Zr, Mg and Mo doped lithium-rich manganese-based positive electrode material and preparation method thereof

Through the lithium-rich manganese-based positive electrode material doped with Zr, Mg, and Mo, the problem of capacity and voltage attenuation during the circulation of layered lithium-rich manganese-based materials is solved, high cycle stability and small voltage attenuation are achieved, and cobalt is reduced The use of elements has promoted the improvement of the electrochemical performance of the positive electrode materials of lithium-ion batteries.

CN119008930AActive Publication Date: 2024-11-22JILIN UNIVERSITY

Patent Information

Application Number
CN202411479090.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-23
Publication Date
2024-11-22
Estimated Expiration
2044-10-23

AI Technical Summary

Technical Problem

Layered lithium-rich manganese-based cathode materials have capacity and voltage attenuation due to uneven distribution of electrochemical activity during the cycle, and the high demand and toxicity of cobalt elements make their cost and environmental pollution a problem, and cobalt-free cathode materials need to be developed to improve the Stability and cost reduction.

Method used

The lithium-rich manganese-based positive electrode material doped with Zr, Mg, and Mo is used to form a spinel phase through solvent thermal reaction and high-temperature sintering, reconstruct the lattice oxygen oxidation behavior, shield the catalytic reaction of the electrode electrolyte interface, and improve the electrochemical performance.

Benefits of technology

High cycle stability and small voltage attenuation were achieved, the first Coulomb efficiency was no less than 85%, the capacity retention rate of 500 cycles was higher than 99% at a current density of 200mA/g, and the catalytic reaction at the electrode electrolyte interface was reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008930A_ABST
    Figure CN119008930A_ABST
Patent Text Reader

Abstract

The invention is suitable for the technical field of lithium ion battery positive electrode material modification, and provides a Zr, Mg and Mo doped lithium-rich manganese-based positive electrode material and a preparation method thereof. The morphology of the lithium-rich manganese-based positive electrode material is secondary particles formed by stacking primary particles, the size of the primary particles is 50-200 nm, and the size of the secondary particles is 8-12 [mu] m. The Zr, Mg and Mo doped lithium-rich manganese-based positive electrode material is synthesized by a simple and feasible method, is applied to the field of lithium ion batteries, and shows ultra-long cycle capacity stability, relatively small voltage attenuation and shielded electrode electrolyte interface catalytic reaction as the positive electrode material of the lithium ion batteries. The method has important significance for promoting the development of improving the electrochemical performance of the positive electrode material of the lithium ion battery by adopting a selective doping thought.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium ion battery positive electrode material modification, and in particular relates to a Zr, Mg, Mo doped lithium-rich manganese-based positive electrode material and a preparation method thereof. Background Art

[0002] In order to solve the environmental problems caused by fossil energy and achieve sustainable social development, the development of high-performance battery technology has become an urgent need. With the increasing demand for rechargeable lithium-ion batteries (LIBs) in electric vehicles, energy storage networks, electronic devices, etc., improving the energy density of LIBs, maintaining their cycle stability, improving their safety, and reducing their costs have become the main challenges of the industry. Layered lithium-rich manganese-based cathode materials (LMR) have high theoretical capacity (>250mAh / g) and high energy density (900Wh / kg) due to the joint participation of anions and cations in redox, but due to its two-phase composite structure, the electrochemical activity is severely unevenly distributed in the crystal, and LMR will experience severe capacity and voltage decay during the cycle, which will reduce its cycle life. Based on the current understanding of LMR, it is believed that the voltage decay is caused by the nanostrain between the composite two-phase crystal domains, which will lead to irreversible oxygen release, transition metal ion (TM) migration and structural rearrangement and other destructive effects, resulting in the high initial capacity of LMR cannot be maintained.

