Sodium-ion battery carbon composite negative electrode active material and preparation method and application thereof

Through the composite material of hard carbon and asphaltene, combined with pore-forming agent and sodium replenishing agent, spray drying and carbonization processes are used to prepare sodium-ion battery carbon composite negative electrode active substances, which solves the problem of poor sodium storage capacity of sodium-ion battery negative electrode materials. It achieves high specific capacity and cycle stability, meeting the high energy density and low cost requirements of sodium ion batteries.

CN119008885APending Publication Date: 2024-11-22SHANDONG QIANTAI TECH RES CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411083869.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Sodium ion batteries require a negative electrode material that can effectively carry sodium ions. Due to the poor sodium storage capacity, slow reaction kinetics and low coverage rate, existing asphaltene materials are difficult to meet the needs of high energy density and low cost.

Method used

Using specific ratios of hard carbon, asphaltene, pore-forming agent, sodium supplementation agent, benzene solvent, wetting agent and crosslinking agent, sodium ion battery carbon composite active substance is prepared through spray drying and carbonization processes to form a core-shell structure , improve the specific surface area and active sites, increase specific capacity and cyclic stability.

Benefits of technology

It achieves high specific capacity, low first-circuit loss rate and excellent cycling performance of sodium ion batteries, improves the electrochemical performance and mechanical strength of the batteries, and adapts to the needs of environmental sustainable development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008885A_ABST
    Figure CN119008885A_ABST
Patent Text Reader

Abstract

The invention provides a carbon composite negative electrode active material of a sodium ion battery as well as a preparation method and application of the carbon composite negative electrode active material. The active material is prepared from the following raw materials: hard carbon, asphaltene, a pore forming agent, a sodium supplementing agent, a benzene solvent, a wetting agent and a cross-linking agent in a mass ratio of (30-70): (15-25): (10-20): (10-20): (10-40): (1.5-3): (5-8). The wetting agent is amino-polyethylene glycol-acrylate; the cross-linking agent is lysine. The hard carbon is selected from one or more of waste engine oil, waste mineral oil and by-product carbon black obtained after lubricating oil is extracted and regenerated from residual oil. The negative electrode active material adopts at least one of waste engine oil, waste mineral oil and residual oil byproduct carbon black as hard carbon, and the hard carbon is compounded with asphaltene soft carbon and the like to form a core-shell structure; the sodium ion battery assembled by the prepared carbon composite negative electrode has good electrochemical performance, such as relatively high first discharge specific capacity, first cycle coulombic efficiency and cycle efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of battery negative electrode materials, and in particular relates to a sodium ion battery carbon composite negative electrode active material and a preparation method and application thereof. Background Art

[0003] Sodium ions have shown great potential in related applications due to their convenient sources, abundant reserves in nature, non-toxicity and chemical stability. It is urgent to develop a low-cost, high-safety alternative to lithium batteries. As an emerging battery technology, sodium ion batteries are gradually entering people's field of vision with their unique advantages and potential.

[0004] The high energy density and low cost of sodium batteries make them a suitable candidate for large-scale energy storage. This is crucial for the sustainable development of energy systems. With higher energy density and lower cost, sodium batteries can replace lithium-ion batteries, reduce dependence on rare and expensive materials, and reduce energy costs. Research on sodium batteries has promoted progress in fields such as materials science, electrochemistry, and engineering. By studying sodium batteries, scientists can better understand basic processes such as ion transport and chemical reactions, and develop new high-performance materials and technologies. Sodium-ion batteries have advantages over lithium-ion batteries in terms of safety, operating temperature, and cycle period. In addition, the over-discharge characteristics of sodium-ion batteries also make them potentially useful in battery transportation.

[0005] However, if sodium-ion batteries want to replace lithium-ion batteries, it is not as simple as replacing lithium ions with sodium ions. Larger than the ionic radius of lithium ions This makes the graphite layer structure that can originally carry lithium ions unsuitable for sodium ions, so if you want to develop sodium-ion batteries, you must find a negative electrode material that can carry sodium ions.

[0006] Asphalt is mainly divided into petroleum asphalt and coal tar asphalt due to different sources and production processes. It has a high carbon atom ratio, is rich in small-sized aromatic molecular compounds, and is composed of aromatic nuclei and side chains. It is easy to form nearly parallel stacked carbon layers during heating, and is an ideal carbon precursor for preparing carbon negative electrodes. Among them, petroleum asphalt is a by-product of heavy oil processing, containing a mixture of hydrocarbons and non-hydrocarbons, mainly composed of carbon, hydrogen, oxygen, sulfur and other elements. In 2022, my country's production was about 39 million tons. Considering the use of petroleum-based asphaltene materials as negative electrode materials for sodium ion batteries, asphaltene has a wider source and lower cost. As of 2022, the global asphaltene reserves are estimated to be 1 to 2 trillion barrels. Due to the characteristics of poor biodegradability, flammability and strong reactivity of asphaltene, its application has become a major problem in the oil industry. In addition to being used as paving materials, natural asphalt is usually used as fuel or discarded in tailings ponds and landfills, resulting in increased costs and waste of resources, while also causing damage to land, water and air. As crude oil continues to become heavier, the output of asphaltene is increasing, and the effective utilization of asphaltene is becoming more and more important. Asphaltene as a negative electrode material for sodium ion batteries is in line with the trend of economic development and is of great significance for solving global environmental and energy problems.

