Lithium-rich manganese-based positive electrode material, preparation method thereof and battery
By increasing the supercrystalline structural phase content and doping sodium or potassium elements, the problem of structural transformation and lithium-nickel mixed discharge of traditional lithium-rich manganese-based positive electrode materials during the charge and discharge cycle is solved, and high specific capacity and cycle stability are achieved. Improved, extending the storage period of materials.
Patent Information
- Application Number
- CN202411131091.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-22
AI Technical Summary
Traditional lithium-rich manganese-based positive electrode materials have layered structure transformation, transition metal migration and lithium-nickel mixed discharge phenomena during the charge and discharge cycle, resulting in low efficiency and fast capacity decay for the first time, limiting their large-scale application.
By increasing the content of the supercrystalline structural phase and doping sodium or potassium elements, the chemical formula of the lithium-rich manganese-based positive electrode material is Li1+nMmNixCoyMn(1-x-y-n-m)O2, and the mass content of the supercrystalline structural phase is controlled at 30% ~50%, to enhance the entry of lithium ions into the transition metal layer, form a locally lithiated and stabilize the lattice structure, and at the same time, sodium or potassium elements are inserted into the lithium layer to provide a pillar effect to inhibit transition metal migration.
It significantly improves the specific capacity, cycle stability and electrochemical properties of the positive electrode material, extends the storage period of the material, avoids the mixed discharge of lithium and nickel, and enhances the structural stability of the material under high voltage.
Smart Images

Figure CN119008928A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium-rich manganese-based positive electrode materials, and in particular to a lithium-rich manganese-based positive electrode material and a preparation method thereof and a battery. Background Art
[0002] With the development of portable electronic products and electric vehicles, there is an urgent need for high energy density lithium-ion batteries. The main factor affecting high energy density lithium-ion batteries is the high capacity of the cathode material. Lithium-rich manganese-based cathode materials are considered to be the most promising next-generation lithium-ion battery cathode materials due to their many advantages such as high capacity and low cost.
[0003] However, traditional lithium-rich manganese-based positive electrode materials will undergo layered structure transformation to spinel phase, the appearance of rock salt phase, and transition metal migration during the charge and discharge cycle, resulting in low first coulombic efficiency and rapid capacity decay in lithium-rich manganese-based positive electrode materials, which seriously hinders the large-scale application of lithium-rich manganese-based positive electrode materials.
[0004] In order to solve the problems faced by lithium-rich manganese-based positive electrode materials, the existing technology generally increases the specific capacity of the positive electrode material at high voltage by adjusting the lithium content in the transition metal layer of the lithium-rich manganese-based positive electrode material. However, in fact, excessive lithium is not easy to enter the transition metal layer of the positive electrode material, but is easily accumulated on the surface of the positive electrode material to form residual alkali, thereby seriously affecting the electrochemical performance of the positive electrode material. Summary of the invention
[0005] In order to improve the above problems existing in the prior art, the present invention provides a lithium-rich manganese-based positive electrode material, a method for preparing the lithium-rich manganese-based positive electrode material, and a battery comprising the lithium-rich manganese-based positive electrode material. The lithium-rich manganese-based positive electrode material of the present invention has high specific capacity, high initial efficiency and stable cycle performance, and significantly improves the electrochemical performance of the lithium-rich manganese-based positive electrode material.
[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0007] The first aspect of the present invention provides a lithium-rich manganese-based positive electrode material, the chemical formula of the lithium-rich manganese-based positive electrode material is Li 1+n M m Ni x Co y Mn (1-x-y-n-m) O2, wherein 0≤n+m≤1, 0≤x≤1, 0≤y≤1, and the M element includes at least one of sodium and potassium;
[0008] The lithium-rich manganese-based positive electrode material comprises a transition metal layer and a lithium layer, the transition metal layer comprises a supercrystalline structure phase with a lattice diffraction peak located at 20° to 25°, and the lithium layer contains the M element;
[0009] Based on the total mass of the lithium-rich manganese-based positive electrode material, the mass content of the supercrystalline structure phase is 30% to 50%.
[0010] The second aspect of the present invention provides a method for preparing the lithium-rich manganese-based positive electrode material according to the first aspect of the present invention, comprising:
[0011] (1) uniformly mixing powders of a lithium-rich manganese-based precursor, a lithium salt and a M salt;
[0012] (2) performing a first sintering of the material obtained in step (1) under an inert atmosphere, and then heating the material for a second sintering;
[0013] (3) The material obtained in step (2) is subjected to a third sintering in an air atmosphere to obtain the lithium-rich manganese-based positive electrode material.
[0014] The third aspect of the present invention provides a battery, the battery comprising a positive electrode, the positive electrode comprising the lithium-rich manganese-based positive electrode material described in the first aspect of the present invention or the lithium-rich manganese-based positive electrode material prepared by the preparation method of the lithium-rich manganese-based positive electrode material described in the second aspect of the present invention.
[0015] Through the above technical solution, the present invention has at least the following advantages compared with the prior art:
[0016] (1) The present invention can effectively improve the specific capacity of the positive electrode material by increasing the content of the supercrystalline structure phase (Li2MnO3) in the lithium-rich manganese-based positive electrode material. The higher the content of the supercrystalline structure phase, the more lithium enters the transition metal layer, so that excess lithium ions can migrate into the transition metal layer to form local lithium-enriched positive electrode materials, thereby playing a role in pinning the lattice structure, stabilizing the material structure during the delithiation process, and further improving the long-term cycle performance of the positive electrode material. Moreover, the more lithium ions exist in the form of the supercrystalline structure phase, the more lithium ions enter the transition metal layer, and the residual alkali on the surface of the positive electrode material is correspondingly reduced, thereby extending the storage period of the material and effectively improving the electrochemical performance of the lithium-rich manganese-based positive electrode material.
[0017] (2) By doping sodium and / or potassium elements into the lithium-rich manganese-based positive electrode material of the present invention, the lithium-nickel mixing phenomenon caused by transition metal reduction can be avoided, so that an appropriate amount of sodium ions and / or potassium atoms are inserted into the lithium layer to play a pillar effect and expand the transmission channel of lithium ions, which not only allows lithium ions to be smoothly embedded and released during the charge and discharge process of the positive electrode material, but also makes its structure more stable, thereby improving the cycle stability of the lithium-rich manganese-based positive electrode material.
[0018] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 Scanning electron microscope image of the lithium-rich manganese-based positive electrode material synthesized in Example 1 of the present invention;
[0020] Figure 2 The cross-sectional morphology scanning electron microscope image and element distribution surface scanning image of the lithium-rich manganese-based positive electrode material synthesized in Example 1 of the present invention;
[0021] Figure 3 XRD pattern of the lithium-rich manganese-based positive electrode material synthesized in Example 1 of the present invention. DETAILED DESCRIPTION
[0022] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0023] When the mixture of lithium-rich manganese-based precursor and lithium salt is prepared into lithium-rich manganese-based positive electrode materials during the high-temperature sintering stage, the excessive lithium ions need to overcome certain potential barriers to be embedded in the transition metal layer, so this part of the excess lithium ions is more likely to accumulate on the surface of the material to form residual alkali rather than migrate into the transition metal layer. However, the capacity of lithium-rich manganese-based positive electrode materials mainly depends on the content of excess lithium entering the transition metal layer. Therefore, if the excess lithium ions cannot be embedded into the transition metal ions, it will seriously affect the specific capacity of the lithium-rich manganese-based positive electrode materials. At the same time, the large amount of residual alkali accumulated on its surface will also make the storage environment requirements of the positive electrode materials more stringent, increase the material cost, and have many effects on the subsequent slurry preparation and the electrochemical performance of the positive electrode materials, and even cause battery safety problems. Therefore, how to effectively increase the number of lithium ions entering the transition metal layer of lithium-rich manganese-based positive electrode materials during the solid phase sintering stage so that it is not easy to form a large amount of residual alkali on its surface is one of the main problems that need to be solved at present; in addition, it is also necessary to develop lithium-rich manganese-based positive electrode materials with more stable structure and performance under high voltage, and effectively improve their specific capacity and cycle stability.
