Electrode plate and lithium ion battery

By using the combined use of ionic conductive agent and carbon material conductive agent in lithium-ion batteries, the side effects of carbon material conductive agent in positive and negative electrode reactions are solved, and the battery's low resistivity, high cycle performance and excellent high temperature are achieved performance.

CN119008957AInactive Publication Date: 2024-11-22DRAGONFLY LAB (SHENZHEN) CO LTD

Patent Information

Application Number
CN202411495996.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-25
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In existing lithium-ion batteries, the conductive agent of carbon material participates in redox during the positive and negative electrode reaction, resulting in battery capacity and safety problems, and it is difficult to separate the electronic conductivity and ionic conductivity functions.

Method used

The combination of ionic conductive agent and carbon material conductive agent is used to define the ratio of its mass ratio and oil absorption value to specific surface area, separate the electronic conductivity and ionic conductivity functions, reduce the use of carbon material conductive agent, and improve battery electrical performance and safety performance. .

Benefits of technology

The low resistivity, high cycle performance and excellent high temperature performance of the battery are achieved, which reduces side reactions and storage capacity losses and improves the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to the technical field of lithium ion batteries, in particular to an electrode plate and a lithium ion battery. The electrode plate comprises a current collector and an active material layer coated on the surface of the current collector, the active material layer comprises an active material and a conductive agent, and the conductive agent comprises an ionic conductive agent and a carbon material conductive agent; wherein the ionic conductive agent is MxOy, and M is any one or more of Mg, Al, Si, Ca, Ti and Zr; the ratio of the oil absorption value to the specific surface area of the ionic conductive agent is not less than 0.8; the mass ratio of the ionic conductive agent to the carbon material conductive agent is 1.5-20. According to the electrode plate, the ionic conductive agent and the carbon material conductive agent are combined to form the conductive agent, and the ratio of the oil absorption value to the specific surface area of the ionic conductive agent and the mass ratio of the ionic conductive agent to the carbon material conductive agent are limited to form the stable conductive slurry; the electrode plate with low resistivity and the lithium ion battery with excellent high-temperature performance and cycle performance are obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to an electrode plate and a lithium ion battery. Background Art

[0002] Lithium-ion batteries have the advantages of high operating voltage, wide operating temperature range, high energy density, large output power, no memory effect and long cycle life. They are not only widely used in 3C digital products such as mobile phones and laptops, but also have a broad application market in new energy vehicles and large-scale energy storage fields.

[0003] In order to increase the conductivity of the electrode plate, a conductive agent is added.

[0004] The conductive agent collects microcurrents between active materials and between active materials and current collectors to reduce the contact resistance of the electrodes and accelerate the movement rate of electrons.

[0005] In addition, the conductive agent can also improve the processing properties of the electrode and promote the infiltration of the electrolyte into the electrode. It can also effectively increase the migration rate of lithium ions in the electrode material and reduce polarization, thereby improving the charge and discharge efficiency of the electrode and the service life of the lithium battery.

[0006] Currently, carbon conductive agents, such as carbon black, are mainly used. However, they will directly participate in the reaction of positive and negative electrodes, which will have a certain impact on battery capacity, safety of use, etc.

[0007] Therefore, the above problems need to be improved. Summary of the invention

[0008] In order to solve the above technical problems, the present invention provides an electrode plate and a lithium-ion battery.

[0009] The present invention adopts the following technical solutions: An electrode plate, comprising a current collector and an active material layer coated on the surface of the current collector; the active material layer comprises an active material and a conductive agent, and the conductive agent comprises an ion conductive agent and a carbon material conductive agent; wherein: The ion conductive agent is MxOy, where M is any one or more of Mg, Al, Si, Ca, Ti, and Zr; The ratio of the oil absorption value to the specific surface area of ​​the ion conductive agent is not less than 0.8; The mass ratio of the ion conductive agent to the carbon material conductive agent is 1.5-20.

[0010] In lithium-ion batteries, electronic conductivity and ionic conductivity are generally accomplished by using carbon materials with high specific surface area. In fact, the two functions can be separated. Especially in batteries made of high surface density and high compaction electrodes, ionic conductivity is more important than electronic conductivity.