[0003] The stock of cobalt in the earth's crust is only 0.001% (mass ratio). The rapid increase in industry demand has caused its cost to continue to rise. In addition, cobalt is highly toxic and seriously pollutes the environment. This poses a major challenge to the industrial production of low-cost, environmentally friendly and sustainable batteries. Reducing the cobalt content of LIBs has become one of the ways to improve its safety and reduce costs. Therefore, developing cobalt-free positive electrode materials and compensating for their lack of stability due to the lack of cobalt through modification, thereby improving their performance has become one of the current goals of developing cobalt-free positive electrode materials. Element doping can effectively balance the electrochemical strain between the composite two phases, reconstruct the lattice oxygen oxidation behavior, shield the catalytic reaction at the electrode electrolyte interface, stabilize the evolution of the crystal structure of the LMR material during the cycle, and improve its electrochemical performance. For this purpose, a Zr, Mg, and Mo-doped lithium-rich manganese-based positive electrode material and a preparation method thereof are proposed. Summary of the invention

[0004] The object of the present invention is to provide a Zr, Mg, Mo doped lithium-rich manganese-based positive electrode material and a preparation method thereof, aiming to solve the problems raised in the above background technology.

[0005] To achieve the above object, the present invention provides the following technical solutions: A Zr, Mg, Mo doped lithium-rich manganese-based positive electrode material, the chemical formula of the lithium-rich manganese-based positive electrode material is Li 1.2 Ni0.2 Mn 0.6-x (Zr, Mg, Mo) x O 2 , x is between 0.004 and 0.012.

[0006] Furthermore, the morphology of the lithium-rich manganese-based positive electrode material is secondary particles formed by the accumulation of primary particles, the primary particle size is 50-200 nm, and the secondary particle size is 8-12 μm.

[0007] Furthermore, the lithium-rich manganese-based positive electrode material has an initial coulombic efficiency of no less than 85% at a current density of 20 mA / g, and a capacity retention rate of more than 99% after 500 cycles at a current density of 200 mA / g.

[0008] A method for preparing the Zr, Mg, and Mo-doped lithium-rich manganese-based positive electrode material according to the above-mentioned method comprises the following steps: Step S1, adding a commercial nickel-manganese precursor into anhydrous ethanol, ultrasonically dispersing, and then stirring at a constant temperature; Step S2, slowly adding a certain amount of Zr alcohol ester into the mixture while stirring, and placing the obtained system in air and stirring at a constant temperature for a certain period of time; Step S3: After stirring, transfer the system into a reactor and add a certain amount of magnesium salt powder and (NH 4 ) 6 Mo 7 O 24 ·4H 2 O, solvothermal reaction at 160-180°C, reaction time 8-12h; Step S4: The solvent thermal reaction product is filtered, washed and dried, and then mixed with Li 2 CO 3 and a certain amount of flux, mixed and ground, then calcined at a high temperature of 700-900°C, and naturally cooled to room temperature; Step S5: washing the calcined product with water and then drying it to finally obtain a Zr, Mg, and Mo-doped lithium-rich manganese-based positive electrode material.

[0009] Furthermore, in step S2, the amount of Zr alcohol ester used satisfies that the Zr atomic ratio is not higher than 1.5% of the product metal atoms.

[0010] Furthermore, in step S3, the amount of magnesium salt powder used satisfies that the Mg atomic ratio is not higher than 2% of the product metal atoms, (NH 4 ) 6 Mo 7 O 24 ·4H 2 The amount of O is such that the Mo atomic ratio is no more than 2% of the product metal atoms.

[0011] Furthermore, in step S4, Li 2 CO 3 The added amount is 5-10% more than the stoichiometric ratio, the added amount of the flux is 400% of the molar number of metal atoms of the target product, the flux includes KCl and NaCl, and the molar ratio of KCl to NaCl is 3:2.

