coating and doping elements to form excellent magnification and cycling performance.

Benefits of technology

The efficient rate performance and cyclic performance of the positive electrode active material are improved, the conductivity is reduced, the side reactions are reduced, and the energy density and cyclic stability of the battery are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004234363940000101
    Figure BDA0004234363940000101
  • Figure BDA0004234363940000111
    Figure BDA0004234363940000111
  • Figure BDA0004234363940000121
    Figure BDA0004234363940000121
Patent Text Reader

Abstract

The invention provides a positive electrode active material, a secondary battery, and an electronic device. The positive electrode active material includes first particles, second particles, and third particles, the third particles being composite particles including the first particles and the second particles; the first particles comprise a lithium iron phosphate material; the second particle comprises a lithium-rich manganese-based material; in the third particles, the first particles account for 66-99% of the mass of the third particles. The positive electrode active material provided by the invention can improve the rate capability and cycle performance of the secondary battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a positive electrode active material, a secondary battery and an electronic device. Background Art

[0002] The compaction density and energy density of olivine-type positive electrode materials, such as lithium iron phosphate and lithium manganese iron phosphate (LMFP for short), are much lower than those of other types of positive electrode materials, such as ternary positive electrode materials and lithium-rich manganese-based materials (LRMO for short).

[0003] At the same time, the high-temperature cycle performance of olivine-type positive electrode materials is poor, but their low-temperature performance is good (due to particle nano-sizing and carbon coating).

[0004] Lithium-rich manganese-based materials have higher compaction, poor low-temperature performance and conductivity, but good high-temperature cycling and higher energy density than olivine-type positive electrode materials.

[0005] The composite of lithium iron manganese phosphate and lithium-rich manganese-based materials can take into account the advantages of both lithium iron manganese phosphate and lithium-rich manganese-based materials. However, many current composite forms are simply physically mixed, which results in poor contact between the two, or requires difficult processing technology, resulting in high costs and difficulty in implementation.

[0006] Chinese patent CN110459749A discloses a composite positive electrode material and a preparation method thereof. The method first mixes the carbon-coated lithium iron manganese phosphate material and the positive electrode material A at high speed, and controls the particle size D50 of the carbon-coated lithium iron manganese phosphate material within the range of 20-200nm, so that the two materials reach a lightly coated state under high-speed mixing, and the lithium iron manganese phosphate material surrounds the surface of the positive electrode material A to form a composite coating material with a core-shell structure. Among them, the mass ratio of the carbon-coated lithium iron manganese phosphate material to the positive electrode material A is less than 66%. However, the patent requires strict control of the particle size of the lithium iron manganese phosphate material, which is difficult to process. At the same time, the proportion of lithium iron manganese phosphate material in the composite material is small, resulting in a larger rate performance.

[0007] At present, how to cleverly utilize the composite effect between lithium iron manganese phosphate and lithium-rich manganese-based materials to obtain lithium-ion batteries with improved rate performance and cycle performance is a technical problem to be solved. Summary of the invention

[0008] In view of the shortcomings of the prior art, the object of the present invention is to provide a positive electrode active material, a secondary battery and an electronic device. The positive electrode active material of the present invention can improve the rate performance and cycle performance of the secondary battery.

[0009] One aspect of the present invention provides a positive electrode active material, which includes a first particle, a second particle and a third particle, wherein the third particle is a composite particle including the first particle and the second particle;

[0010] The first particles include lithium iron phosphate material;

[0011] The second particles include a lithium-rich manganese-based material;

[0012] In the third particles, the mass percentage of the first particles to the third particles is 66%-99%.

[0013] A second aspect of an embodiment of the present invention provides a secondary battery, which includes a positive electrode plate and a negative electrode plate, wherein the positive electrode plate includes a current collector and a positive electrode active material layer provided on at least one surface of the current collector, and the positive electrode active material layer includes the positive electrode active material.

[0014] A third aspect of the embodiments of the present invention provides an electronic device, which includes the secondary battery.