[0007] Soft carbon is an amorphous carbon material with a high degree of graphitization and easy to undergo high graphitization. It is usually converted from raw materials such as petroleum coke, coal coke and asphaltene through a high-temperature heat treatment process. Soft carbon materials are unique among many carbon materials because of their high long-range order, which gives them unique advantages in energy storage applications. When it comes to the charging and discharging process of sodium-ion batteries, soft carbon materials exhibit a similar working mechanism to lithium-ion batteries, that is, they tend to form stable electrode structures for reversible charge transfer. However, despite the similarities in energy storage performance, soft carbon faces the challenge of lower specific capacity when storing sodium ions.

[0008] Asphaltene materials are soft carbon materials with poor sodium storage capacity. Compared with hard carbon materials such as biomass, they have the disadvantages of low active sites and slow reaction kinetics. Therefore, how to modify asphaltene materials so that they can be better used in sodium-ion batteries is a key research topic.

[0009] During the coating process, carbon black particles are easy to combine, precipitate and agglomerate, resulting in a low coating rate. Summary of the invention

[0010] In view of this, the object of the present invention is to provide a carbon composite negative electrode active material for a sodium ion battery and a preparation method and application thereof. The carbon composite negative electrode active material has a high coverage rate, a large specific surface area, and many active sites. The battery assembled with the prepared negative electrode has the advantages of large specific capacity and low first-cycle loss rate.

[0011] The present invention provides a sodium ion battery carbon composite negative electrode active material, wherein the raw materials for preparing the material include hard carbon, asphaltene, a pore former, a sodium supplementing agent, a benzene solvent, a wetting agent and a cross-linking agent in a mass ratio of (30-70):(15-25):(10-20):(10-20):(10-40):(1.5-3):(5-8);

[0012] The hard carbon is selected from one or more of waste engine oil, waste mineral oil and carbon black, a byproduct of lubricating oil extracted from residual oil;

[0013] The wetting agent is amino-polyethylene glycol-acrylate;

[0014] The cross-linking agent is lysine.

[0015] Preferably, the pore-forming agent is urea;

[0016] The sodium supplement is sodium carbonate and / or sodium bicarbonate.

[0017] Preferably, the mass ratio of hard carbon, asphaltene, pore former, sodium supplementer, benzene solvent, wetting agent and crosslinking agent is (30-50):(15-25):(10-20):(10-20):(10-35):(1.5-2.5):(5.5-6.5).

[0018] The present invention provides a method for preparing a carbon composite negative electrode active material for a sodium ion battery as described in the above technical solution, comprising the following steps:

[0019] Mixing hard carbon, asphaltene, pore-forming agent and sodium supplementing agent, adding benzene solvent, wetting agent and cross-linking agent, coating and drying under spraying conditions to obtain dry powder;

[0020] The dry powder and the carbonized support are mixed and then carbonized, and then ground after cooling to obtain a carbon composite negative electrode active material for a sodium ion battery.

[0021] Preferably, the spraying conditions include:

[0022] The pulse interval is 1.4-1.6s, the feed temperature is 70-80℃, the vibrator interval is 4-6s, the inlet air temperature is 140-160℃, the exhaust air temperature is 80-90℃, the homogenization pressure is 18-22MPa, the temperature in the tower is 90-125℃, and the time is 5-10 minutes.

[0023] Preferably, the carbonization process comprises:

[0024] Under an inert atmosphere, the temperature is increased to 440-460°C at a heating rate of 9-11°C / min, and kept at this temperature for 10-300 minutes; then the temperature is continued to be increased to 1000-1500°C at a heating rate of 9-11°C / min, and kept at this temperature for 10-300 minutes.

[0025] Preferably, the carbonized support is a zirconium bead with a particle size of 0.05 to 50 mm.

[0026] Preferably, the mass ratio of the dry powder to the carbonized support is (10-30):(90-70).

[0027] The present invention provides a sodium ion battery carbon composite negative electrode, comprising the sodium ion battery carbon composite negative electrode active material, a binder and a conductive filler according to the above technical solution in a mass ratio of (6-10):(2-3):(1-2).

[0028] The present invention provides a sodium ion battery, comprising the sodium ion battery carbon composite negative electrode described in the above technical solution.