[0012] Compared with the prior art, the present invention has the following beneficial effects: Compared with the existing doped lithium-rich manganese-based materials, the present invention uses a simple and feasible method to synthesize Zr, Mg, and Mo doped lithium-rich manganese-based positive electrode materials, which are applied in the field of lithium-ion batteries. As a positive electrode material for lithium-ion batteries, it exhibits ultra-long cycle capacity stability, small voltage decay, and shielded electrode electrolyte interface catalytic reaction. The present invention is of great significance to promoting the development of the selective doping idea to improve the electrochemical performance of lithium-ion battery positive electrode materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 XRD diagrams of the doped electrode materials obtained in Examples 1 to 4.

[0014] Figure 2 These are SEM images of the doped electrode materials obtained in Examples 1 to 4.

[0015] Figure 3 This is the first charge and discharge of the doped electrode materials obtained in Examples 1 to 4 under 0.1C (20 mA / g current density) conditions.

[0016] Figure 4 For Li 1.2 Ni 0.2 Mn 0.6 O 2 and Li 1.2 Ni 0.2 Mn 0.576 Zr 0.008 Mg 0.012 Mo 0.004 O 2 -B is a comparison of the cycling performance of the two samples at a current density of 200 mA / g.

[0017] Figure 5 For Li 1.2 Ni 0.2 Mn 0.6 O 2 and Li 1.2 Ni 0.2 Mn 0.576 Zr 0.008 Mg 0.012 Mo 0.004 O 2-B is a comparison of the rate performance of the two samples. DETAILED DESCRIPTION

[0018] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0019] The specific implementation of the present invention is described in detail below in conjunction with specific embodiments.

[0020] One embodiment of the present invention provides a Zr, Mg, Mo doped lithium-rich manganese-based positive electrode material, the chemical formula of the lithium-rich manganese-based positive electrode material is Li 1.2 Ni 0.2 Mn 0.6-x (Zr, Mg, Mo) x O 2 , x is between 0.004 and 0.012.

[0021] As a preferred embodiment of the present invention, the morphology of the lithium-rich manganese-based positive electrode material is secondary particles formed by the accumulation of primary particles, the primary particle size is 50-200 nm, and the secondary particle size is 8-12 μm.

[0022] As a preferred embodiment of the present invention, the lithium-rich manganese-based positive electrode material has an initial coulombic efficiency of not less than 85% at a current density of 20 mA / g, and a capacity retention rate of more than 99% after 500 cycles at a current density of 200 mA / g.

[0023] A method for preparing the Zr, Mg, and Mo-doped lithium-rich manganese-based positive electrode material according to the above-mentioned method comprises the following steps: Step S1, adding a commercial nickel-manganese precursor into anhydrous ethanol, ultrasonically dispersing, and then stirring at a constant temperature; Step S2, slowly adding a certain amount of Zr alcohol ester to the mixture while keeping stirring, and placing the resulting system in air and stirring at a constant temperature for a certain period of time; in the step S2, the amount of Zr alcohol ester is such that the Zr atomic ratio is not higher than 1.5% of the product metal atoms.

[0024] Step S3: After stirring, transfer the system into a reactor and add a certain amount of magnesium salt powder and (NH 4 ) 6 Mo 7 O 24 ·4H 2 O, and a solvent thermal reaction is carried out at 160-180° C. for 8-12 hours; in step S3, the amount of magnesium salt powder used satisfies that the Mg atomic ratio is not higher than 2% of the product metal atoms, (NH 4) 6 Mo 7 O 24 ·4H 2 The amount of O is such that the Mo atomic ratio is no more than 2% of the product metal atoms.

[0025] Step S4: The solvent thermal reaction product is filtered, washed and dried, and then mixed with Li 2 CO 3 and a certain amount of flux are mixed and ground, and then calcined at a high temperature of 700-900°C, and naturally cooled to room temperature; in step S4, Li 2 CO 3 The added amount is 5-10% more than the stoichiometric ratio, the added amount of the flux is 400% of the molar number of metal atoms of the target product, the flux includes KCl and NaCl, and the molar ratio of KCl to NaCl is 3:2.

[0026] Step S5: washing the calcined product with water and then drying it to finally obtain a Zr, Mg, and Mo-doped lithium-rich manganese-based positive electrode material.