[0015] The positive progressive effect of the present invention is that the positive electrode active material of the present invention efficiently utilizes the high rate performance of lithium iron phosphate materials and the high cycle performance advantages of lithium-rich manganese-based materials, and the two positive electrode materials are compounded into secondary particles in the form of primary particles to form a composite positive electrode active material with excellent rate performance and cycle performance. DETAILED DESCRIPTION

[0016] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.

[0017] Positive electrode active material

[0018] A first aspect of an embodiment of the present invention provides a positive electrode active material, which includes a first particle, a second particle and a third particle, wherein the third particle is a composite particle including the first particle and the second particle;

[0019] The first particles include lithium iron phosphate material;

[0020] The second particles include a lithium-rich manganese-based material;

[0021] The mass percentage of the first particle in the positive electrode active material is 66%-99%. The researchers of the present invention found that the lithium-rich manganese-based material itself has no carbon coating layer, the electrical conductivity is very low, and the powder resistivity is 85000Ω·m (powder resistivity is the ratio between the actual resistance value and the theoretical resistance value, which is an indicator of the current conductivity of the powder material). LMFP generally has a carbon layer coating, and the powder resistivity is very low, about 20Ω·m. Therefore, when the content of lithium-rich manganese-based material is too high, it will lead to a decrease in the electrical conductivity of the secondary battery and a decrease in the rate performance. The present invention improves the rate performance by increasing the mass proportion of lithium iron phosphate material. At the same time, the primary particles of lithium iron phosphate and lithium-rich manganese-based materials are agglomerated to form secondary particles, the contact area between the obtained positive electrode active material and the electrolyte becomes smaller, the rate of side reactions becomes smaller, and the cycle performance is improved. As for the cycle performance, on the other hand, the lithium-rich manganese-based material, as a lithium-rich material, has a reduced initial efficiency, and the replenished lithium ions cannot all be embedded back into the lithium-rich manganese-based material. The lithium embedding sites of the lithium iron phosphate material just play a role, that is, the lithium-rich manganese-based material exists as a lithium supplement, which works together with the aforementioned secondary particle agglomerates to improve the cycle performance.

[0022] In this specification, the chemical composition of the lithium iron phosphate material can be based on conventional lithium iron phosphate positive electrode active materials in the art, which are generally represented by the following chemical formula I in the art: Li a Mn x Fe 1-x-y M y PO4; wherein a is 0.9-1.1; x is 0-1.0; y is 0-0.02; M represents a doping element, and M includes one or more of Ti, Mg, Ni, Co, Al, V, Cr, Zr and Nb. The addition of doping elements is beneficial to improving the conductivity and ion conductivity of lithium iron phosphate materials, thereby improving the rate performance. If it is too low, the improvement effect is not significant, and if it is too high, the number of active sites will be reduced, and the energy density will be reduced.

[0023] In some embodiments, in the chemical formula I, the value of a is 0.95, 1 or 1.05. If a is too low, the average potential is low, resulting in low energy density and significantly affecting the rate performance of the secondary battery. In a preferred embodiment, the value of a is 1-1.1, and most preferably 1.05.

[0024] In some embodiments, in the chemical formula I, the value of x is 0.4-0.9, for example, 0.5, 0.6, 0.7 or 0.8.

[0025] In some embodiments, in the chemical formula I, the value of y is 0.001-0.02, such as 0.001, 0.002, 0.003 or 0.005. Too high or too low a content of the doping element will result in a decrease in energy density.

[0026] In some embodiments, in the chemical formula I, the value of x / (1-xy) is 1-5, for example, 1.5, 1.6, 2, 2.5, 3, 4 or 4.1.

[0027] In some embodiments, the M is V and / or Ti.

[0028] In this specification, the chemical composition of the lithium-rich manganese-based material can be based on conventional lithium-rich manganese-based materials in the art, which are generally represented by the following chemical formula II in the art: Li 1+(b / (2+b)) Mn 2b / (2+b) M (6 / (2+b))-2 O2, wherein the value of b is 0-1 and is not 0, and M includes one or more of Ni, Co, Mn, Mg, Al, Ti, Zr, Nb, La, Sr and W.