[0029] The present invention provides a carbon composite negative electrode active material for a sodium ion battery, wherein the raw materials include hard carbon, asphaltenes, pore formers, sodium supplementers, solvents, wetting agents and crosslinking agents in a mass ratio of (30-70):(15-25):(10-20):(10-20):(10-40):(1.5-3):(5-8); the hard carbon is selected from one or more of the carbon black byproducts after the extraction of waste engine oil, waste mineral oil and residual oil to regenerate lubricating oil; the wetting agent is amino-polyethylene glycol-acrylate; and the crosslinking agent is lysine. The present invention adopts a specific type of hard carbon, composites it with asphaltenes and soft carbon into a core-shell structure, and works together with pore formers, sodium supplementers, wetting agents and crosslinking agents to make the active material have a large specific surface area and many active sites, and the assembled battery has the advantages of large specific capacity and low first-cycle loss rate. Experimental results show that the specific surface area of ​​the negative electrode is 15.6-31.6m 2 / g, the first discharge specific capacity is 269.4~308.8mAh / g, and the first cycle coulomb efficiency is 82.3~92.5%; the battery's 1000 cycle discharge capacity is 206.9~257.2mAh / g, and the cycle efficiency is 76.8~85.7%. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is the Raman image of the carbon composite negative electrode active material of Example 1;

[0031] Figure 2 This is an electron scanning microscope image of the carbon composite negative electrode active material of Example 4;

[0032] Figure 3 This is the long cycle charge and discharge performance diagram of Example 1. DETAILED DESCRIPTION

[0033] The present invention provides a sodium ion battery carbon composite negative electrode active material, wherein the raw materials for preparing the material include hard carbon, asphaltene, a pore former, a sodium supplementing agent, a solvent, a wetting agent and a cross-linking agent in a mass ratio of (30-70):(15-25):(10-20):(10-20):(10-40):(1.5-3):(5-8);

[0034] The hard carbon is selected from one or more of waste engine oil, waste mineral oil and carbon black, a byproduct of lubricating oil extracted from residual oil;

[0035] The wetting agent is amino-polyethylene glycol-acrylate;

[0036] The cross-linking agent is lysine.

[0037] The carbon composite negative electrode active material of the sodium ion battery provided by the present invention is a core-shell structure, and the capsule core (i.e., core) adopts at least one of the byproduct carbon black of waste oil, waste mineral oil and residual oil, and has the characteristics of low working voltage, high specific capacity, high first-cycle coulomb efficiency, high compaction density, high electronic and ionic conductivity, stable structure (small volume deformation) and air stability, low cost and safety and non-toxicity. The spray drying process is adopted, and the cross-linking agent and wetting agent are used to promote the integrity of the core-shell coating, pore formation is coupled with sodium supplementation, and the capsule wall (i.e., shell) adopts asphalt-based hard carbon negative electrode, which has good electrochemical performance and high specific capacity, and also has excellent cycle resistance and mechanical strength, which is conducive to promoting environmental sustainable development.

[0038] In the present invention, one or more of the byproduct carbon black after waste engine oil, waste mineral oil and residual oil extraction and regeneration of lubricating oil is used as hard carbon, that is, the byproduct carbon black after waste engine oil extraction and regeneration of lubricating oil, the byproduct carbon black after waste mineral oil extraction and regeneration of lubricating oil, or the byproduct carbon black after residual oil extraction and regeneration of lubricating oil; wherein, the byproduct carbon black after residual oil extraction and regeneration of lubricating oil has smaller particles, larger surface area, high specific surface area and porosity, which helps to improve the battery current density and capacity. At the same time, carbon black has excellent chemical stability and electrochemical properties, which can ensure the battery life and stability.

[0039] The asphaltene described in the present invention is common asphalt or asphalt with a softening point of 190°C.

[0040] The pore-forming agent in the present invention is urea; the sodium supplement is sodium carbonate and / or sodium bicarbonate. In the present invention, the negative electrode active material uses urea as a pore-forming agent. In the high temperature range, urea is carbonized and decomposed into ammonia, carbon dioxide and other gases to play a pore-forming role, increase the specific surface area of ​​the powder, and provide more active sites.

[0041] The wetting agent in the present invention is amino-polyethylene glycol-acrylate, specifically selected from model HT-8163 wetting agent, which reasonably disperses the carbon black powder in the toluene solvent through a certain charge repulsion principle or polymer steric hindrance effect, effectively inhibiting the precipitation and agglomeration of carbon black particles.

[0042] The cross-linking agent in the present invention is lysine, which is a small molecule cross-linking agent. The functional group -COOH in the structure is an acidic group, while -NH 2 It is a basic group that links carbon black particles and asphaltene macromolecular chains to increase the coverage rate of carbon black particles.