[0024] Based on the problems existing in the above-mentioned prior art, the first aspect of the present invention provides a lithium-rich manganese-based positive electrode material, the chemical formula of the lithium-rich manganese-based positive electrode material is Li 1+n M m Ni x Co y Mn(1-x-y-n-m) O2, wherein 0≤n+m≤1 (for example, 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9), 0≤x≤1 (for example, 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9), 0≤y≤1 (for example, 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9), and the M element includes at least one of sodium and potassium;
[0025] The lithium-rich manganese-based positive electrode material comprises a transition metal layer and a lithium layer, the transition metal layer comprises a supercrystalline structure phase having a lattice diffraction peak located at 20° to 25° (for example: 20°, 20.5°, 21°, 21.5°, 22°, 22.5°, 23°, 23.5°, 24°, 24.5°, 25°), and the lithium layer contains the M element; based on the total mass of the lithium-rich manganese-based positive electrode material, the mass content of the supercrystalline structure phase is 30% to 50%, and exemplarily, the mass content of the supercrystalline structure phase can be 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%.
[0026] The present invention increases the content of the supercrystalline structure phase (Li2MnO3) in the lithium-rich manganese-based positive electrode material so that the mass content of the supercrystalline structure phase in the lithium-rich manganese-based positive electrode material is 30% to 50%, which can effectively increase the amount of lithium ions entering the transition metal layer, thereby improving the specific capacity of the positive electrode material. The higher the content of the supercrystalline structure phase, the more lithium enters the transition metal layer, indicating that most of the excess lithium ions have migrated into the transition metal layer during the high-temperature sintering process to prepare the lithium-rich manganese-based positive electrode material, and exist in the form of a supercrystalline structure phase, forming local lithium-enriched positive electrode material, thereby playing a role in pinning the lattice structure, stabilizing the material structure and chemical properties during the delithiation process, and thus improving the cyclic stability of the positive electrode material under long cycles. Moreover, the more lithium ions exist in the form of the supercrystalline structure phase, the more lithium ions enter the transition metal layer, and the amount of residual alkali on the surface of the positive electrode material is correspondingly reduced, thereby extending the storage period of the material and effectively improving the electrochemical properties of the lithium-rich manganese-based positive electrode material.
[0027] Furthermore, the appropriate amount of sodium and / or potassium doped into the lithium-rich manganese-based positive electrode material of the present invention can play a pillar effect. This is because the ionic radius of sodium and / or potassium is larger than that of lithium ions. Therefore, when they are doped into the lithium-rich manganese-based positive electrode material, an appropriate amount of sodium and / or potassium ions will be inserted into the lithium layer, which can play a "pillar" role, inhibiting the collapse of the layered structure during deep delithiation (high voltage), and maintaining the structural stability of the positive electrode material. Moreover, due to their larger ionic radius, they can increase the interlayer spacing of the positive electrode material, which is conducive to the deintercalation of lithium ions, increases the diffusion coefficient of lithium and improves the rate performance of the lithium-rich manganese-based positive electrode material; moreover, they can expand the transmission channel of lithium ions, which not only allows lithium ions to be smoothly inserted and removed from the positive electrode material during the charge and discharge process, but also makes its structure more stable, further improving the cycle stability of the lithium-rich manganese-based positive electrode material.
[0028] Furthermore, the huge electron cloud formed by the more extranuclear electrons possessed by sodium and / or potassium elements can effectively inhibit the migration of transition metals through electrostatic repulsion and magnetic interaction, thereby weakening the mixing and phase transition of lithium ions / nickel ions, avoiding the lithium-nickel mixing phenomenon caused by transition metal reduction, and further improving the cycle stability of lithium-rich manganese-based positive electrode materials.
[0029] In summary, the present invention controls the content of the supercrystalline structure phase (Li2MnO3) in the lithium-rich manganese-based positive electrode material and designs to add sodium and / or potassium elements as lithium layer doping, so that the lithium-rich manganese-based positive electrode material can not only exhibit a significant specific capacity, but also ensure that it exhibits excellent long-cycle stability, and significantly improves the electrochemical properties of the lithium-rich manganese-based positive electrode material.
[0030] In the present invention, based on the total mass of the lithium-rich manganese-based positive electrode material, the mass content of the supercrystalline structure phase is 30% to 50%. Exemplarily, the mass content of the supercrystalline structure phase can be 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, or 50%. The more the content of Li2MnO3 supercrystalline structure phase, the more lithium enters the transition metal layer, and the more capacity can be released under high voltage. Therefore, the more the proportion of supercrystalline structure phase in the material, the higher the specific capacity of the positive electrode material. However, the mass content of supercrystalline structure phase should not be too high. This is mainly due to the low electronic conductivity of supercrystalline structure phase. Too much supercrystalline structure phase will inevitably reduce the electronic conductivity of lithium-rich manganese-based overall material, thereby affecting the electrochemical properties of lithium-rich manganese-based positive electrode material. When the mass content of supercrystalline structure phase is too low, it means that the amount of lithium ions entering the transition metal layer is relatively small, which affects the specific capacity of the positive electrode material. Therefore, it is necessary to control the mass content of supercrystalline structure phase based on the total mass of lithium-rich manganese-based positive electrode material within an appropriate range. In a preferred embodiment, the mass content of supercrystalline structure phase is 45% to 49%.
[0031] In the present invention, the lithium-rich manganese-based positive electrode material has a layered structure, which can be regarded as a doping layer formed by the lithium layer and the transition metal layer alternately stacked. The structural characteristics of these materials determine the performance of the lithium-rich manganese-based positive electrode material in terms of specific capacity and cycle stability under high voltage conditions. Therefore, in order to further improve the electrochemical performance of the lithium-rich manganese-based positive electrode material, in a specific embodiment, the splitting angle between the (006) crystal plane diffraction peak and the (102) crystal plane diffraction peak of the lithium-rich manganese-based positive electrode material is ≥0. 3°, exemplarily, the splitting angle between the (006) crystal plane diffraction peak and the (102) crystal plane diffraction peak of the lithium-rich manganese-based positive electrode material can be 0.3°, 0.4°, 0.5°, or 0.6°; the splitting angle between the (108) crystal plane diffraction peak and the (110) crystal plane diffraction peak of the lithium-rich manganese-based positive electrode material is ≥0.5°, exemplarily, the splitting angle between the (108) crystal plane diffraction peak and the (110) crystal plane diffraction peak of the lithium-rich manganese-based positive electrode material can be 0.5°, 0.6°, 0.7°, or 0.8°. It should be noted that the splitting angle between the (006) and (102) and (108) and (110) crystal plane diffraction peaks can reflect the quality of the layered structure of the lithium-rich manganese-based positive electrode material. Therefore, by controlling the splitting angle between the (006) and (102) and (108) and (110) crystal plane diffraction peaks to be greater than a specific value and having a certain degree of splitting, a more regular layered structure can be obtained, and the degree of cation mixing will also be relatively low, thereby further improving the electrochemical performance of the positive electrode material. In a preferred embodiment, the splitting angle between the (006) crystal plane diffraction peak and the (102) crystal plane diffraction peak of the lithium-rich manganese-based positive electrode material is 0.4° to 0.6°; the splitting angle between the (108) crystal plane diffraction peak and the (110) crystal plane diffraction peak of the lithium-rich manganese-based positive electrode material is 0.6° to 0.8°.