[0029] In this specification, the chemical formula composition of the lithium-rich manganese-based material can also be expressed by the following chemical formula: Li p Mn q M i O2, wherein the value of p is 1.05-1.4, the value of q is 0.5-0.75, and the value of i is 0.01-0.45. Those skilled in the art know that the p, q, and i may also be referred to as stoichiometric numbers.

[0030] In some embodiments, in the chemical formula II, the value of b is preferably 0.1-0.5. If b is too low, the LRMO capacity will be low, and if the value is too high, the LRMO capacity irreversibility will be too high, the electrochemical activity will be poor, and the energy density will be low.

[0031] In some embodiments, in the chemical formula II, the stoichiometric number of the Li element is 1.05-1.4, for example, 1.1, 1.13, 1.2, 1.25, 1.26, 1.3 or 1.33.

[0032] In some embodiments, in the chemical formula II, the stoichiometric number of the Mn element is 0.5-0.8, for example, 0.51, 0.515, 0.55, 0.565, 0.585, 0.59, 0.595, 0.5995, 0.6, 0.625, 0.645 or 0.66.

[0033] In some embodiments, in the chemical formula II, the stoichiometric value of the doping element M is 0.1-0.5, for example, 0.115, 0.2, 0.2005, 0.205, 0.21, 0.215, 0.255, 0.256, 0.305 or 0.435.

[0034] In some embodiments, in the chemical formula II, the doping element M is preferably one or more of Ni, Co and Mg.

[0035] In this specification, particle size D50 is used to indicate the particle size of the corresponding particles, and its physical meaning is the particle size corresponding to the cumulative volume fraction of 50%, that is, the volume of particles smaller than this particle size accounts for 50% of the total volume of all particles. For example, it can be measured by a laser particle size analyzer.

[0036] In some embodiments, the D50 particle size of the first particle can adopt the particle size of the primary particles of lithium iron phosphate conventional in the art, preferably 0.3-1.5 μm, such as 0.4 μm, 0.5 μm or 0.6 μm. In the present invention, the D50 of the first particle can be selected to have a larger particle size to implement the present invention without requiring a difficult processing process.

[0037] In some embodiments, the D50 particle size of the second particles is within the conventional D50 particle size range of primary particles in the art, generally less than 1 μm, preferably 0.3-0.8 μm, such as 0.6 μm or 0.7 μm.

[0038] In some embodiments, the D50 particle size of the third particles is preferably 5-10 μm.

[0039] In this specification, according to the common understanding in the art, the third particles generally refer to particles formed by the accumulation or aggregation of the first particles and the second particles.

[0040] In some embodiments, in the third particles, the total number of the first particles and the second particles is preferably 10-30 / μm 2 , for example 15 / μm 2 , 16 / μm 2 , 17 / μm 2 , 18 / μm 2 , 19 / μm 2 , 20 / μm 2 or 25 / μm 2 The total number refers to the number of the first particles and the second particles in the third particles per unit spherical area.

[0041] In some embodiments, the method for counting the total number of first particles and second particles per unit spherical surface area in the third particle comprises the following steps: (1) selecting a positive electrode active material sample, wherein the particle size of the positive electrode active material sample is 0.8-1.2 times the average particle size D50 of the third particle, performing SEM detection on the sample to obtain a SEM spectrum at a magnification of 10K; (2) according to the SEM spectrum obtained in step (1), calculating the total number σ (individuals / μm) of the first particles and the second particles per unit spherical surface area in the positive electrode active material by the following formula 2 ):

[0042] σ=(x1+x2) / 2*(y1+y2) / 2 / (A / C*B / C)

[0043] in,

[0044] x1 represents the number of primary particles in the horizontal direction of the lower edge of the image in the SEM image of the third particle at 10K magnification;