[0011] When only carbon material conductive agents are used, it will cause the side effect of electronic conductivity while completing the ion conductivity function, that is, it will participate in the redox reaction in the positive and negative electrodes, resulting in a loss of battery performance.

[0012] Therefore, the present invention combines ionic conductive agents and carbon material conductive agents as conductive agents, reduces the usage of carbon material conductive agents, and improves the influence of conductive agents on the electrical performance and safety performance of batteries.

[0013] The present invention limits the ratio of the oil absorption value to the specific surface area of ​​the ion conductive agent to not less than 0.8.

[0014] When the ratio of oil absorption value to specific surface area is too low, one reason is that the specific surface area is too large, which makes it difficult to process the slurry in the battery material slurrying process. Even if it can be processed, it is easy to cause the slurry to be unstable, resulting in difficulty in coating. Another reason is that the oil absorption value is too low, then it loses its function as a conductive agent.

[0015] When the ratio is within the specified value of the present invention, a balance between the oil absorption value and the specific surface area value of the ion conductive agent can be achieved, which not only has an effective conductive effect but also ensures the stability of the conductive slurry.

[0016] The present invention also limits the mass ratio of the ion conductive agent to the carbon material conductive agent to 1.5-20.

[0017] When the mass ratio of the ion conductive agent to the carbon material conductive agent is too large, the ion conductive agent content is too high and the carbon material content is too low, resulting in excessive resistivity of the electrode, causing battery polarization, increased impedance, and severe heat generation.

[0018] When the mass ratio of the ion conductive agent to the carbon material conductive agent is too small, the carbon material content is too high, resulting in an increase in the specific surface area of ​​the electrode and an increase in side reactions, leading to a loss of cycle or storage capacity.

[0019] Specifically, as an embodiment of the present invention, the mass ratio of the ion conductive agent to the carbon material conductive agent is 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20 or a range consisting of any two of these values.

[0020] Preferably, the mass ratio of the ion conductive agent to the carbon material conductive agent is 4-15.

[0021] Specifically, as an embodiment of the present invention, under the premise that the ratio of the oil absorption value to the specific surface area of ​​the ion conductive agent is greater than 0.8, in order to ensure the stability of the slurry and the appropriate oil absorption value and specific surface area, the oil absorption value of the ion conductive agent is 150-800 ml / 100 g, and the specific surface area of ​​the ion conductive agent is 60-500 m 2 / g.

[0022] More specifically, the ratio of the oil absorption value to the specific surface area of ​​the ion conductive agent is 0.85, 0.9, 1, 1.5, 2, 5, 6, 8, 10, 12, 15, 18, 20, 30, 40, 50, 60, 70, 80 or a range consisting of any two of these values.

[0023] When the ratio of the oil absorption value to the specific surface area is too large, it means that the pores of the particles on the surface of the material are very dense, the structure is complex to process, and the manufacturing cost will be very high.

[0024] Preferably, the ratio of the oil absorption value to the specific surface area of ​​the ion conductive agent is 1.5-10.

[0025] More specifically, the oil absorption value of the ion conductive agent is 150 ml / 100g, 200 ml / 100g, 250 ml / 100g, 300 ml / 100g, 350 ml / 100g, 400 ml / 100g, 450 ml / 100g, 500 ml / 100g, 600 ml / 100g, 700 ml / 100g, 800 ml / 100g or a range consisting of any two of these values.

[0026] The specific surface area of ​​the ion conductive agent is 60 m 2 / g, 80m 2 / g、100m 2 / g, 120m 2 / g, 150m 2 / g, 180m 2 / g, 200m 2 / g, 250m 2 / g、300m 2 / g, 350m 2 / g, 400m 2 / g, 450m 2 / g、500m 2 / g or a range consisting of any two of these values.

[0027] Specifically, as an embodiment of the present invention, the carbon material conductive agent includes one or more of carbon black, acetylene black, graphene, carbon nanotubes, and Ketjen black.