[0032] Furthermore, in the present invention, the (003) crystal plane diffraction peak intensity I of the lithium-rich manganese-based positive electrode material is (003) The diffraction peak intensity of (104) crystal plane is (104) The ratio I (003) / I (104) ≥1.8. Exemplary, I (003) / I (104) The value of can be 1.8, 1.9, 2, 2.1, 2.2, 2.3, etc. The (003) crystal plane diffraction peak reflects the hexagonal structure, while the (104) crystal plane diffraction peak reflects the sum of the hexagonal structure and the cubic structure. (003) / I (104) The larger the ratio is, the higher the degree of hexagonal unit cell ordering of the material is. (003) / I (104) When ≥1.8, the closer it is to the ideal hexagonal structure, the more complete the crystal structure is, and the lower the degree of cation mixing is.(003) / I (104) When the ratio of is within a suitable range, the migration of transition metal ions can be effectively hindered, and the degree of cation mixing can be reduced, thereby further improving the electrochemical performance of lithium-rich manganese-based positive electrode materials. In a preferred embodiment, I (003) / I (104) =1.8~2.3.
[0033] In a specific embodiment, based on the molar amount of the total metal elements of the lithium-rich manganese-based positive electrode material, the molar content of the lithium element in the lithium-rich manganese-based positive electrode material is 52.7% mol to 59.6% mol. Exemplarily, the molar content of the lithium element in the lithium-rich manganese-based positive electrode material can be 52.7% mol, 52.8% mol, 52.9% mol, 53% mol, 53.5% mol, 54% mol, 54.5% mol, 55% mol, 55.5% mol, 56% mol, 56.5% mol, 57% mol, 57.5% mol, 58% mol, 58.5% mol, 59% mol, 59.1% mol, 59.2% mol, 59.3% mol, 59.4% mol, 59.5% mol, 59.6% mol. In lithium-rich manganese-based positive electrode materials, too much lithium in the lattice will lead to poor kinetics, thereby causing the specific capacity and rate performance of the positive electrode material to decrease, while too little lithium will directly lead to a decrease in the reversible specific capacity of the positive electrode material. Therefore, the specific capacity and cycle stability of the positive electrode material can be improved by further adjusting the molar content of lithium in the lithium-rich manganese-based positive electrode material. In a preferred embodiment, the molar content of lithium in the lithium-rich manganese-based positive electrode material is 57% mol to 59% mol.
[0034] In a specific embodiment, based on the molar amount of the total metal elements of the lithium-rich manganese-based positive electrode material, the molar content of the M element in the lithium-rich manganese-based positive electrode material is 0.4% mol to 1.8% mol. Exemplarily, the molar content of the M element in the lithium-rich manganese-based positive electrode material can be 0.4% mol, 0.5% mol, 0.6% mol, 0.7% mol, 0.8% mol, 0.9% mol, 1% mol, 1.1% mol, 1.2% mol, 1.3% mol, 1.4% mol, 1.5% mol, 1.6% mol, 1.7% mol, 1.8% mol. Doping an appropriate amount of sodium ions or potassium ions into the lithium layer can effectively improve the cation mixing, and at the same time play the role of a pillar, which is conducive to the rapid diffusion of lithium ions, stable structure, etc., but too little sodium ions or potassium ions doping has a very weak effect, which does not achieve a significant increase in effect, not only increasing the cost, but also adding additional processes; and excessive sodium ions or potassium ions doping will not only seriously hinder the diffusion of lithium ions, but also lead to a reduction in the sites of lithium ions, thereby affecting the specific capacity of the positive electrode material. Therefore, the specific capacity and cycle stability of the positive electrode material can be improved by further adjusting the molar content of the M element in the lithium-rich manganese-based positive electrode material. In a preferred embodiment, the molar content of the M element in the lithium-rich manganese-based positive electrode material is 0.8% mol to 1.2% mol.
[0035] In a specific embodiment, based on the molar amount of the total metal elements of the lithium-rich manganese-based positive electrode material, the molar content of the transition metal element in the lithium-rich manganese-based positive electrode material is 40% mol to 45.5% mol. Exemplarily, the molar content of the transition metal element in the lithium-rich manganese-based positive electrode material can be 40% mol, 40.1% mol, 40.2% mol, 40.3% mol, 40.4% mol, 40.5% mol, 40.6% mol, 40.7% mol, 40.8% mol, 40.9% mol, 41% mol, 41.5% mol, 42% mol, 42.5% mol, 43% mol, 43.5% mol, 44% mol, 44.5% mol, 45% mol, 45.5% mol. The redox reaction of transition metal elements during the charge and discharge process helps to maintain the electrochemical performance of the battery. Insufficient content will lead to performance degradation. Therefore, the molar content of transition metal elements in lithium-rich manganese-based positive electrode materials should not be too low. At the same time, the molar content of transition metal elements in lithium-rich manganese-based positive electrode materials should not be too high. Excessive transition metal elements may migrate to lithium vacancies during the cycle, resulting in the transformation of the layered structure to the spinel phase structure, thereby reducing the average discharge voltage of the battery and affecting various aspects of the performance of lithium-rich manganese-based positive electrode materials. Therefore, the electrochemical performance of the positive electrode material can be improved by further adjusting the molar content of transition metal elements in the lithium-rich manganese-based positive electrode material, and the specific capacity, structural stability and long cycle performance of the positive electrode material can be further improved. In a preferred embodiment, the molar content of the transition metal element in the lithium-rich manganese-based positive electrode material is 40% mol to 42.2% mol.
[0036] In a specific embodiment, based on the molar amount of the total metal elements of the lithium-rich manganese-based positive electrode material, the ratio of the total molar content of the lithium element and the M element in the lithium-rich manganese-based positive electrode material to the molar content of the transition metal element is 1.2 to 1.5. Exemplarily, the ratio of the total molar content of the lithium element and the M element in the lithium-rich manganese-based positive electrode material to the molar content of the transition metal element can be 1.2, 1.25, 1.3, 1.35, 1.4, 1.45, 1.5. Excess lithium ions are a prerequisite for high specific capacity, especially the increase in lithium content in the transition metal layer will significantly increase the capacity of the material at high voltage. Therefore, the content relationship between the lithium element and the lithium layer doping element M and the transition metal element can be adjusted by further controlling the ratio of the total molar content of the lithium element and the M element to the molar content of the transition metal element to further improve the specific capacity of the positive electrode material. In a preferred embodiment, the ratio of the total molar content of the lithium element and the M element to the molar content of the transition metal element in the lithium-rich manganese-based positive electrode material is 1.4 to 1.5.