[0043] The present invention adopts sodium carbonate and / or sodium bicarbonate as sodium supplement, and high temperature products carbon dioxide and sodium oxide are used to bury sodium in the air on the hard carbon surface in advance, so as to improve the problems of excessive loss of specific capacity in the first cycle and low capacity retention rate after cycle.

[0044] The mass ratio of hard carbon, asphaltene, pore former, sodium supplementer, benzene solvent, wetting agent and crosslinking agent in the present invention is (30-70):(15-25):(10-20):(10-20):(10-40):(1.5-3):(5-8). In a specific embodiment, the mass ratio of the hard carbon, asphaltene, pore former, sodium supplement, benzene solvent, wetting agent and cross-linking agent is 30:15:10:10:27:2:6; or the mass ratio of the hard carbon, asphaltene, pore former, sodium supplement, benzene solvent, wetting agent and cross-linking agent is 30:15:10:10:26:2:7; or the mass ratio of the hard carbon, asphaltene, pore former, sodium supplement, benzene solvent, wetting agent and cross-linking agent is 37:15:10:10:20:2:6; or the mass ratio of the hard carbon, asphaltene, pore former, sodium supplement, benzene solvent, wetting agent and cross-linking agent is 30:22:10:10:20:2:6; or the mass ratio of the hard carbon, asphaltene, pore former, sodium supplement, benzene solvent, wetting agent and cross-linking agent is 30:20:10:10:22:2:6.

[0045] The present invention provides a method for preparing the carbon composite negative electrode active material for a sodium ion battery according to the above technical solution, comprising the following steps:

[0046] Mixing hard carbon, asphaltene, pore-forming agent and sodium supplementing agent, adding benzene solvent, wetting agent and cross-linking agent, coating and drying under spraying conditions to obtain dry powder;

[0047] The dry powder and the carbonized support are mixed and then carbonized, and then ground after cooling to obtain a carbon composite negative electrode active material for a sodium ion battery.

[0048] The method provided by the present invention uses a spray drying method to complete the coating and drying. The spray dryer uses a spraying method to disperse the material into tiny droplets, thereby increasing the contact area between the material and the hot air and accelerating the drying speed. The spray drying has the advantages of high efficiency, strong adaptability, good product quality, simple operation, energy saving and environmental protection.

[0049] The benzene solvent described in the present invention can dissolve asphaltene, making it easier to coat hard carbon and the coating is uniform; the benzene solvent is toluene, ethylbenzene and the like.

[0050] The conditions described in the present invention include:

[0051] The pulse interval is 1.4-1.6s, the feed temperature is 70-80℃, the vibrator interval is 4-6s, the inlet air temperature is 140-160℃, the exhaust air temperature is 80-90℃, the homogenization pressure is 18-22MPa, the temperature in the tower is 90-125℃, and the time is 5-10 minutes.

[0052] In a specific embodiment, the spray conditions include:

[0053] The pulse interval is 1.5 seconds, the feed temperature is 75°C, the vibrator interval is 5 seconds, the inlet air temperature is 150°C, the exhaust air temperature is 85°C, the homogenizer pressure is 20Mpa, the tower temperature is 90°C, and the time is 10 minutes.

[0054] After obtaining the dry powder, the present invention mixes the dry powder with a carbonized support and then carbonizes the mixture, and grinds the mixture after cooling to obtain a carbon composite negative electrode active material for a sodium ion battery.

[0055] The carbonized support in the present invention is a zirconium bead with a particle size of 0.05 to 50 mm; the mass ratio of the dry powder to the carbonized support is (10 to 30): (90 to 70). In a specific embodiment, the mass ratio of the dry powder to the carbonized support is 1:4.

[0056] The carbonization process of the present invention comprises:

[0057] Under an inert atmosphere, the temperature is increased to 440-460°C at a heating rate of 9-11°C / min, and kept at this temperature for 10-300 minutes; then the temperature is continued to be increased to 1000-1500°C at a heating rate of 9-11°C / min, and kept at this temperature for 10-300 minutes.

[0058] The carbonization process of the present invention preferably includes:

[0059] In N 2 In the atmosphere, the temperature was raised to 450°C at a rate of 10°C / min and kept at that temperature for 50 to 150 min; the temperature was then raised to 1200°C at a rate of 10°C / min and kept at that temperature for 30 to 100 min.

[0060] In a specific embodiment, the carbonization process includes:

[0061] In N 2 In the atmosphere, the temperature was raised to 450°C at a rate of 10°C / min and kept at that temperature for 100min; then the temperature was further raised to 1200°C at a rate of 10°C / min and kept at that temperature for 30min.

[0062] After the carbonization is completed, the method is cooled to room temperature to obtain a hard carbon negative electrode active material block; and then the hard carbon negative electrode active material is further ground to obtain a sodium ion battery carbon composite negative electrode active material.