[0045] x2 represents the number of primary particles in the horizontal direction of the upper edge of the image in the SEM image of the third particle at 10K magnification;

[0046] y1 represents the number of primary particles in the horizontal direction of the left edge of the image in the SEM image of the third particle at 10K magnification;

[0047] y2 represents the number of primary particles in the horizontal direction of the right edge of the image in the SEM image of the third particle at 10K magnification;

[0048] A represents the actual measured lateral length of the SEM image of the third particle at 10K times, in mm;

[0049] B represents the actual measured length in the longitudinal direction of the SEM image of the third particle at 10K times, in mm;

[0050] C represents the actual measured length corresponding to the scale of 1 μm in the SEM image of the third particle at 10K times, and the unit is mm / μm;

[0051] When calculating the total number of first particles and second particles in the SEM image of the third particle at a 10K magnification, as long as a part of the first particle or the second particle appears, it is counted as one particle.

[0052] In a preferred embodiment, the mass percentage of the first particles in the positive electrode active material is 70%-80%, such as 75%. In a preferred embodiment, the mass percentage of the second particles in the positive electrode active material is 5%-30%, such as 10%, 15%, 20% or 25%.

[0053] In a preferred embodiment, in the first particle, part or all of the surface of the particle of the lithium iron phosphate material contains a carbon layer. The mass of the carbon layer accounts for a percentage of 0.5%-3.5% of the total mass of the first particle, such as 1%, 1.5%, 2%, 2.5%, 3% or 3.1%. The carbon layer is coated on the surface of the lithium iron phosphate particle, which has excellent conductivity, thereby improving the rate performance of the battery. At the same time, the coating of the carbon layer reduces the dissolution of Mn in LMFP, and also improves the cycle performance. If the coating amount is too low, the coating effect is poor, and if it is too high, the active sites of LMFP will be reduced, resulting in a decrease in energy density.

[0054] In some embodiments, the compressive strength of the third particles is preferably 5-40 MPa. In some embodiments, the higher the particle size D50 of the third particles, the higher the compressive strength, but when the compressive strength is too high, the rate performance will be reduced.

[0055] In some embodiments, the method for preparing the positive electrode active material comprises the following steps: wet-mixing the raw material of the first particles with the raw material of the second particles, and then spray-granulating.

[0056] The wet mixing may have the meaning commonly understood in the art, and generally refers to adding a solvent, usually ethanol, to the mixture to be mixed.

[0057] The spray granulation may be a conventional operation in the art. Those skilled in the art know that third particles with different particle sizes can be obtained by controlling the rotation speed of the spray granulation.

[0058] Secondary battery

[0059] Another aspect of the present invention provides a secondary battery, It comprises a positive electrode sheet and a negative electrode sheet, wherein the positive electrode sheet comprises a current collector and a positive electrode active material layer arranged on at least one surface of the current collector, and the positive electrode active material layer comprises the positive electrode active material.

[0060] In some embodiments, the current collector may be made of a sheet or foil of a metal such as aluminum, nickel, titanium, stainless steel, etc., preferably aluminum foil. In some specific embodiments, the positive electrode active material layer may be disposed on both surfaces of the current collector or on a single surface.

[0061] In some embodiments, the positive electrode active material layer generally further includes a conventional binder and a conductive agent in the art. The binder may include, but is not limited to, polyvinylidene fluoride. The conductive agent may include, but is not limited to, carbon black. The mass ratio of the positive electrode active material, the conductive agent, and the binder may be conventional in the art, such as 97:1.5:1.5.

[0062] In some embodiments, the preparation method of the positive electrode sheet can be conventional in the art, generally comprising the following steps: applying a positive electrode slurry containing the positive electrode active material, a conductive agent and a binder to one side of the current collector, and then drying. The solvent of the positive electrode slurry can be conventional in the art, generally without special limitation, for example, it can be nitrogen methyl pyrrolidone.