[0037] In the present invention, the lithium layer contains the M element, and an appropriate amount of M element ions will be inserted into the lithium layer, which can play the role of a "pillar" to inhibit the collapse of the layered structure during deep delithiation (high voltage), and well maintain the structural stability of the positive electrode material. In addition, due to the characteristics of the M element, the mixing and phase transition of lithium ions / nickel ions can be weakened, thereby avoiding the lithium-nickel mixing phenomenon caused by transition metal reduction. Based on the above analysis, it can be seen that it is very important to control the content of the M element contained in the lithium layer.
[0038] In a specific embodiment, when the M element includes the sodium element and the potassium element, the molar content of the M element is 1% mol to 4% mol based on the molar amount of the total metal elements of the lithium layer. Exemplarily, the molar content of the sodium element can be 1% mol, 1.5% mol, 2% mol, 2.5% mol, 3% mol, 3.5% mol, or 4% mol.
[0039] In a specific embodiment, when the M element includes only the sodium element, the molar content of the sodium element is 2% mol to 4% mol. Exemplarily, the molar content of the sodium element may be 2% mol, 2.5% mol, 3% mol, 3.5% mol, or 4% mol.
[0040] In a specific embodiment, when the M element includes only the potassium element, the molar content of the potassium element is 1% mol to 3% mol. Exemplarily, the molar content of the potassium element can be 1% mol, 1.5% mol, 2% mol, 2.5% mol, or 3% mol.
[0041] Sodium and potassium ions can be inserted into the lithium layer. Due to their larger ionic radius, they can increase the interlayer spacing of the lithium doping layer of the lithium-rich manganese-based positive electrode material. In addition, the huge electron cloud formed by the more extranuclear electrons of sodium and potassium ions can effectively inhibit the migration of transition metals through electrostatic repulsion and magnetic interaction, thereby weakening the Li + / Ni 2 + Mixing and phase transformation can improve the cycle stability of lithium-rich manganese-based positive electrode materials; the present invention can further improve the structural properties of lithium-rich manganese-based positive electrode materials by adjusting the molar content of the M element in the lithium layer under different conditions, thereby improving its cycle stability under high voltage conditions and extending the cycle life of the positive electrode material.
[0042] In a specific embodiment, the lithium-rich manganese-based positive electrode material is a secondary particle formed by a primary particle, and the particle size of the primary particle is 300-500nm. Exemplarily, the particle size of the primary particle is 300nm, 310nm, 320nm, 330nm, 340nm, 350nm, 360nm, 370nm, 380nm, 390nm, 400nm, 410nm, 420nm, 430nm, 440nm, 450nm, 460nm, 470nm, 480nm, 490nm, 500nm, and the particle size of the secondary particle is 5μm to 15μm. Exemplarily, the particle size of the secondary particle can be 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm. The lithium-rich manganese-based positive electrode material of the present invention is a secondary particle composed of primary particles. Compared with single crystal large particles, the secondary particles composed of primary particles are more convenient for uniformly doping heterogeneous elements into the lattice during the element doping process, thereby increasing the amount of lithium elements entering the transition metal layer and reducing the amount of residual alkali on the surface of the lithium-rich manganese-based positive electrode material, thereby further increasing the specific capacity released by the positive electrode material under high voltage and improving the electrochemical performance of the lithium-rich manganese-based positive electrode material.
[0043] In a specific embodiment, the BET of the lithium-rich manganese-based positive electrode material is 1m 2 / g~3m 2 / g, for example, the BET of the lithium-rich manganese-based positive electrode material can be 1m 2 / g, 1.1m 2 / g, 1.2m 2 / g, 1.3m 2 / g, 1.4m 2 / g, 1.5m 2 / g, 1.6m 2 / g, 1.7m 2 / g, 1.8m 2 / g, 1.9m 2 / g, 2m 2 / g, 2.1m 2 / g, 2.2m 2 / g, 2.3m 2 / g, 2.4m 2 / g, 2.5m 2 / g, 2.6m 2 / g, 2.7m 2 / g, 2.8m 2 / g, 2.9m 2 / g, 3m 2 / g; the compaction density of the lithium-rich manganese-based positive electrode material is between 2.6cc / g and 2.9cc / g. For example, the compaction density of the lithium-rich manganese-based positive electrode material can be 2.6cc / g, 2.7cc / g, 2.8cc / g, and 2.9cc / g. A larger specific surface area BET helps to improve the contact between the positive electrode material and the electrolyte, thereby promoting the transmission of lithium ions and electron transfer. This improvement is particularly reflected in the charge and discharge efficiency and high-rate charge and discharge performance of the battery. The present invention can further improve its electrochemical activity and cycle stability by controlling the specific surface area BET of the lithium-rich manganese-based positive electrode material within a suitable range.
[0044] Moreover, there is a certain correlation between the specific surface area BET and the compaction density of the positive electrode material. Generally, the smaller the BET, the lower the porosity, and the higher the compaction density. In addition, the compaction density of the lithium-rich manganese-based positive electrode material directly determines the volume energy density. Therefore, the influence of the compaction density on the electrochemical performance cannot be ignored. In addition, the porosity, BET and primary particle size of the lithium-rich manganese-based positive electrode material intuitively determine the compaction density of the material and the permeability of the electrolyte. Therefore, by simultaneously controlling the porosity, BET and primary particle size of the lithium-rich manganese-based positive electrode material, the compaction density of the material and the contact between the electrode particles can be effectively increased, thereby improving the electronic conductivity and lithium ion transfer rate, and further improving the reversible specific capacity, volume specific energy and rate performance of the lithium-rich manganese-based positive electrode material.
[0045] The second aspect of the present invention provides a method for preparing the lithium-rich manganese-based positive electrode material according to the first aspect of the present invention, comprising:
[0046] (1) uniformly mixing powders of a lithium-rich manganese-based precursor, lithium bromide and M salt;
[0047] (2) performing a first sintering of the material obtained in step (1) under an inert atmosphere, and then heating the material for a second sintering;
[0048] (3) The material obtained in step (2) is subjected to a third sintering in an air atmosphere to obtain the lithium-rich manganese-based positive electrode material.
[0049] In the present invention, lithium bromide can be decomposed to produce bromine gas during the calcination process. Since bromine gas is reducing, the transition metal in the transition metal layer will undergo a reduction reaction to generate a low-valent state under the action of bromine gas. In order to balance the charge, the excess lithium ions added in the sintering stage will smoothly migrate into the transition metal layer, so that the lithium content in the transition metal layer increases, thereby effectively improving its specific capacity under high voltage; moreover, under the action of bromine gas, the residual alkali on the surface of the positive electrode material can be reduced by reducing the activation energy of lithium ions entering the transition metal layer, thereby avoiding the accumulation of excess lithium ions on the surface of the positive electrode material, thereby improving the electrochemical performance of the lithium-rich manganese-based positive electrode material.
[0050] In a specific embodiment, the M salt includes a sodium salt and / or a potassium salt, the sodium salt includes at least one of sodium carbonate, sodium hydroxide, sodium acetate, sodium oxalate, sodium nitrate and sodium sulfate, and the potassium salt includes at least one of potassium carbonate, potassium hydroxide, potassium acetate, potassium oxalate, potassium nitrate and potassium sulfate. In a preferred embodiment, the sodium salt includes sodium carbonate, and the potassium salt includes potassium carbonate.
[0051] In one embodiment, the lithium-rich manganese-based precursor includes Ni x Co y Mn 1-x-y CO3, where 0≤x≤1 (for example: 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1), 0≤y≤1 (for example: 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1).