[0063] The present invention provides a sodium ion battery carbon composite negative electrode, comprising the sodium ion battery carbon composite negative electrode active material, a binder and a conductive filler according to the above technical solution in a mass ratio of (6-10):(2-3):(1-2).

[0064] The binder in the present invention is selected from polyvinylidene fluoride; the conductive filler is selected from conductive carbon black, and the particle size is 1 to 10 μm. In a specific embodiment, the mass ratio of the carbon composite negative electrode active material, the binder and the conductive filler of the sodium ion battery is 7:2:1.

[0065] In the present invention, after the negative electrode active material, the binder and the conductive filler are mixed, a solvent accounting for 18 to 22% of the mass of the powder is added; the solvent is preferably N-methylpyrrolidone.

[0066] The slurry obtained above is coated on the current collector, which is aluminum foil. After drying, it is cut into discs and used as negative electrode plates. The loading amount of active material on each plate is 1-2 mg / m 2 .

[0067] The present invention provides a sodium ion battery, comprising the sodium ion battery carbon composite negative electrode described in the above technical solution.

[0068] The sodium ion battery provided by the present invention has a large specific capacity and a small loss rate because soft and hard carbon composite negative electrode powder is used in the negative electrode.

[0069] In order to further illustrate the present invention, a sodium ion battery carbon composite negative electrode active material and its preparation method and application provided by the present invention are described in detail below in combination with embodiments, but they should not be understood as limiting the scope of protection of the present invention.

[0070] Example 1

[0071] In parts by weight, 30 parts of hard carbon, 15 parts of ordinary asphalt, 10 parts of pore-forming agent, and 10 parts of sodium supplement are fully mixed, stirred and ground evenly. Continue to add 27 parts of toluene, 2 parts of wetting agent HT-8163, and 6 parts of cross-linking agent lysine and stir evenly. Complete the coating drying process in a spray dryer, set the pulse interval to 1.5 seconds, the feed temperature to 75°C, the vibrator interval to 5 seconds, the inlet temperature to 150°C, the exhaust temperature to 85°C, the homogenizer pressure to 20Mpa, the tower temperature to 90°C, and the time to 10 minutes. The collected dry powder was transferred to an alumina porcelain boat, and zirconium beads as carbonization support were added. The mass ratio of dry powder to zirconium beads was 1:4, and the mixture was fully mixed. The mixture was carbonized in a tubular heating furnace under argon protection, and the temperature was increased to 450°C at a heating rate of 10°C / min, and kept warm for 100 minutes; the temperature was then increased to 1200°C at a heating rate of 10°C / min, and kept warm for 30 minutes; the mixture was cooled to room temperature to obtain a hard carbon negative electrode active material block; the mixture was fully ground and passed through a 400-mesh sieve to obtain a carbon composite negative electrode active material powder. The tested ash content was 0.05%, the moisture content was 0.02%, and the tap density was 0.82g / cm 3 .

[0072] The negative electrode active material glass powder, binder (polyvinylidene fluoride), and conductive carbon black (particle size distribution 1-10μm) powder are mixed in a mass ratio of 7:2:1, and then an appropriate amount of solvent N-methylpyrrolidone (accounting for 20wt% of the powder) is dropped into the ball mill. The resulting slurry is coated on aluminum foil and dried. After vacuum drying at 60°C for 12 hours, it is cut into discs with a diameter of 12mm and used as negative electrodes. The loading of active material on each pole piece is about 2mg / m 2 The sodium sheet was used as the reference electrode, and the weighed electrode, CR2032 battery case, diaphragm (glass fiber, Whatman) and nickel foam were placed in an argon-filled glove box. The concentration of NaPF was 1 mol / L during the battery assembly process. 6 The electrolyte, whose solvent is ethylene carbonate (EC) and dimethyl carbonate (DMC) (volume ratio 1:1), was prepared together in an argon-filled glove box (H 2 O<0.1ppm, O 2 <0.1ppm) to prepare CR2032 button cells. The battery cycle performance was tested at a current density of 0.1A / g using a LAND CT3001A battery test system.

[0073] Embodiments 2 to 5

[0074] According to the preparation process of Example 1, carbon composite negative electrode active material powder was prepared using hard carbon, asphaltene, pore former, sodium supplement agent, benzene solvent, wetting agent and cross-linking agent of different masses shown in Table 1.