[0028] Specifically, as an embodiment of the present invention, based on the mass of the electrode plate being 100%, the mass percentage of the conductive agent in the electrode plate is 0.3-10%.

[0029] Specifically, as an embodiment of the present invention, the electrode plate is a positive electrode plate, the active material is a positive electrode active material, and the positive electrode active material is selected from at least one of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, lithium manganese iron phosphate, lithium nickel cobalt manganese oxide, and nickel manganese spinel.

[0030] Specifically, as an embodiment of the present invention, the electrode plate is a negative electrode plate, the active material is a negative electrode active material, and the negative electrode active material is selected from at least one of natural graphite, artificial graphite, mesophase carbon microbeads, lithium titanate, silicon alloy, tin alloy, and active lithium metal.

[0031] Specifically, as an embodiment of the present invention, the active material layer also includes a binder, and the binder includes polyvinylidene fluoride, a copolymer of vinylidene fluoride, polytetrafluoroethylene, a copolymer of vinylidene fluoride-hexafluoropropylene, a copolymer of tetrafluoroethylene-hexafluoropropylene, a copolymer of tetrafluoroethylene-perfluoroalkyl vinyl ether, a copolymer of ethylene-tetrafluoroethylene, a copolymer of vinylidene fluoride-tetrafluoroethylene, a copolymer of vinylidene fluoride-trifluoroethylene, a copolymer of vinylidene fluoride-trichloroethylene, a copolymer of vinylidene fluoride-fluoroethylene, a copolymer of vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene, thermoplastic polyimide, thermoplastic resins such as polyethylene and polypropylene; acrylic resin; and one or more of styrene butadiene rubber.

[0032] On the other hand, the present invention also provides a lithium-ion battery, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the positive electrode sheet and / or the negative electrode sheet is the above-mentioned electrode sheet.

[0033] The electrode plate of the present invention adopts an ion conductive agent and a carbon material conductive agent to form a conductive agent, and the ratio of the oil absorption value and the specific surface area of ​​the ion conductive agent and the mass ratio of the ion conductive agent and the carbon material conductive agent are limited to form a stable conductive slurry with good conductive effect, thereby obtaining an electrode plate with low resistivity and a lithium ion battery with excellent high temperature performance and cycle performance. DETAILED DESCRIPTION

[0034] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0035] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making any creative work shall fall within the protection scope of the present invention.

[0036] Example 1 The method for preparing a lithium-ion battery in this embodiment comprises the following steps: 1) Preparation of negative electrode The negative electrode active material artificial graphite, the conductive agent, and the negative electrode binder styrene-butadiene rubber were mixed in a mass ratio of 95:3:2, and then dispersed in deionized water to obtain a negative electrode slurry.

[0037] The slurry is coated on both sides of the copper foil, and after drying, rolling and vacuum drying, a nickel lead wire is welded on with an ultrasonic welder to obtain a negative electrode sheet.

[0038] The conductive agent includes carbon black and Al2O3, and the mass ratio of Al2O3 to carbon black is 10, and the ratio of the oil absorption value to the specific surface area of ​​Al2O3 is 4.

[0039] 3) Preparation of positive electrode Lithium iron phosphate, conductive carbon black Super-P and binder polyvinylidene fluoride (PVDF) are uniformly mixed in a mass ratio of 96:2:2, and then dispersed in N-methyl-2-pyrrolidone (NMP) to obtain a positive electrode slurry.

[0040] The slurry is evenly coated on both sides of the aluminum foil, and after drying, calendering and vacuum drying, a positive electrode material layer is obtained, and an aluminum lead wire is welded with an ultrasonic welder to obtain a positive electrode sheet.

[0041] 4) Preparation of electrolyte: Ethylene carbonate (EC) and diethyl carbonate (DEC) were mixed in a mass ratio of 1:1, and then lithium hexafluorophosphate (LiPF6) was added to a molar concentration of 1.0 mol / L.

[0042] 5) Battery Assembly: A three-layer separator with a thickness of 20 μm is placed between the positive plate and the negative plate, and then the positive plate, the negative plate and the separator are assembled into a soft-pack battery cell; an aluminum-plastic film material is selected for the outer shell for packaging and molding, and then the electrolyte injection, aging, formation, capacity division and other processes are carried out respectively to obtain a lithium-ion battery.