[0027] In the embodiments of the present invention, the three doping elements Zr, Mg, and Mo have different doping selectivities in the two phases of the lithium-rich material, and their respective diffusion rates during high-temperature sintering are also different, thereby forming selective doping between the two phases and constructing a spinel phase on the particle surface. These structural designs reconstruct the anion oxidation capacity composition during the first charge process, weaken the catalytic reaction at the electrode electrolyte interface, and at the same time, through the in-situ diffusion of the spinel phase, reduce the structural degradation during the cycle, thereby achieving the stability of the long cycle of the layered lithium-rich manganese-based material.

[0028] Example 1: A lithium-rich manganese-based positive electrode material Li 1.2 Ni 0.2 Mn 0.6 O 2 The preparation method comprises the following steps: S1. Combine the commercial nickel-manganese precursor with Li 2 CO 3 , KCl, and NaCl are mixed and ground, among which Li 2 CO 3 5% molar excess, then calcined at 850°C for 12h, and cooled naturally to room temperature; S2. Wash, filter and dry the calcined product to obtain the target product.

[0029] Example 2: A lithium-rich manganese-based positive electrode material Li 1.2 Ni 0.2 Mn 0.588 Mg 0.01 Mo 0.002 O2 The preparation method comprises the following steps: S1. Add the commercial nickel-manganese precursor into the reactor, add 1% metal atomic ratio of magnesium salt powder and 1% metal atomic ratio of (NH 4 ) 6 Mo 7 O 24 ·4H 2 O, solvothermal reaction was carried out with ethanol as solvent for 12 h; S2, the solvent thermal reaction product was filtered, washed and dried, and then mixed with KCl, NaCl and 5% molar excess Li 2 CO 3 The mixture was mixed and ground, then calcined at 850 °C for 12 h and cooled naturally to room temperature.

[0030] S3, washing, filtering and drying the product obtained by calcination to obtain the target product.

[0031] Example 3: A lithium-rich manganese-based positive electrode material Li 1.2 Ni 0.2 Mn 0.576 Zr 0.008 Mg 0.012 Mo 0.004 O 2 -A preparation method, comprising the following steps: S1. Add the commercial nickel-manganese precursor into the reactor and add 1% metal atomic ratio of ZrO 2 , 1% metal atomic ratio MgCO 3 and 1.5% metal atomic ratio (NH 4 ) 6 Mo 7 O 24 ·4H 2 O, solvothermal reaction was carried out with ethanol as solvent for 12 h; S2, the solvent thermal reaction product was filtered, washed and dried, and then mixed with KCl, NaCl and 5% molar excess Li 2 CO 3 Mix and grind, then calcine at 850℃ for 12h, and cool naturally to room temperature; S3, washing, filtering and drying the product obtained by calcination to obtain the target product.

[0032] Example 4: A lithium-rich manganese-based positive electrode material Li 1.2 Ni 0.2 Mn 0.576 Zr 0.008 Mg 0.012 Mo 0.004 O 2 -B preparation method, comprising the following steps: S1. Add the commercial nickel-manganese precursor into anhydrous ethanol, disperse it by ultrasonic, and then stir it at a constant temperature of 60°C; S2, 1% metal atomic ratio of Zr (C 3 H 7 O) 4 Slowly add while stirring, and place the resulting system in air at 60°C with constant stirring for 5 h; S3. After the stirring is completed, the system is transferred into a reactor and 1% metal atomic ratio of MgCO is added. 3 and 1.5% metal atomic ratio (NH 4 ) 6 Mo 7 O 24 ·4H 2 O, solvothermal reaction for 12 h; S4, the solvent thermal reaction product was filtered, washed and dried, and then mixed with KCl, NaCl and 5% molar excess Li 2 CO 3 Mix and grind, then calcine at 850℃ for 12h, and cool naturally to room temperature; S5. Wash, filter and dry the calcined product to obtain the target product.