[0075] Table 1 Types and amounts of raw materials used in Examples 1 to 5

[0076]

[0077]

[0078] The present invention tests the performance of the sodium ion battery assembled with the negative electrode material prepared in the embodiment, and the results are shown in Table 2 at a current density of 0.1 A / g:

[0079] Table 2 Performance test results of the battery prepared in Example

[0080]

[0081] Comparative Example 1

[0082] Grind 0.05g of Ketjen black finely; grind 1g of coal tar pitch finely and dissolve it in 30mL of dichloromethane, evenly disperse and mix it with the finely ground Ketjen black, dry and remove dichloromethane to obtain a mixture of asphalt and Ketjen black; under an argon atmosphere, put the mixture of asphalt and Ketjen black into a tubular furnace and heat it at a temperature program of 5℃ / min to 200℃ and stay for 2h; then heat it to 1400℃ at 5℃ / min and stay for 2h; after cooling to room temperature, grind it finely to obtain an asphalt-based hard carbon sodium ion battery negative electrode material.

[0083] Weigh 0.45g of the asphalt-based hard carbon prepared above and 0.05g of the binder (CMC) slurry and evenly apply them on the aluminum foil. After vacuum drying at 80°C for 12h, take out the punched sheet. In a glove box protected by high-purity argon, use the prepared electrode and metal sodium sheet as the counter electrode, glass fiber diaphragm, and the electrolyte solvent is NaPF 6 Ester electrolyte, without any other additives, assembled into 2032 button cells. Electrochemical sodium storage performance test was carried out at room temperature with a voltage range of 0-3V. The sample was tested for battery cycle performance at a current density of 0.1A / g.

[0084] Comparative Example 2

[0085] Add 1.5g of asphalt and 1.5g of calcium gluconate into a mortar and grind manually for 30 minutes to evenly mix the two to obtain a raw carbon source; place the raw carbon source in a high-temperature furnace, heat it to 450°C at a rate of 5°C / min under an argon atmosphere and keep it warm for 1 hour. The resulting product is pickled with a 1 mol / L hydrochloric acid solution, and then centrifuged and washed until the filtered water is pH neutral, then dried and ground into fine powder to obtain a precursor; place the precursor in a high-temperature furnace, heat it to 1200°C at a rate of 10°C / min under an argon atmosphere and keep it warm for 2 hours, cool it, and grind it into fine powder to obtain a sodium ion battery modified asphalt-based hard carbon material.

[0086] The modified asphalt-based hard carbon material was used as the negative electrode material to assemble a half-cell, and the electrochemical performance of the asphalt-based carbon negative electrode material modified by different gluconic acid-based metal salts was compared. To ensure sufficient sodium ions, the half-cell used a sodium metal disc as the counter electrode, and the electrolyte used a concentration of 1moL / LNaPF 6 The electrolyte dosage was 160 μL, and the loading amount of active material on the negative electrode was controlled to be 2 mg cm -2 The assembled battery was tested for its cycle performance at a current density of 0.1 A / g.

[0087] Comparative Example 3 (Put in a vacuum drying oven for drying)

[0088] In parts by weight, 30 parts of carbon black, a byproduct of the extraction of regenerated lubricating oil from waste oil, 15 parts of ordinary asphalt, 10 parts of pore-forming agent, and 10 parts of sodium supplement are fully mixed, stirred and ground evenly and placed in an alumina porcelain boat. Continue to add 27 parts of toluene, 2 parts of wetting agent HT-8163, and 6 parts of cross-linking agent lysine and stir evenly. Continue to add 150 parts of carbonized support zirconium beads, mix thoroughly, and place in a vacuum drying oven to dry. The alumina porcelain boat is placed in a tubular heating furnace, carbonized under argon protection, heated to 450°C at a heating rate of 10°C / min, and kept warm for 100min; then heated to 1200°C at a heating rate of 10°C / min, and kept warm for 30min; cooled to room temperature to obtain a hard carbon negative electrode active material block; fully ground, passed through a 400-mesh sieve, and obtained a carbon composite negative electrode active material powder.

[0089] The negative electrode active material glass powder, binder (polyvinylidene fluoride), and conductive carbon black (particle size distribution 1-10μm) powder are mixed in a mass ratio of 7:2:1, and then an appropriate amount of solvent N-methylpyrrolidone (accounting for 20wt% of the powder) is dropped into the ball mill. The resulting slurry is coated on aluminum foil and dried. After vacuum drying at 60°C for 12 hours, it is cut into discs with a diameter of 12mm and used as negative electrodes. The loading of active material on each pole piece is about 2mg / m 2 The sodium sheet was used as the reference electrode, and the weighed electrode, CR2032 battery case, diaphragm (glass fiber, Whatman) and nickel foam were placed in an argon-filled glove box. The concentration of NaPF was 1 mol / L during the battery assembly process. 6 The electrolyte, whose solvent is ethylene carbonate (EC) and dimethyl carbonate (DMC) (volume ratio 1:1), was prepared together in an argon-filled glove box (H 2 O<0.1ppm, O 2 <0.1ppm) was used to prepare CR2032 button cells. The battery cycle performance was tested at a current density of 0.1A / g using a LAND CT3001A battery test system.