[0063] In this specification, "secondary battery" refers to a storage device that can be repeatedly charged and discharged, and is a term that includes storage elements such as so-called storage batteries and double-layer capacitors. In addition, in this specification, "lithium-ion secondary battery" refers to a secondary battery that uses lithium ions as charge carriers and achieves charging and discharging by the movement of lithium ions between positive and negative electrodes.

[0064] In some embodiments, the secondary battery is a soft pack battery.

[0065] In some embodiments, the negative electrode plate can be any of various negative electrode plates suitable for lithium-ion secondary batteries in the art, which generally includes a current collector and a negative electrode active material layer disposed on at least one surface of the current collector.

[0066] In some embodiments, the negative electrode active material layer includes at least a negative electrode active material, a conductive agent, a binder and a thickener. The present invention does not specifically limit the types of the negative electrode active material, the conductive agent, the binder and the thickener, and they can be selected according to actual needs.

[0067] In some embodiments, the negative electrode active material may be, for example, graphite.

[0068] In some embodiments, the conductive agent may be, for example, acetylene black.

[0069] In some embodiments, the binder may be, for example, sodium carboxymethyl cellulose.

[0070] In some embodiments, the thickener may be, for example, styrene-butadiene rubber.

[0071] In some embodiments, the lithium-ion secondary battery includes at least an electrolyte, and the electrolyte can be selected according to actual needs. The electrolyte can be a conventional electrolyte used in secondary batteries in the art, the electrolyte in the electrolyte includes but is not limited to LiPF6, and the solvent in the electrolyte includes but is not limited to one or a combination of two or more of ethylene carbonate, ethyl methyl carbonate and diethyl carbonate.

[0072] Electronic Devices

[0073] The electronic device in the present invention includes the secondary battery according to the second aspect.

[0074] Exemplarily, the electronic device described in the present invention may be, but is not limited to, a mobile device (such as a mobile phone, a tablet computer, a laptop computer, a video recorder, a portable printer / copier, etc.), an electric vehicle (such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship and a satellite, an energy storage system and a backup power supply, etc.

[0075] Unless otherwise specified, the respective parameters involved in this specification have the common meanings known in the art and can be measured by methods known in the art. For example, the test can be performed according to the method given in the embodiments of the present invention. In addition, the preferred schemes and options of various parameters given in various preferred embodiments can be combined arbitrarily, and the various combinations obtained are considered to be within the scope of the disclosure of the present invention. The beneficial effects of the present invention are further described below in conjunction with the embodiments.

[0076] Example 1

[0077] (1) Positive electrode active material

[0078] 75g of LiMn 0.6 Fe 0.395 V 0.005 PO4@1.5%C (i.e., the first particle, where @ represents a core-shell structure, i.e., LiMn 0.6 Fe 0.395 V 0.005 PO4 is the core, C is the shell, and the mass percentage of the shell carbon to the core is 1.5%) and 25g of Li 1.2 Mn 0.595 Ni 0.195 Mg 0.01 The first particles, the second particles and the composite particles (i.e., the third particles) are mixed and wet-grinded, and the solvent is ethanol. Then, spray granulation is performed to obtain a positive electrode active material. The first particles, the second particles and the composite particles (i.e., the third particles) containing the first particles and the second particles are present in the obtained positive electrode active material.

[0079] (2) Positive electrode and negative electrode

[0080] The positive electrode active material, conductive carbon black (Super P) and polyvinylidene fluoride (PVDF) prepared above were mixed in a mass ratio of 97:1.5:1.5, and then nitrogen methyl pyrrolidone (NMP) was gradually added with high-speed stirring to prepare a positive electrode slurry with a certain viscosity. The prepared slurry was then evenly coated on aluminum foil, placed in a blast drying oven at 120°C for 10 minutes, and finally the dried electrode sheet was rolled and cut to make a positive electrode sheet.

[0081] Graphite is used as the negative electrode.

[0082] (3) Lithium-ion battery

[0083] The prepared positive electrode sheet and the graphite negative electrode sheet were assembled into a 1Ah soft pack battery. After liquid injection, a fresh battery cell was obtained after 4.5V formation and aging process.