[0033] Embodiment 5: A method of using Li 1.2 Ni 0.2 Mn 0.576 Zr 0.008 Mg 0.012 Mo 0.004 O 2 -B A method for preparing a button cell from a lithium-rich manganese-based positive electrode material, comprising the following steps: Li 1.2 Ni 0.2 Mn 0.576 Zr 0.008 Mg 0.012 Mo 0.004 O 2 -B positive electrode material is mixed with 10% by mass of conductive carbon and binder, a certain amount of N-methylpyrrolidone solution is added, stirred evenly and coated on aluminum foil, and dried in a vacuum oven; then the electrode sheet is cut out with a slicer; then it is transferred to a glove box with argon atmosphere, and assembled into a button battery with lithium metal sheet as the counter electrode, glass fiber filter paper as the diaphragm, and a mixed solution of ethylene carbonate, ethyl methyl carbonate and dimethyl carbonate of lithium hexafluorophosphate as the electrolyte.

[0034] The Li 1.2 Ni 0.2 Mn 0.576 Zr 0.008 Mg 0.012 Mo0.004 O 2 -B The mass ratio of the positive electrode material to the binder and the Li 1. 2 Ni 0.2 Mn 0.576 Zr 0.008 Mg 0.012 Mo 0.004 O 2 -B The mass ratio of positive electrode material to conductive agent is 8:1.

[0035] The binder is polyvinylidene fluoride, and the conductive agent is acetylene black.

[0036] Figure 1 The XRD patterns of the doped electrode materials obtained in Examples 1 to 4 are shown below. Figure 1 It can be seen that the XRD of the doped electrode materials prepared in Examples 1 to 4 all show characteristic peaks of the lithium-rich material structure, and the doping of Zr, Mg and Mo does not change the crystal structure of the material.

[0037] Figure 2 The following are SEM images of the doped electrode materials obtained in Examples 1 to 4. Figure 2 It can be seen that the doped electrode materials prepared in Examples 1 to 4 are all composed of secondary particle balls of 8 to 10 μm, and the doping of Zr, Mg, and Mo elements does not change the microscopic morphology of the materials.

[0038] Figure 3 The first charge and discharge of the doped electrode materials prepared in Examples 1 to 4 under 0.1C (20 mA / g current density) conditions. Figure 3 It can be seen that, firstly, Zr, Mg, and Mo doping changed the shape of the high voltage (>4.5V) charging curve and reconstructed the oxidation behavior of lattice oxygen. Secondly, Mg and Mo doping reduced the first discharge capacity of the electrode material. After the introduction of Zr, the attenuation of the first capacity can be effectively suppressed. The co-doping of Zr, Mg, and Mo elements improved the coulombic efficiency of the first cycle, while Li 1.2 Ni 0.2 Mn 0.576 Zr 0.008 Mg 0.012 Mo 0.004 O 2 -B's first coulombic efficiency can reach up to 95.7%.

[0039] Figure 4 For Li 1.2 Ni 0.2 Mn 0.6 O 2 and Li 1.2 Ni 0.2 Mn 0.576 Zr 0.008Mg 0.012 Mo 0.004 O 2 -B Comparison of the cycling performance of the two samples at a current density of 200 mA / g. Figure 4 It can be seen that Li co-doped with Zr, Mg, and Mo 1.2 Ni 0.2 Mn 0.576 Zr 0.008 Mg 0.012 Mo 0.004 O 2 -B achieves the stability of lithium-rich materials in extremely long cycles, and the capacity remains 100% after 500 cycles.

[0040] Figure 5 For Li 1.2 Ni 0.2 Mn 0.6 O 2 and Li 1.2 Ni 0.2 Mn 0.576 Zr 0.008 Mg 0.012 Mo 0.004 O 2 -B Comparison of the rate performance of the two samples. Figure 5 It can be seen that the co-doping of Zr, Mg and Mo elements achieves the improvement of the rate performance of lithium-rich materials, and the initial capacity can still be fully restored after recovering to a small rate.