[0043] Example 2 This embodiment is basically the same as the embodiment 1, the only difference being that the negative electrode conductive agent is different, specifically: The mass ratio of Al2O3 to carbon black is 8.

[0044] Example 3 This embodiment is basically the same as the embodiment 1, the only difference being that the negative electrode conductive agent is different, specifically: The mass ratio of Al2O3 to carbon black is 15.

[0045] Example 4 This embodiment is basically the same as the embodiment 1, the only difference being that the negative electrode conductive agent is different, specifically: The mass ratio of Al2O3 to carbon black is 1.5.

[0046] Example 5 This embodiment is basically the same as the embodiment 1, the only difference being that the negative electrode conductive agent is different, specifically: The mass ratio of Al2O3 to carbon black is 4.

[0047] Example 6 This embodiment is basically the same as the embodiment 1, the only difference being that the negative electrode conductive agent is different, specifically: The mass ratio of Al2O3 to carbon black is 16.

[0048] Example 7 This embodiment is basically the same as the embodiment 1, the only difference being that the negative electrode conductive agent is different, specifically: The mass ratio of Al2O3 to carbon black is 20.

[0049] Example 8 This embodiment is basically the same as the embodiment 1, the only difference being that the negative electrode conductive agent is different, specifically: The ratio of oil absorption value to specific surface area of ​​Al2O3 is 1.5.

[0050] Example 9 This embodiment is basically the same as the embodiment 1, the only difference being that the negative electrode conductive agent is different, specifically: The ratio of oil absorption value to specific surface area of ​​Al2O3 is 5.

[0051] Example 10 This embodiment is basically the same as the embodiment 1, the only difference being that the negative electrode conductive agent is different, specifically: The ratio of oil absorption value to specific surface area of ​​Al2O3 is 10.

[0052] Embodiment 11 This embodiment is basically the same as the embodiment 1, the only difference being that the negative electrode conductive agent is different, specifically: The ratio of oil absorption value to specific surface area of ​​Al2O3 is 0.8.

[0053] Example 12 This embodiment is basically the same as the embodiment 1, the only difference being that the negative electrode conductive agent is different, specifically: The ratio of oil absorption value to specific surface area of ​​Al2O3 is 12.

[0054] Example 13 This embodiment is basically the same as the embodiment 1, the only difference being that the negative electrode conductive agent is different, specifically: The conductive agent includes carbon black and MgO, and the mass ratio of MgO to carbon black is 10. The ratio of the oil absorption value to the specific surface area of ​​MgO is 4.

[0055] Embodiment 14 This embodiment is basically the same as the embodiment 1, the only difference being that the negative electrode conductive agent is different, specifically: The conductive agent includes carbon black and SiO2, and the mass ratio of SiO2 to carbon black is 10, and the ratio of the oil absorption value to the specific surface area of ​​SiO2 is 4.

[0056] Embodiment 15 This embodiment is basically the same as the embodiment 1, the only difference being that the negative electrode conductive agent is different, specifically: The conductive agent includes carbon black and CaO, and the mass ratio of CaO to carbon black is 10. The ratio of the oil absorption value of CaO to the specific surface area is 4.

[0057] Example 16 This embodiment is basically the same as the embodiment 1, the only difference being that the negative electrode conductive agent is different, specifically: The conductive agent includes acetylene black and TiO2, and the mass ratio of TiO2 to acetylene black is 10, and the ratio of the oil absorption value to the specific surface area of ​​TiO2 is 4.

[0058] Embodiment 17 This embodiment is basically the same as the embodiment 1, the only difference being that the negative electrode conductive agent is different, specifically: The conductive agent includes carbon nanotubes and ZrO2, and the mass ratio of ZrO2 to the carbon nanotubes is 10. The ratio of the oil absorption value to the specific surface area of ​​ZrO2 is 4.