[0052] In a specific embodiment, the average particle size Dv50 of the lithium-rich manganese-based precursor is 5μm to 15μm. Exemplarily, the average particle size Dv50 of the lithium-rich manganese-based precursor can be 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm. Smaller precursor particle size helps to improve the electrochemical performance of the material. The positive electrode material formed by the precursor with a small particle size after high-temperature sintering has a smaller particle size, which is conducive to the diffusion of lithium ions and electron transfer. However, too small a particle size will cause the compaction density of the positive electrode material to be too small, thereby affecting the processing performance of the lithium-rich manganese-based positive electrode material; if the particle size of the lithium-rich manganese-based precursor is too large, it will also be easy to crush when preparing the pole piece, affecting the reversible specific capacity of the positive electrode material. Therefore, the present invention can further improve the electrochemical performance and cycle stability of the positive electrode material by controlling the average particle size Dv50 of the lithium-rich manganese-based precursor to 5μm to 15μm. In a preferred embodiment, the average particle size Dv50 of the lithium-rich manganese-based precursor is 7 μm to 10 μm.
[0053] In one embodiment, the BET value of the lithium-rich manganese-based precursor is 40 m 2 / g~100m 2 / g. Exemplarily, the BET value of the lithium-rich manganese-based precursor may be 40 m 2 / g, 50m 2 / g, 60m 2 / g, 70m 2 / g, 80m 2 / g, 90m 2 / g、100m 2 / g. The precursor has a larger BET value, which can increase the contact area with the lithium salt during mixing, making the two mixed more uniformly, and facilitating the obtaining of a positive electrode material with good consistency during the subsequent calcination process. In a preferred embodiment, the BET value of the lithium-rich manganese-based precursor is 70m 2 / g~90m 2 / g.
[0054] In a specific embodiment, the ratio of the total molar amount of the lithium bromide and the M salt to the molar amount of the lithium-rich manganese-based precursor is 1.2 to 1.6. For example, the ratio can be 1.2, 1.3, 1.4, 1.5, 1.6. When the above ratio is less than 1.2, it means that the total molar amount of lithium bromide and M salt added is too small, and the molar amount of the lithium-rich manganese-based precursor is too large, which will lead to the formation of lithium-deficient phase of the positive electrode material, seriously affecting the specific capacity of the prepared lithium-rich manganese-based positive electrode material; when the above ratio is greater than 1.6, it means that the total molar amount of lithium bromide and M salt added is too large, and the molar amount of the lithium-rich manganese-based precursor is too small, then in the process of generating the lithium-rich manganese-based positive electrode material, it is easy to cause lithium accumulation on the surface of the material and increase the amount of residual alkali, affecting the electrochemical properties of the positive electrode material; therefore, on the basis of the above-mentioned preparation method of the lithium-rich manganese-based positive electrode material, by further controlling the molar ratio between the reaction components within a suitable range, the influence of the preparation process on the specific capacity and electrochemical properties of the lithium-rich manganese-based positive electrode material can be avoided.
[0055] In a specific embodiment, the ratio of the molar amount of lithium bromide to the molar amount of the M salt is [(1.2-1.5)-a] / a, wherein 0.005≤a≤0.3. Doping an appropriate amount of sodium ions or potassium ions into the lithium layer can effectively improve the cation mixing, and at the same time play the role of a pillar, which is conducive to the rapid diffusion of lithium ions and stable structure, etc. However, the effect of too little sodium ions or potassium ions is very weak and cannot achieve a significant increase in effect, which not only increases the cost, but also adds additional processes; while the doping of excessive sodium ions or potassium ions will not only seriously hinder the diffusion of lithium ions, but also reduce the sites of lithium ions, resulting in a decrease in the specific capacity of the positive electrode material.
[0056] In one embodiment, the inert atmosphere comprises nitrogen and / or argon.
[0057] In a specific embodiment, the heating rate of the first sintering is 0.5°C / min to 10°C / min, the sintering temperature of the first sintering is 400°C to 600°C, and the sintering time of the first sintering is 1h to 8h.
[0058] In a specific embodiment, the heating rate of the second sintering is 0.5°C / min to 10°C / min, the sintering temperature of the second sintering is 700°C to 1000°C, and the sintering time of the second sintering is 5h to 10h.
[0059] In a specific implementation manner, the sintering temperature of the third sintering is 700° C. to 1000° C., and the sintering time of the third sintering is 10 h to 25 h.
[0060] It should be noted that, first, at low temperature and under the protection of inert gas, the mixture of lithium salt and precursor is pre-fired, i.e., the first sintering, so that the lithium salt lithium bromide is slowly melted, and under the protection of inert gas, the lithium bromide is heated and decomposed into bromine gas to reduce part of the transition metal. Then, after heating to 700-1000°C, the lithium salt lithium bromide is further melted and decomposed, and the lithium ions are further diffused into the precursor. Then, in an air atmosphere, the lithium ions and the transition metal form a layered structure, and due to the reduction of bromine gas in the early stage, part of the transition metal still maintains a low valence state. At this time, in order to balance the charge, the excess lithium ions added will smoothly migrate into the transition metal layer, so that the lithium content in the transition metal layer increases, thereby effectively improving its specific capacity under high voltage.
[0061] The third aspect of the present invention provides a battery, the battery comprising a positive electrode, the positive electrode comprising the lithium-rich manganese-based positive electrode material described in the first aspect of the present invention or the lithium-rich manganese-based positive electrode material prepared by the preparation method of the lithium-rich manganese-based positive electrode material described in the second aspect of the present invention.
[0062] The battery of the present invention also includes a negative electrode, a separator and an electrolyte, wherein the separator can be a separator conventionally used in the art, such as a PP film, a PE film, etc., and the negative electrode and the electrolyte can also be prepared by conventional methods in the art or obtained through commercial channels, which will not be repeated here.
[0063] In the present invention, the preparation method of the battery is: stack the prepared positive electrode plate, separator, and negative electrode plate in order, ensure that the separator is between the positive and negative electrode plates to play an isolating role, and then obtain a bare battery cell without liquid injection by winding; place the bare battery cell in an outer packaging foil, inject the prepared electrolyte into the dried bare battery cell, and obtain the desired battery through vacuum packaging, standing, formation, shaping, sorting and other processes.
[0064] In order to better illustrate the content of the invention, the invention is further verified by specific examples below. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the invention, rather than limiting the claims of the invention.
[0065] Example 1
[0066] This embodiment provides a method for preparing a lithium-rich manganese-based positive electrode material, which is used to prepare a lithium-rich manganese-based positive electrode material. The preparation method comprises the following steps:
[0067] (1) Lithium-rich manganese-based carbonate precursor (Ni 0.25 Co 0.125 Mn 0.625 CO3, average particle size Dv50 is 8μm, BET value is 70m 2 / g), lithium bromide powder and Na2CO3 powder are weighed according to the molar ratio of 1:1.5345:0.0155 (calculation shows that the ratio of the total molar amount of lithium bromide and sodium salt Na2CO3 added to the molar amount of the lithium-rich manganese-based precursor is 1.55, and the molar ratio of lithium bromide and sodium salt Na2CO3 is 99:1), and are fully mixed with the help of a mixer to obtain a mixture.