[0041] The above are only preferred embodiments of the present invention. It should be pointed out that, for those skilled in the art, several modifications and improvements can be made without departing from the concept of the present invention. These should also be regarded as the protection scope of the present invention. These will not affect the effect of the implementation of the present invention and the practicality of the patent.

Claims

1. A Zr, Mg, Mo doped lithium-rich manganese-based positive electrode material, characterized in that: The chemical formula of the lithium-rich manganese-based positive electrode material is Li 1.2 Ni 0.2 Mn 0.6-x (Zr, Mg, Mo) x O2, x is between 0.004 and 0.

012.

2. The Zr, Mg, Mo-doped lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: The morphology of the lithium-rich manganese-based positive electrode material is secondary particles formed by the accumulation of primary particles, the size of the primary particles is 50-200 nm, and the size of the secondary particles is 8-12 μm.

3. The Zr, Mg, Mo-doped lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: The lithium-rich manganese-based positive electrode material has an initial coulombic efficiency of no less than 85% at a current density of 20 mA / g, and a capacity retention rate of more than 99% after 500 cycles at a current density of 200 mA / g.

4. A method for preparing a Zr, Mg, Mo-doped lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: The following steps are involved: Step S1, adding a commercial nickel-manganese precursor into anhydrous ethanol, ultrasonically dispersing, and then stirring at a constant temperature; Step S2, slowly adding a certain amount of Zr alcohol ester into the mixture while stirring, and placing the obtained system in air and stirring at a constant temperature for a certain period of time; Step S3: After stirring, transfer the system into a reactor and add a certain amount of magnesium salt powder and (NH4)6Mo7O 24 4H2O, solvothermal reaction at 160~180℃, reaction time 8~12h; Step S4, after filtering, washing and drying, the solvent thermal reaction product is mixed with Li2CO3 and a certain amount of flux and ground, then calcined at a high temperature of 700-900°C, and naturally cooled to room temperature; Step S5: washing the calcined product with water and then drying it to finally obtain a Zr, Mg, and Mo-doped lithium-rich manganese-based positive electrode material.

5. The method for preparing a Zr, Mg, Mo-doped lithium-rich manganese-based positive electrode material according to claim 4, characterized in that: In the step S2, the amount of Zr alcohol ester used satisfies that the Zr atomic ratio is not higher than 1.5% of the product metal atoms.

6. The method for preparing a Zr, Mg, Mo-doped lithium-rich manganese-based positive electrode material according to claim 4, characterized in that: In step S3, the amount of magnesium salt powder used satisfies that the Mg atomic ratio is not higher than 2% of the product metal atoms, (NH4)6Mo7O 24 The amount of 4H2O used is such that the Mo atomic ratio is no more than 2% of the product metal atoms.

7. The method for preparing a Zr, Mg, Mo-doped lithium-rich manganese-based positive electrode material according to claim 4, characterized in that: In the step S4, the amount of Li2CO3 added is 5-10% more than the stoichiometric ratio, the amount of flux added is 400% of the molar number of metal atoms of the target product, and the flux includes KCl and NaCl, and the molar ratio of KCl to NaCl is 3:2.

Citation Information

Patent Citations

  • Composite lithium-rich positive electrode material and preparation method and application thereof

    CN111509206A

  • Fluorine ion gradient doped lithium-rich manganese-based positive electrode material as well as preparation method and application thereof

    CN114420920A

  • Lithium ion battery positive electrode material, preparation method and application thereof

    CN116207247A

  • Lithium-rich manganese-based layered positive electrode material based on morphology control and preparation method of lithium-rich manganese-based layered positive electrode material

    CN116454265A

  • Zr-Al co-doped cobalt-free lithium-rich manganese-based positive electrode material and preparation method thereof

    CN116598469A

Cited By

  • A lithium-rich manganese-based positive electrode material, a preparation method thereof and a lithium ion battery

    CN122968277A