[0059] Embodiment 18 The method for preparing a lithium-ion battery in this embodiment comprises the following steps: 1) Preparation of negative electrode The negative electrode active material artificial graphite, the conductive carbon black Super-P, and the negative electrode binder styrene-butadiene rubber were mixed in a mass ratio of 95:3:2, and then dispersed in deionized water to obtain a negative electrode slurry.

[0060] The slurry is coated on both sides of the copper foil, and after drying, rolling and vacuum drying, a nickel lead wire is welded on with an ultrasonic welder to obtain a negative electrode sheet.

[0061] 3) Preparation of positive electrode Lithium iron phosphate, a conductive agent, and a binder polyvinylidene fluoride (PVDF) are uniformly mixed in a mass ratio of 96:2:2, and then dispersed in N-methyl-2-pyrrolidone (NMP) to obtain a positive electrode slurry.

[0062] The slurry is evenly coated on both sides of the aluminum foil, and after drying, calendering and vacuum drying, a positive electrode material layer is obtained, and an aluminum lead wire is welded with an ultrasonic welder to obtain a positive electrode sheet.

[0063] The conductive agent includes carbon black and Al2O3, and the mass ratio of Al2O3 to carbon black is 10, and the ratio of the oil absorption value to the specific surface area of ​​Al2O3 is 4.

[0064] 4) Preparation of electrolyte: Ethylene carbonate (EC) and diethyl carbonate (DEC) were mixed in a mass ratio of 1:1, and then lithium hexafluorophosphate (LiPF6) was added to a molar concentration of 1.0 mol / L.

[0065] 5) Battery Assembly: A three-layer separator with a thickness of 20 μm is placed between the positive plate and the negative plate, and then the positive plate, the negative plate and the separator are assembled into a soft-pack battery cell; an aluminum-plastic film material is selected for the outer shell for packaging and molding, and then the electrolyte injection, aging, formation, capacity division and other processes are carried out respectively to obtain a lithium-ion battery.

[0066] Embodiment 19 The method for preparing a lithium-ion battery in this embodiment comprises the following steps: 1) Preparation of negative electrode The negative electrode active material artificial graphite, the conductive agent, and the negative electrode binder styrene-butadiene rubber were mixed in a mass ratio of 95:3:2, and then dispersed in deionized water to obtain a negative electrode slurry.

[0067] The slurry is coated on both sides of the copper foil, and after drying, rolling and vacuum drying, a nickel lead wire is welded on with an ultrasonic welder to obtain a negative electrode sheet.

[0068] The conductive agent includes carbon black and Al2O3, and the mass ratio of Al2O3 to carbon black is 10, and the ratio of the oil absorption value to the specific surface area of ​​Al2O3 is 4.

[0069] 3) Preparation of positive electrode Lithium iron phosphate, a conductive agent, and a binder polyvinylidene fluoride (PVDF) are uniformly mixed in a mass ratio of 96:2:2, and then dispersed in N-methyl-2-pyrrolidone (NMP) to obtain a positive electrode slurry.

[0070] The slurry is evenly coated on both sides of the aluminum foil, and after drying, calendering and vacuum drying, a positive electrode material layer is obtained, and an aluminum lead wire is welded with an ultrasonic welder to obtain a positive electrode sheet.

[0071] The conductive agent includes carbon black and Al2O3, and the mass ratio of Al2O3 to carbon black is 10, and the ratio of the oil absorption value to the specific surface area of ​​Al2O3 is 4.

[0072] 4) Preparation of electrolyte: Ethylene carbonate (EC) and diethyl carbonate (DEC) were mixed in a mass ratio of 1:1, and then lithium hexafluorophosphate (LiPF6) was added to a molar concentration of 1.0 mol / L.

[0073] 5) Battery Assembly: A three-layer separator with a thickness of 20 μm is placed between the positive plate and the negative plate, and then the positive plate, the negative plate and the separator are assembled into a soft-pack battery cell; an aluminum-plastic film material is selected for the outer shell for packaging and molding, and then the electrolyte injection, aging, formation, capacity division and other processes are carried out respectively to obtain a lithium-ion battery.

[0074] Comparative Example 1 This comparative example is basically the same as Example 1, except that the negative electrode conductive agent is only carbon black.