[0090] Comparative Example 4 (without wetting agent)

[0091] In parts by weight, 30 parts of carbon black, a byproduct of waste oil extraction and regeneration of lubricating oil, 15 parts of ordinary asphalt, 10 parts of pore-forming agent, and 10 parts of sodium supplement are fully mixed, stirred and ground evenly. Continue to add 29 parts of toluene and 6 parts of cross-linking agent and stir evenly. Complete the coating drying process in a spray dryer, set the pulse interval to 1.5 seconds, the feed temperature to 75°C, the vibrator interval to 5 seconds, the inlet temperature to 150°C, the exhaust temperature to 85°C, the homogenizer pressure to 20Mpa, the tower temperature to 90°C, and the time to 10 minutes. The collected dry powder was transferred to an alumina porcelain boat, and zirconium beads as a carbonization support were added. The mass ratio of dry powder to zirconium beads was 1:4, and the mixture was carbonized in a tubular heating furnace under argon protection. The temperature was increased to 450°C at a heating rate of 10°C / min and kept warm for 100 minutes; the temperature was then increased to 1200°C at a heating rate of 10°C / min and kept warm for 30 minutes; the mixture was cooled to room temperature to obtain a hard carbon negative electrode active material block; the mixture was fully ground and passed through a 400-mesh sieve to obtain a carbon composite negative electrode active material powder.

[0092] The negative electrode active material glass powder, binder (polyvinylidene fluoride), and conductive carbon black (particle size distribution 1-10μm) powder are mixed in a mass ratio of 7:2:1, and then an appropriate amount of solvent N-methylpyrrolidone (accounting for 20wt% of the powder) is dropped into the ball mill. The resulting slurry is coated on aluminum foil and dried. After vacuum drying at 60°C for 12 hours, it is cut into discs with a diameter of 12mm and used as negative electrodes. The loading of active material on each pole piece is about 2mg / m 2 The sodium sheet was used as the reference electrode, and the weighed electrode, CR2032 battery case, diaphragm (glass fiber, Whatman) and nickel foam were placed in an argon-filled glove box. The concentration of NaPF was 1 mol / L during the battery assembly process. 6 The electrolyte, whose solvent is ethylene carbonate (EC) and dimethyl carbonate (DMC) (volume ratio 1:1), was prepared together in an argon-filled glove box (H 2 O<0.1ppm, O 2 <0.1ppm) to prepare CR2032 button cells. The battery cycle performance was tested at a current density of 0.1A / g using a LAND CT3001A battery test system.

[0093] Comparative Example 5 (without crosslinking agent)

[0094] In parts by weight, 30 parts of carbon black, a byproduct of lubricating oil extracted from waste oil, 15 parts of ordinary asphalt, 10 parts of pore-forming agent urea, and 10 parts of sodium carbonate supplement were fully mixed and stirred and ground evenly. 33 parts of toluene and 2 parts of wetting agent HT-8163 were added and stirred evenly. The coating drying process was completed in a spray dryer, with a pulse interval of 1.5 seconds, a feed temperature of 75°C, a vibrator interval of 5 seconds, an inlet air temperature of 150°C, an exhaust air temperature of 85°C, a homogenizer pressure of 20Mpa, a tower temperature of 90°C, and a time of 10 minutes. The collected dry powder was transferred to an alumina porcelain boat and fully mixed with a carbonization support, and carbonized in a tubular heating furnace under argon protection. The temperature was increased to 450°C at a heating rate of 10°C / min and kept warm for 100 minutes; then the temperature was increased to 1200°C at a heating rate of 10°C / min and kept warm for 30 minutes; cooled to room temperature to obtain a hard carbon negative electrode active material block; fully ground and passed through a 400-mesh sieve to obtain a carbon composite negative electrode active material powder.

[0095] The negative electrode active material glass powder, binder (polyvinylidene fluoride), and conductive carbon black (particle size distribution 1-10μm) powder are mixed in a mass ratio of 7:2:1, and then an appropriate amount of solvent N-methylpyrrolidone (accounting for 20wt% of the powder) is dropped into the ball mill. The resulting slurry is coated on aluminum foil and dried. After vacuum drying at 60°C for 12 hours, it is cut into discs with a diameter of 12mm and used as negative electrodes. The loading of active material on each pole piece is about 2mg / m 2 The sodium sheet was used as the reference electrode, and the weighed electrode, CR2032 battery case, diaphragm (glass fiber, Whatman) and nickel foam were placed in an argon-filled glove box. The concentration of NaPF was 1 mol / L during the battery assembly process. 6 The electrolyte, whose solvent is ethylene carbonate (EC) and dimethyl carbonate (DMC) (volume ratio 1:1), was prepared together in an argon-filled glove box (H 2 O<0.1ppm, O 2 <0.1ppm) to prepare CR2032 button cells. The battery cycle performance was tested at a current density of 0.1A / g using a LAND CT3001A battery test system.