[0068] (2) The mixture obtained in (1) is placed in a box-type atmosphere furnace, first heated to 500° C. at a heating rate of 2° C. / min in an inert atmosphere, and kept at this temperature for 5 h; then heated to 900° C. at a heating rate of 2° C. / min in an inert atmosphere, kept at this temperature for 2 h, and then sintered at 900° C. in an air atmosphere for 12 h to obtain a lithium-rich manganese-based positive electrode material having a lithium layer doped with 3% mol Na, with a chemical formula of Li 1.168. Na 0.024 Ni 0.2 Co 0.1 Mn 0.5 O2.
[0069] The lithium-rich manganese-based positive electrode material obtained in Example 1 was analyzed using a scanning electron microscope to obtain a scanning electron microscope image thereof, as shown in FIG. Figure 1 As shown. Figure 1 It can be seen that the morphology and structure of the lithium-rich manganese-based positive electrode material prepared in the embodiment of the present invention is secondary particles formed by primary particles, wherein the grain size of the primary particles is 400 nm, and the particle size of the secondary particles is 7.5 μm.
[0070] The cross-sectional morphology scanning electron microscope image of a single lithium-rich manganese-based material spherical particle and the element distribution surface scan, such as Figure 2 As shown in the figure, it can be seen that the sodium element in the material is evenly distributed in the bulk phase, and it can be analyzed that the molar content of lithium element in the lithium-rich manganese-based positive electrode material is 58.65% mol, the molar content of sodium element is 1.2% mol, and the molar content of transition metal elements is 40.15% mol.
[0071] The XRD pattern of sodium-doped lithium-rich manganese-based cathode material is shown in Figure 3It can be found that a superlattice diffraction peak appears around 21°, corresponding to the generation of Li@Mn6 superstructure units in the transition metal layer. This shows that the material is mainly composed of layered hexagonal LiMO2 (R-3m space group) structure and monoclinic Li2MnO3 (C2 / m space group) structure, and there is a clear split between the (006) / (102) and (108) / (110) peaks. The splitting angle between the (006) crystal plane diffraction peak and the (102) crystal plane diffraction peak is 0.57, and the splitting angle between the (108) crystal plane diffraction peak and the (110) crystal plane diffraction peak is 0.77, which indicates that the material has a very good layered structure. At the same time, Figure 3 Middle I (003) / I (104) The ratio of represents the degree of cation mixing. It can be seen from the calculation that the I(003) / I (104) The ratio is 2.208.
[0072] According to the Rietveld refinement results of XRD, the proportion of supercrystalline structure phase Li2MnO3 in the lithium-rich manganese-based positive electrode material is 49.70%, and the lithium-nickel mixed ratio is 4.54%;
[0073] In addition, the BET value of the prepared lithium-rich manganese-based cathode material was measured by a fully automatic specific surface analyzer to be 2.037 m 2 / g; the compaction density of the prepared lithium-rich manganese-based positive electrode material was measured by a 300KN material compaction tester to be 2.85cc / g. The specific test and analysis results can be found in Tables 1 and 2.
[0074] Example 2
[0075] The preparation method of the lithium-rich manganese-based positive electrode material of this embodiment is basically the same as that of Example 1, except that: in step (1), the lithium-rich manganese-based positive electrode material carbonate precursor, lithium bromide powder and Na2CO3 powder are weighed according to a molar ratio of 1:1.5395:0.0105, and are fully mixed with the aid of a mixer to obtain a mixture; then, high-temperature sintering is performed according to the calcination process in Example 1 to obtain a lithium-rich manganese-based positive electrode material having a lithium layer doped with 2% mol Na. Other test and analysis results are shown in Tables 1 and 2.
[0076] Example 3
[0077] The preparation method of the lithium-rich manganese-based positive electrode material of this embodiment is basically the same as that of Example 1, except that: in step (1), the lithium-rich manganese-based positive electrode material carbonate precursor, lithium bromide powder and Na2CO3 powder are weighed according to a molar ratio of 1:1.5295:0.0205, and are fully mixed with the aid of a mixer to obtain a mixture; then, high-temperature sintering is performed according to the calcination process in Example 1 to obtain a lithium-rich manganese-based positive electrode material having a lithium layer doped with 4% mol Na. Other test and analysis results are shown in Tables 1 and 2.
[0078] Example 4
[0079] The preparation method of the lithium-rich manganese-based positive electrode material of this embodiment is basically the same as that of Example 1, except that: in step (1), the lithium-rich manganese-based positive electrode material carbonate precursor, lithium bromide powder and Na2CO3 powder are weighed according to a molar ratio of 1:1.5445:0.0055, and are fully mixed with the aid of a mixer to obtain a mixture; then, high-temperature sintering is performed according to the calcination process in Example 1 to obtain a lithium-rich manganese-based positive electrode material having a lithium layer doped with 1% mol Na. Other test and analysis results are shown in Tables 1 and 2.
[0080] Example 5
[0081] The preparation method of the lithium-rich manganese-based positive electrode material of this embodiment is basically the same as that of Example 1, except that: in step (1), the lithium-rich manganese-based positive electrode material carbonate precursor, lithium bromide powder and Na2CO3 powder are weighed according to a molar ratio of 1:1.5245:0.0255, and are fully mixed with the help of a mixer to obtain a mixture; then, high-temperature sintering is performed according to the calcination process in Example 1 to obtain a lithium-rich manganese-based positive electrode material having a lithium layer doped with 5% mol Na. Other test and analysis results are shown in Tables 1 and 2.
[0082] Example 6
[0083] The preparation method of the lithium-rich manganese-based positive electrode material of this embodiment is basically the same as that of Example 1, except that: in step (1), the lithium-rich manganese-based positive electrode material carbonate precursor, lithium bromide powder and K2CO3 powder are weighed according to a molar ratio of 1:1.5445:0.0055, and are fully mixed with the help of a mixer to obtain a mixture; then, high-temperature sintering is performed according to the calcination process in Example 1 to obtain a lithium-rich manganese-based positive electrode material with a lithium layer doped with 1% mol K. Other test and analysis results are shown in Table 1.
[0084] Example 7
[0085] The preparation method of the lithium-rich manganese-based positive electrode material of this embodiment is basically the same as that of Example 1, except that: in step (1), the lithium-rich manganese-based positive electrode material carbonate precursor, lithium bromide powder and K2CO3 powder are weighed according to a molar ratio of 1:1.5395:0.0105, and are fully mixed with the help of a mixer to obtain a mixture; then, high-temperature sintering is performed according to the calcination process in Example 1 to obtain a lithium-rich manganese-based positive electrode material having a lithium layer doped with 2% mol K. Other test and analysis results are shown in Tables 1 and 2.
[0086] Example 8
[0087] The preparation method of the lithium-rich manganese-based positive electrode material of this embodiment is basically the same as that of Example 1, except that: in step (1), the lithium-rich manganese-based positive electrode material carbonate precursor, lithium bromide powder and K2CO3 powder are weighed according to a molar ratio of 1:1.5345:0.0155, and are fully mixed with the help of a mixer to obtain a mixture; then, high-temperature sintering is performed according to the calcination process in Example 1 to obtain a lithium-rich manganese-based positive electrode material having a lithium layer doped with 3% mol K. Other test and analysis results are shown in Tables 1 and 2.
[0088] Example 9
[0089] The preparation method of the lithium-rich manganese-based positive electrode material of this embodiment is basically the same as that of Example 1, except that: in step (1), the lithium-rich manganese-based positive electrode material carbonate precursor, lithium bromide powder and K2CO3 powder are weighed according to a molar ratio of 1:1.549745:0.000255, and are fully mixed with the aid of a mixer to obtain a mixture; then, high-temperature sintering is performed according to the calcination process in Example 1 to obtain a lithium-rich manganese-based positive electrode material having a lithium layer doped with 0.5% mol K. Other test and analysis results are shown in Tables 1 and 2.