[0075] Comparative Example 2 This comparative example is basically the same as Example 1, except that the negative electrode conductive agent is different, specifically: The mass ratio of Al2O3 to carbon black is 1.

[0076] Comparative Example 3 This comparative example is basically the same as Example 1, except that the negative electrode conductive agent is different, specifically: The mass ratio of Al2O3 to carbon black is 2:1.

[0077] Comparative Example 4 This comparative example is basically the same as Example 1, except that the negative electrode conductive agent is different, specifically: The ratio of oil absorption value to specific surface area of ​​Al2O3 is 0.6.

[0078] Comparative Example 5 The preparation method of the lithium ion battery in this comparative example comprises the following steps: 1) Preparation of negative electrode The negative electrode active material artificial graphite, the conductive carbon black Super-P, and the negative electrode binder styrene-butadiene rubber were mixed in a mass ratio of 95:3:2, and then dispersed in deionized water to obtain a negative electrode slurry.

[0079] The slurry is coated on both sides of the copper foil, and after drying, rolling and vacuum drying, a nickel lead wire is welded on with an ultrasonic welder to obtain a negative electrode sheet.

[0080] 3) Preparation of positive electrode Lithium iron phosphate, conductive carbon black Super-P and binder polyvinylidene fluoride (PVDF) are uniformly mixed in a mass ratio of 96:2:2, and then dispersed in N-methyl-2-pyrrolidone (NMP) to obtain a positive electrode slurry.

[0081] The slurry is evenly coated on both sides of the aluminum foil, and after drying, calendering and vacuum drying, a positive electrode material layer is obtained, and an aluminum lead wire is welded with an ultrasonic welder to obtain a positive electrode sheet.

[0082] 4) Preparation of electrolyte: Ethylene carbonate (EC) and diethyl carbonate (DEC) were mixed in a mass ratio of 1:1, and then lithium hexafluorophosphate (LiPF6) was added to a molar concentration of 1.0 mol / L.

[0083] 5) Battery Assembly: A three-layer separator with a thickness of 20 μm is placed between the positive plate and the negative plate, and then the positive plate, the negative plate and the separator are assembled into a soft-pack battery cell; an aluminum-plastic film material is selected for the outer shell for packaging and molding, and then the electrolyte injection, aging, formation, capacity division and other processes are carried out respectively to obtain a lithium-ion battery.

[0084] The lithium ion batteries prepared in the examples and comparative examples were subjected to performance tests as follows: Note: The currents involved in the following test methods are all expressed as xC, where x is a number and C represents the nominal capacity of the battery. For example, a charging current of a battery with a nominal capacity of 1Ah of 0.5C represents 0.5×1=0.5A, and 6C represents 6×1=6A.

[0085] 1. Four-probe electrode resistance ① Take the rolled electrode sample, stick a 50μm thick high-temperature tape on the surface of the electrode dressing, and roll it back and forth 5 times with a 2kg roller to ensure that the tape and the electrode dressing are well adhered and flat without bubbles; ② Peel off the electrode attached to the high-temperature tape, and obtain a sample with the dressing attached to the tape; ③ Use a φ14mm sampler to cut the sample in ② into several small discs for testing; ④ Test and record the thickness of each small disc in ③; ⑤ Aim the four-probe probe at the center of the small disc, input the sample diameter, thickness and other information on the equipment software, and adjust the test range and current value on the equipment according to the equipment prompts; ⑥ Click Test to get the resistivity value of the sample being tested.

[0086] 2. Initial charge and discharge efficiency ①Charging process: 0.05C constant current charging for 60 minutes; 0.1C constant current charging for 60 minutes; 0.2C constant current charging for 120 minutes; ② Capacity division step: 0.33C constant current constant voltage charging to 3.8V, 0.05C cut-off; 0.33C discharge to 2.0V; ③First charge and discharge efficiency = 0.33C discharge capacity / (0.05C charge capacity+0.1C charge capacity+0.2C charge capacity+0.33C constant current and constant voltage charge capacity) × 100%.