[0084] The composition of the electrolyte is as follows: 1 mol / L LiPF6 is dispersed in a mixture of 30% ethylene carbonate (EC), 35% ethyl methyl carbonate (EMC) and 35% dimethyl carbonate (DMC).

[0085] The parameters of the first particles and the second particles in the positive electrode active material in Examples 2-30 and Comparative Examples 1-5 are shown in Table 1 below, and the rest is the same as in Example 1. The preparation method of the positive electrode sheet and the lithium ion secondary battery is also the same as in Example 1.

[0086] In the following Examples 1-30, the particle size D50 of the third particles is 5-10 μm.

[0087] The preparation method of the positive electrode active material in Comparative Example 3 is as follows: 75g LiMn 0.6 Fe 0.395 V 0.005 PO4@1.5%C and 25gLi 1.2 Mn 0.595 Ni 0.195 Mg 0.01 O2 dry mixing can obtain the positive electrode material of Comparative Example 3.

[0088] Effect Example 1

[0089] 1. Compressive strength

[0090] The positive electrode active material layer was cut into 1.54 cm 2 The discs were cold pressed at different pressures, and their morphologies were observed using a CP-SEM (Cross Section Polisher-Scanning Electron Microscope). The minimum pressure at which 80% of the third particles with a size of D50±2 μm were broken was the compressive strength.

[0091] 2. Cycle test

[0092] In the range of 2.5-4.2V, charge and discharge were performed at 1C at 45°C for 500 cycles, and the capacity ratio of the 500th cycle to the 1st cycle was recorded as its capacity retention rate.

[0093] 3. Energy density

[0094] At 25°C, the constant-capacity lithium-ion battery is charged and discharged three times in the voltage range of 2V to 4.2V at a charge and discharge rate of 0.3C (calculated based on the mass of the positive electrode material) to obtain the discharge energy of the last cycle. The discharge energy is divided by the mass of the positive electrode material to obtain the weight energy density (unit: Wh / kg).

[0095] 4. Rate performance

[0096] At 25°C, the battery is charged to 4.2V at 0.3C, constant voltage is set to 0.05C, and then discharged to 2.0V at 0.3C to obtain capacity 1. The battery is charged to 4.2V at 0.3C, constant voltage is set to 0.05C, and then discharged to 2.0V at 3C to obtain capacity 2. Capacity 2 / capacity 1 is its rate performance.

[0097] Table 1

[0098]

[0099]

[0100]

[0101]

[0102] Among them, ①“\” indicates that the component is not contained; ②The first particle ratio indicates the mass percentage of all first particles in the positive electrode active material to the positive electrode active material, and the second particle ratio indicates the mass percentage of all second particles in the positive electrode active material to the positive electrode active material.

[0103] According to Table 1, in some preferred embodiments, the ratio of carbon-coated lithium iron phosphate material in the positive electrode active material is controlled to be above 66%, so that the rate performance is significantly improved, and the primary particles of lithium-rich manganese-based material and the primary particles of carbon-coated lithium iron phosphate are further agglomerated into secondary particles, which effectively improves the cycle performance and energy density. Among them, the control of the particle size D50 of the primary particles of lithium-rich manganese-based material takes into account better rate performance and cycle performance.

[0104] Specifically, Comparative Example 1 contains only lithium iron phosphate material, does not contain lithium-rich manganese-based materials, and does not form secondary particles in agglomerated form. Compared with Example 1, not only is the energy density low, but the rate performance and cycle performance are also poor. Comparative Example 2 contains only lithium-rich manganese-based materials, which have high energy density, but significantly reduce rate performance. Although Comparative Example 3 contains two positive electrode active materials, it does not form agglomerates of secondary particles, but is simply a conventional mixture, which ultimately leads to the failure to improve energy density, cycle performance, and rate performance.