[0090] Example 10
[0091] The preparation method of the lithium-rich manganese-based positive electrode material of this embodiment is basically the same as that of Example 1, except that: in step (1), the lithium-rich manganese-based positive electrode material carbonate precursor, lithium bromide powder and K2CO3 powder are weighed according to a molar ratio of 1:1.5295:0.0205, and are fully mixed with the aid of a mixer to obtain a mixture; then, high-temperature sintering is performed according to the calcination process in Example 1 to obtain a lithium-rich manganese-based positive electrode material having a lithium layer doped with 4% mol K. Other test and analysis results are shown in Tables 1 and 2.
[0092] Embodiment 11
[0093] The preparation method of the lithium-rich manganese-based positive electrode material of this embodiment is basically the same as that of Example 1, except that: in step (2), the mixture obtained in (1) is placed in a box-type atmosphere furnace, first heated to 500°C at a heating rate of 2°C / min in an inert atmosphere, and kept warm for 5 hours; then heated to 900°C in an air atmosphere at a heating rate of 2°C / min, and sintered in an air atmosphere for 14 hours to obtain a lithium-rich manganese-based positive electrode material doped with a lithium layer.
[0094] Example 12
[0095] The preparation method of the lithium-rich manganese-based positive electrode material of this embodiment is basically the same as that of Example 1, except that: in step (2), the mixture obtained in (1) is placed in a box-type atmosphere furnace, first heated to 500°C at a heating rate of 2°C / min in an inert atmosphere, and kept warm for 5 hours; then heated to 900°C at a heating rate of 2°C / min in an inert atmosphere, kept warm for 7 hours, and then sintered at 900°C in an air atmosphere for 7 hours to obtain a lithium-rich manganese-based positive electrode material doped with a lithium layer.
[0096] Embodiment 13
[0097] The preparation method of the lithium-rich manganese-based positive electrode material in this embodiment is basically the same as that in Example 1, except that the average particle size Dv50 of the lithium-rich manganese-based carbonate precursor is 7 μm, and the BET value is 130 μm. 2 / g, other test and analysis results are shown in Tables 1 and 2.
[0098] Embodiment 14
[0099] The preparation method of the positive electrode active material of this embodiment is basically the same as that of embodiment 1, except that the average particle size Dv50 of the lithium-rich manganese-based carbonate precursor is 4 μm, and the BET value is 70 μm. 2 / g, other test and analysis results are shown in Tables 1 and 2.
[0100] Comparative Example 1
[0101] The preparation method of the lithium-rich manganese-based positive electrode material of this comparative example is basically the same as that of Example 1, except that: in step (1), the carbonate precursor of the lithium-rich manganese-based positive electrode material and the lithium carbonate powder are weighed according to a molar ratio of 1:0.77, and are fully mixed with the aid of a mixer to obtain a mixture; then, high-temperature sintering is performed according to the calcination process in Example 1 to obtain a lithium-rich manganese-based positive electrode material. Other test and analysis results are shown in Tables 1 and 2.
[0102] Comparative Example 2
[0103] The preparation method of the lithium-rich manganese-based positive electrode material of this comparative example is basically the same as that of Example 1, except that: in step (1), the carbonate precursor of the lithium-rich manganese-based positive electrode material and the lithium bromide powder are weighed according to a molar ratio of 1:1.55, and are fully mixed with the aid of a mixer to obtain a mixture; then, high-temperature sintering is performed according to the calcination process in Example 1 to obtain a lithium-rich manganese-based positive electrode material. Other test and analysis results are shown in Tables 1 and 2.
[0104] Comparative Example 3
[0105] The preparation method of the lithium-rich manganese-based positive electrode material of this comparative example is basically the same as that of Example 1, except that: in step (1), the carbonate precursor of the lithium-rich manganese-based positive electrode material, lithium carbonate powder and Na2CO3 powder are weighed according to a molar ratio of 1:0.76725:0.0155, and are fully mixed with the help of a mixer to obtain a mixture; then, high-temperature sintering is performed according to the calcination process in Example 1 to obtain a lithium-rich manganese-based positive electrode material having a lithium layer doped with 3% mol Na. Other test and analysis results are shown in Tables 1 and 2.
[0106] Comparative Example 4
[0107] The preparation method of the lithium-rich manganese-based positive electrode material of this comparative example is basically the same as that of Example 1, except that: in step (1), the carbonate precursor of the lithium-rich manganese-based positive electrode material, lithium hydroxide powder and Na2CO3 powder are weighed according to a molar ratio of 1:1.5345:0.0155, and are fully mixed with the help of a mixer to obtain a mixture; then, high-temperature sintering is performed according to the calcination process in Example 1 to obtain a lithium-rich manganese-based positive electrode material having a lithium layer doped with 3% mol Na. Other test and analysis results are shown in Tables 1 and 2.
[0108] Comparative Example 5
[0109] The preparation method of the lithium-rich manganese-based positive electrode material of this comparative example is basically the same as that of Example 1, except that: in step (2), the mixture obtained in (1) is placed in a box-type atmosphere furnace, first heated to 500°C in an air atmosphere at a heating rate of 2°C / min, and kept warm for 5 hours; then heated to 900°C in an air atmosphere at a heating rate of 2°C / min, and sintered in an air atmosphere for 14 hours to obtain a lithium-rich manganese-based positive electrode material having a lithium layer doped with 3% mol Na. Other test and analysis results are shown in Tables 1 and 2.
[0110] Table 1
[0111]
[0112]
[0113] Table 2
[0114]
[0115]
[0116] Test Case
[0117] The lithium-rich manganese-based positive electrode materials prepared in the examples and comparative examples were subjected to electrochemical lithium storage performance tests. The specific steps are as follows:
[0118] (1) Test for residual lithium and residual alkali content: The positive electrode materials in the obtained examples and comparative examples were tested for residual lithium Li2CO3 and residual lithium LiOH content, referring to the detection method for positive electrode materials of lithium-ion batteries in GB / T 41704: determination of magnetic foreign matter content and residual alkali content. A certain volume of water was used to dissolve the residual alkali on the surface of a certain mass of sample, and the filtrate was filtered and titrated with a standard hydrochloric acid titration solution. The titration end point was determined by the potential jump during the reaction process, and the content was calculated. The residual lithium Li2CO3 (%) content and residual lithium LiOH (%) content were obtained by conversion. The results are shown in Table 3.
[0119] (2) Battery performance test: The positive electrode materials obtained in the above-mentioned embodiments and comparative examples were mixed with the conductive agent and the binder PVDF in a ratio of 0.8:0.1:0.1, and an appropriate amount of NMP solvent was added and mixed, and the desired slurry was obtained by sufficient stirring, and then coated on Al foil and dried in a vacuum oven at 120° C. for 12 h to obtain a positive electrode sheet;
[0120] The obtained positive electrode sheet was rolled and punched into a 12mm disc, and assembled into a CR2032 button battery with a metal lithium sheet as the negative electrode in an argon-protected glove box. After each button battery was left to stand for 4 hours under normal conditions, the charge and discharge capacity was tested at a temperature of 25°C. The gram capacity test conditions were: 0.1C charging to 4.8V, constant voltage charging to 0.05C cut-off, standing for 5 minutes, and 0.1C discharge to 2.0V. The cycle test conditions were: 0.5C charging to 4.6V, constant voltage charging to 0.05C cut-off, standing for 5 minutes, and 0.5C discharge to 2.0V. The charge gram capacity, discharge gram capacity, first efficiency, and capacity retention rate after 100 cycles were recorded respectively, and the results are shown in Table 3.