[0096] The performance of the sodium ion battery assembled with the negative electrode material prepared in the comparative example of the present invention was tested at a current density of 0.1 A / g. The results are shown in Table 3:

[0097] Table 3 Performance test results of batteries prepared in comparative example

[0098]

[0099] As can be seen from the above embodiments, the present invention provides a carbon composite negative electrode active material for a sodium ion battery, wherein the raw materials include hard carbon, asphaltene, pore forming agent, sodium supplement agent, benzene solvent, wetting agent and cross-linking agent in a mass ratio of (30-70):(15-25):(10-20):(10-20):(30-40):(1.5-3):(5-8); the hard carbon is selected from one or more of the carbon black byproducts of waste engine oil, waste mineral oil and residual oil after extraction and regeneration of lubricating oil; the wetting agent is amino-polyethylene glycol-acrylate; and the cross-linking agent is lysine. The negative electrode active material uses at least one of the carbon black byproducts of waste engine oil, waste mineral oil and residual oil as hard carbon, and forms a core-shell structure with asphaltene soft carbon, etc., adopts a spray drying process, and the cross-linking agent and wetting agent promote the integrity of the core-shell coating, and the pore forming is coupled with sodium supplementation, so that the sodium ion battery assembled with the prepared carbon composite negative electrode has good electrochemical performance: higher first discharge specific capacity, first cycle coulomb efficiency and cycle efficiency, etc. The experimental results show that the specific surface area of ​​the negative electrode is 15.6~31.6m 2 / g, the first discharge specific capacity is 269.4~308.8mAh / g, and the first cycle coulomb efficiency is 82.3~92.5%; the battery's 1000 cycle discharge capacity is 206.9~257.2mAh / g, and the cycle efficiency is 76.8~85.7%.

[0100] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A carbon composite negative electrode active material for a sodium ion battery, wherein the raw materials for preparation include hard carbon, asphaltene, a pore former, a sodium supplement, a benzene solvent, a wetting agent and a cross-linking agent in a mass ratio of (30-70):(15-25):(10-20):(10-20):(10-40):(1.5-3):(5-8); The hard carbon is selected from one or more of waste engine oil, waste mineral oil and carbon black, a byproduct of lubricating oil extracted from residual oil; The wetting agent is amino-polyethylene glycol-acrylate; The cross-linking agent is lysine.

2. The carbon composite negative electrode active material for sodium ion battery according to claim 1, characterized in that: The pore-forming agent is urea; The sodium supplement is sodium carbonate and / or sodium bicarbonate.

3. The carbon composite negative electrode active material for sodium ion batteries according to claim 1, characterized in that: The mass ratio of hard carbon, asphaltene, pore former, sodium supplementer, benzene solvent, wetting agent and cross-linking agent is (30-50):(15-25):(10-20):(10-20):(10-35):(1.5-2.5):(5.5-6.5).

4. A method for preparing a carbon composite negative electrode active material for a sodium ion battery according to any one of claims 1 to 3, comprising the following steps: Mixing hard carbon, asphaltene, pore-forming agent and sodium supplementing agent, adding benzene solvent, wetting agent and cross-linking agent, coating and drying under spraying conditions to obtain dry powder; The dry powder and the carbonized support are mixed and then carbonized, and then ground after cooling to obtain a carbon composite negative electrode active material for a sodium ion battery.

5. The preparation method according to claim 4, characterized in that: The spray conditions include: The pulse interval is 1.4-1.6s, the feed temperature is 70-80℃, the vibrator interval is 4-6s, the inlet air temperature is 140-160℃, the exhaust air temperature is 80-90℃, the homogenization pressure is 18-22MPa, the temperature in the tower is 90-125℃, and the time is 5-10 minutes.

6. The preparation method according to claim 4, characterized in that: The carbonization process includes: Under an inert atmosphere, the temperature is increased to 440-460°C at a heating rate of 9-11°C / min, and kept at this temperature for 10-300 minutes; then the temperature is continued to be increased to 1000-1500°C at a heating rate of 9-11°C / min, and kept at this temperature for 10-300 minutes.

7. The preparation method according to claim 4, characterized in that: The carbonized support is a zirconium bead with a particle size of 0.05 to 50 mm.

8. The preparation method according to claim 4, characterized in that: The mass ratio of the dry powder to the carbonized support is (10-30):(90-70).

9. A sodium ion battery carbon composite negative electrode, comprising the sodium ion battery carbon composite negative electrode active material according to any one of claims 1 to 3, a binder and a conductive filler in a mass ratio of (6-10): (2-3): (1-2).

10. A sodium ion battery, comprising the sodium ion battery carbon composite negative electrode according to claim 9.

Citation Information

Cited By

  • Preparation method of spherical pitch-based hard carbon and sodium ion battery

    CN120463195A