[0105] On the basis of the above, the researchers further explored the implementation scheme to obtain better results. In particular, the content of lithium iron phosphate material is in the range of 70%-80%, and the energy density, rate performance and cycle performance are all at an excellent level. In fact, it is well known to those skilled in the art that the rate performance of lithium iron phosphate material is inferior to that of lithium-rich manganese-based materials. Therefore, when the two are mixed, an excessive amount of lithium iron phosphate material is generally not added. The researchers of the present invention unexpectedly discovered that a large amount of lithium iron phosphate material coated with a carbon layer or doped with elements will improve the rate performance. The above embodiments also show that the coating, element content and doping elements of the carbon layer will also significantly affect the performance of various aspects of the secondary battery. In this embodiment, the content of the carbon layer is preferably in the range of 1%-2%. In the lithium iron phosphate material, the content of lithium element is preferably in the range of 1-1.05, which has a significant contribution to energy density, cycle performance and rate performance.

Claims

1. A positive electrode active material, characterized in that: The method comprises a first particle, a second particle and a third particle, wherein the third particle is a composite particle comprising the first particle and the second particle; The first particles include lithium iron phosphate material; the second particles include lithium-rich manganese-based material; The mass percentage of the first particles to the positive electrode active material is 66%-99%.

2. The positive electrode active material according to claim 1, characterized in that The positive electrode active material satisfies one or both of the following conditions: (a) The chemical formula of the lithium iron phosphate material is: Li a Mn x Fe 1-x-y M y PO4; wherein the value of a is 0.9-1.1; the value of x is 0-1.0; the value of y is 0-0.02; M includes one or more of Ti, Mg, Ni, Co, Al, V, Cr, Zr and Nb; (b) The chemical formula of the lithium-rich manganese-based material is Li 1+(b / (2+b)) Mn 2b / (2+b) M (6 / (2+b))-2 O2, wherein the value of b is 0-1 and is not 0, and M includes one or more of Ni, Co, Mn, Mg, Al, Ti, Zr, Nb, La, Sr and W.

3. The positive electrode active material according to claim 2, characterized in that In the chemical formula of the lithium iron phosphate material, the value of a is 1-1.1, the value of x is 0.5-0.8, the value of y is 0.003-0.005, and M is V or Ti.

4. The positive electrode active material according to claim 1, characterized in that The surface of the lithium iron phosphate material is also coated with a carbon layer, and the carbon layer accounts for 1%-2% of the total mass of the lithium iron phosphate material.

5. The positive electrode active material according to claim 1, characterized in that In the chemical formula of the lithium-rich manganese-based material, the stoichiometric number of Li is 1.05-1.4, the stoichiometric number of Mn is 0.5-0.75, the stoichiometric number of M is 0.01-0.45, and M is Ni and / or Mg.

6. The positive electrode active material according to any one of claims 1 to 5, characterized in that The mass percentage of the first particles to the positive electrode active material is 70%-80%.

7. The positive electrode active material according to any one of claims 1 to 5, characterized in that The positive electrode active material satisfies one or both of the following conditions: (a) the D50 particle size of the first particles is 0.3-1.5 μm; (b) The D50 particle size of the second particles is 0.3-0.8 μm.

8. The positive electrode active material according to any one of claims 1 to 5, characterized in that The positive electrode active material satisfies one or more of the following conditions: (a) the D50 particle size of the third particles is 5-10 μm; (b) In the third particles, the total number of the first particles and the second particles is 10-30 / μm 2 ; (c) The compressive strength of the third particles is 5-40 MPa.

9. A secondary battery, characterized in that: It comprises a positive electrode sheet and a negative electrode sheet, wherein the positive electrode sheet comprises a current collector and a positive electrode active material layer arranged on at least one surface of the current collector, and the positive electrode active material layer comprises the positive electrode active material according to any one of claims 1 to 8.

10. An electronic device, characterized in that: It comprises the secondary battery as claimed in claim 9.

Citation Information

Cited By

  • Positive electrode sheet and lithium-ion battery using same

    WO2026157099A1