[0121] (3)R wp (%) Calculation: R wp (%) is the weighted contour coefficient. According to the XRD patterns corresponding to the above embodiments and comparative examples, the Rietveld refinement results are recorded in Table 3.
[0122] Table 3
[0123]
[0124]
[0125] As can be seen from Table 3, the discharge specific capacity, first efficiency and capacity retention rate after 100 cycles of the lithium-rich manganese-based positive electrode material prepared by appropriate lithium layer doping (sodium ion or potassium ion doping) and lithium bromide as lithium salt and appropriate calcination process have been greatly improved. This further confirms that in the high-temperature solid-phase sintering stage, lithium bromide is used as a lithium salt, with appropriate calcination atmosphere and process steps, lithium bromide can be decomposed to produce bromine gas, reduce the transition metal in the transition metal layer, and promote the smooth entry of excess lithium ions into the transition metal layer, so that the transition metal layer is more lithium-rich. The positive electrode material, while also greatly reducing the large amount of residual alkali generated on the surface of the material. In addition, in order to further prevent the transition metal from causing serious cation mixing due to reduction, sodium ions or potassium ions are doped into the lithium layer. At the same time, the lithium layer doping effectively expands the interlayer spacing of the lithium layer in the lithium-rich manganese-based material, expands the channel for lithium ion migration, and improves the migration speed of lithium ions.
[0126] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A lithium-rich manganese-based positive electrode material, characterized in that: The general chemical formula of the lithium-rich manganese-based positive electrode material is Li 1+ n M m Ni x Co y Mn (1-x-y-n-m) O2, wherein 0≤n+m≤1, 0≤x≤1, 0≤y≤1, and the M element includes at least one of sodium and potassium; The lithium-rich manganese-based positive electrode material comprises a transition metal layer and a lithium layer, the transition metal layer comprises a supercrystalline structure phase with a lattice diffraction peak located at 20° to 25°, and the lithium layer comprises the M element; Based on the total mass of the lithium-rich manganese-based positive electrode material, the mass content of the supercrystalline structure phase is 30% to 50%.
2. The lithium-rich manganese-based positive electrode material according to claim 1, wherein: The lithium-rich manganese-based positive electrode material has a layered structure, the splitting angle between the (006) crystal plane diffraction peak and the (102) crystal plane diffraction peak of the lithium-rich manganese-based positive electrode material is ≥0.3°, and the splitting angle between the (108) crystal plane diffraction peak and the (110) crystal plane diffraction peak of the lithium-rich manganese-based positive electrode material is ≥0.5°; And / or, the (003) crystal plane diffraction peak intensity I of the lithium-rich manganese-based positive electrode material (003) The diffraction peak intensity of (104) crystal plane is (104) The ratio I (003) / I (104) ≥1.
8.
3. The lithium-rich manganese-based positive electrode material according to claim 1, wherein: Based on the molar amount of the total metal elements of the lithium-rich manganese-based positive electrode material, The molar content of lithium in the lithium-rich manganese-based positive electrode material is 52.7% mol to 59.6% mol; And / or, the molar content of the M element in the lithium-rich manganese-based positive electrode material is 0.4% mol to 1.8% mol; And / or, the molar content of transition metal elements in the lithium-rich manganese-based positive electrode material is 40% mol to 45.5% mol; And / or, the ratio of the total molar content of the lithium element and the M element to the molar content of the transition metal element in the lithium-rich manganese-based positive electrode material is 1.2 to 1.
5.
4. The lithium-rich manganese-based positive electrode material according to claim 1, wherein: When the M element includes the sodium element and the potassium element, the molar content of the M element is 1% mol to 4% mol based on the molar amount of the total metal elements in the lithium layer; And / or, when the M element includes only the sodium element, the molar content of the sodium element is 2% mol to 4% mol based on the molar amount of the total metal elements in the lithium layer; And / or, when the M element includes only the potassium element, the molar content of the potassium element is 1 mol% to 3 mol% based on the molar amount of the total metal elements in the lithium layer.
5. The lithium-rich manganese-based positive electrode material according to claim 1, wherein: The lithium-rich manganese-based positive electrode material is a secondary particle formed by a primary particle, the particle size of the primary particle is 300nm to 500nm, and the particle size of the secondary particle is 5μm to 15μm; And / or, the BET of the lithium-rich manganese-based positive electrode material is 1m 2 / g~3m 2 / g, and the compaction density of the lithium-rich manganese-based positive electrode material is between 2.6cc / g and 2.9cc / g.
6. A method for preparing the lithium-rich manganese-based positive electrode material according to any one of claims 1 to 5, characterized in that: include: (1) uniformly mixing powders of a lithium-rich manganese-based precursor, lithium bromide and M salt; (2) performing a first sintering of the material obtained in step (1) under an inert atmosphere, and then heating the material for a second sintering; (3) The material obtained in step (2) is subjected to a third sintering in an air atmosphere to obtain the lithium-rich manganese-based positive electrode material.
7. The method according to claim 6, wherein: The M salt includes sodium salt and / or potassium salt, the sodium salt includes at least one of sodium carbonate, sodium hydroxide, sodium acetate, sodium oxalate, sodium nitrate and sodium sulfate, and the potassium salt includes at least one of potassium carbonate, potassium hydroxide, potassium acetate, potassium oxalate, potassium nitrate and potassium sulfate; And / or, the lithium-rich manganese-based precursor includes Ni x Co y Mn 1-x-y CO3, where 0≤x≤1, 0≤y≤1; Preferably, the average particle size Dv50 of the lithium-rich manganese-based precursor is 5 μm to 15 μm; Preferably, the BET value of the lithium-rich manganese-based precursor is 40m 2 / g~100m 2 / g.
8. The method according to claim 6, wherein: The ratio of the total molar amount of the lithium bromide and the M salt to the molar amount of the lithium-rich manganese-based precursor is 1.2 to 1.6; And / or, the ratio of the molar amount of the lithium bromide to the molar amount of the M salt is [(1.2-1.6)-a] / a, wherein 0.005≤a≤0.
3.
9. The method according to claim 6, wherein: The inert atmosphere includes nitrogen and / or argon; and / or, the heating rate of the first sintering is 0.5°C / min to 10°C / min, the sintering temperature of the first sintering is 400°C to 600°C, and the sintering time of the first sintering is 1h to 8h; and / or, the heating rate of the second sintering is 0.5°C / min to 10°C / min, the sintering temperature of the second sintering is 700°C to 1000°C, and the sintering time of the second sintering is 5h to 10h; And / or, the sintering temperature of the third sintering is 700° C. to 1000° C., and the sintering time of the third sintering is 10 h to 25 h.
10. A battery, characterized in that: comprising a positive electrode, wherein The positive electrode comprises the lithium-rich manganese-based positive electrode material according to any one of claims 1 to 5 or the lithium-rich manganese-based positive electrode material prepared by the preparation method of the lithium-rich manganese-based positive electrode material according to any one of claims 6 to 9.