[0087] 3.6C constant current charging test and temperature test ① Stick the temperature probes to the positive ear, negative ear, and battery surface to test and record the temperature at each location; ② Place the battery in a 25℃ environment for 3 hours; ③0.33C constant current discharge to 2.0V, leave for 30 minutes; ④6C constant current charge to 3.8V, leave for 30 minutes; ⑤Record the 6C charging curve and the temperature change curve at each position.

[0088] 4.55℃ Cycle Test ① Place the soft-pack battery in a 55°C environment for 3 hours; ②1C constant current and constant voltage charging to 3.8V, 0.05C cut-off; leave for 30 minutes; ③1C constant current discharge to 2.0V; leave for 30 minutes; ④Cycle steps ②~③; ⑤ Repeat this cycle 500 times and record the first discharge capacity and the last discharge capacity.

[0089] The capacity retention rate of the cycle is calculated as follows: Battery capacity retention rate (%) = last discharge capacity / first discharge capacity × 100%.

[0090] 5.60℃ fully charged high temperature storage ① Capacity test: Place at 25℃ for 3h; Charge at 0.33C constant current and constant voltage to 3.8V, cut off at 0.05C, place for 30min; Discharge at 0.33C constant current to 2.0V, place for 30min; Cycle 3 times, record the average capacity value C0; ②Battery full charge: 0.33C0 constant current constant voltage charge to 3.8V, 0.05C cut-off; ③ After storing the fully charged battery in a 60℃ environment for 30 days, take out the battery and place it in a 25℃ environment. First, discharge it at a constant current of 0.33C0 to 2.0V and record the remaining capacity.

[0091] The performance test results of various embodiments and comparative examples are shown in Tables 1-4.

[0092] Table 1 Experimental comparison of different mass ratios of Al2O3 and carbon black

[0093] From the test results of Examples 1-7 and Comparative Examples 1-3 in Table 1, it can be seen that for the electrode plate of the present invention, when ionic conductive agents and carbon material conductive agents are selected as conductive agents, and the ratio of the oil absorption value to the specific surface area of ​​the ionic conductive agent is limited to not less than 0.8, and the mass ratio of the ionic conductive agent to the carbon material conductive agent is 1.5-20, the prepared electrode plate has a low impedance, and the lithium ion battery has good cycle performance and high temperature performance.

[0094] At the same time, it can be seen from the test results of Examples 1-7 that when the mass ratio of the ion conductive agent to the carbon material conductive agent is 4-15, the battery performance is better.

[0095] It can be seen from the test results of Comparative Examples 1-3 and Examples 1-7 that when the mass ratio of the ion conductive agent to the carbon material conductive agent is less than 1.5, or when only the carbon material conductive agent is used, the initial charge and discharge efficiency of the battery is low, and the 55°C cycle capacity retention rate is also low; when the mass ratio of the ion conductive agent to the carbon material conductive agent is greater than 20, the electrode impedance is large, resulting in a battery temperature exceeding 60°C at the end of 6C fast charging, and a large amount of heat generation.

[0096] Table 2 Experimental comparison of the ratio of oil absorption value to specific surface area of ​​different Al2O3

[0097] From the test results of Example 1, Examples 8-12 and Comparative Example 4 in Table 2, it can be seen that when the ratio of the oil absorption value to the specific surface area of ​​the ion conductive agent is too small, the 6C constant current charging ratio is low.

[0098] At the same time, it can be seen from the test results of Example 1 and Examples 8-12 that when the ratio of the oil absorption value to the specific surface area of ​​the ion conductive agent is in the range of 1.5 to 10, the cost is relatively low.

[0099] Table 3 Experimental comparison of ionic conductive agents of different materials

[0100] It can be seen from the test results of Example 1 and Examples 13-17 in Table 3 that for different types of MxOy ion conductive agents and carbon material conductive agents, as long as the ratio of the oil absorption value of the ion conductive agent to the specific surface area and the mass ratio of the ion conductive agent to the carbon material conductive agent meet the corresponding conditions, the impedance of the obtained electrode plates is low, and the battery cycle performance and high temperature performance are not much different, indicating that the electrode plates of the present invention are universal for different types of ion conductive agents and carbon material conductive agents.

[0101] Table 4 Experimental comparison of different positive and negative electrode formula ratios

[0102] It can be seen from the test results of Example 1, Examples 18-19 and Comparative Example 5 in Table 4 that the electrode plates of the present invention can be used as positive electrode plates and / or negative electrode plates. When the negative electrode conductive agent adopts ionic conductive agent and carbon material conductive agent, the initial charge and discharge efficiency of the battery is optimized; when the positive electrode conductive agent adopts ionic conductive agent and carbon material conductive agent, the high temperature storage performance of the battery is optimized; when both the positive and negative electrode conductive agents adopt ionic conductive agent and carbon material conductive agent, the battery performance is better.

[0103] Compared with using only carbon black as a conductive agent, the present invention can effectively reduce the impact of the side reactions caused by carbon black on the battery's charge and discharge performance and high-temperature performance, and help to obtain a lithium-ion battery with excellent high-temperature performance and cycle performance.

[0104] The present invention is further described above with the aid of specific embodiments. However, it should be understood that the specific description here should not be construed as limiting the essence and scope of the present invention. Various modifications made to the above embodiments by ordinary technicians in the field after reading this specification are all within the scope of protection of the present invention.

Claims

1. An electrode plate, characterized in that: It includes a current collector and an active material layer coated on the surface of the current collector; the active material layer includes an active material and a conductive agent, and the conductive agent includes an ion conductive agent and a carbon material conductive agent; wherein: The ion conductive agent is MxOy, where M is any one or more of Mg, Al, Si, Ca, Ti, and Zr; The ratio of the oil absorption value to the specific surface area of ​​the ion conductive agent is not less than 0.8; The mass ratio of the ion conductive agent to the carbon material conductive agent is 1.5-20.

2. The electrode plate according to claim 1, characterized in that: The oil absorption value of the ion conductive agent is 150-800 ml / 100 g.

3. The electrode plate according to claim 1, characterized in that: The specific surface area of ​​the ion conductive agent is 60-500m 2 / g.

4. The electrode plate according to claim 1, characterized in that: The ratio of the oil absorption value to the specific surface area of ​​the ion conductive agent is 1.5-10.

5. The electrode plate according to claim 1, characterized in that: The mass ratio of the ion conductive agent to the carbon material conductive agent is 4-15.

6. The electrode plate according to claim 1, characterized in that: The carbon material conductive agent includes one or more of carbon black, acetylene black, graphene, carbon nanotubes, and Ketjen black.

7. The electrode plate according to claim 1, characterized in that: Taking the mass of the electrode plate as 100%, the mass percentage of the conductive agent to the electrode plate is 0.3-10%.

8. The electrode plate according to claim 1, characterized in that: The electrode plate is a positive electrode plate, the active material is a positive electrode active material, and the positive electrode active material is selected from at least one of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, lithium manganese iron phosphate, lithium nickel cobalt manganese oxide, and nickel manganese spinel.

9. The electrode plate according to claim 1, characterized in that: The electrode plate is a negative electrode plate, the active material is a negative electrode active material, and the negative electrode active material is selected from at least one of natural graphite, artificial graphite, mesophase carbon microspheres, lithium titanate, silicon alloy, tin alloy, and active lithium metal.

10. A lithium ion battery, characterized in that: It comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the positive electrode sheet and / or the negative electrode sheet is the electrode sheet according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Ionic conductive agent, electrode plate group and lithium ion battery

    CN115050965A

  • Positive electrode composition for lithium ion secondary battery, positive electrode for lithium ion secondary battery, and lithium ion secondary battery

    CN116031384A

  • Method and device to prevent damage from storm and flood damage on construction sites using a digital elevation model

    KR1020220043933A

Cited By

  • Current collector, electrode plate and lithium ion battery

    CN119230843A

  • Lithium-intercalated silicon carbon material, preparation method thereof and application of lithium-intercalated silicon carbon material in lithium ion battery

    CN120767318A

  • A lithium intercalation silicon-carbon material, its preparation method and use in lithium ion batteries

    CN120767318B