Electrolyte, battery, battery pack and electric equipment

By using 1,3-bis(2-fluoroethoxy)propane and lithium salt in the electrolyte, the side reaction and safety of the battery at high temperature are solved, and the stability of the battery is improved. life.

CN119009088APending Publication Date: 2024-11-22BYD CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410918459.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In high-temperature environments, heat is prone to accumulate inside the battery, resulting in damage to the electrode-electrolyte interface layer structure, aggravation of side reactions, reducing battery life, and may cause safety problems such as uneven metal deposition and battery short circuit.

Method used

1,3-bis(2-fluoroethoxy)propane is used as the solvent of the electrolyte, combined with lithium salt, adjust the ion-solvent coordination structure, reduce free solvent, inhibit side reactions, improve oxidative stability, and pass diluent Optimize conductivity.

Benefits of technology

It improves the battery's service stability and life in high temperature environments, extends the battery's service life, and improves the battery's safety and charging and discharging performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009088A_ABST
    Figure CN119009088A_ABST
Patent Text Reader

Abstract

The invention discloses an electrolyte, a battery, a battery pack and electric equipment, and the electrolyte comprises 1, 3-bis (2-fluoroethoxy) propane and an electrolyte salt. Wherein the electrolyte salt comprises a lithium salt. According to the electrolyte disclosed by the invention, the 1, 3-bis (2-fluoroethoxy) propane is adopted as the solvent, so that an ion-solvent coordination structure is favorably adjusted, and a free solvent in the electrolyte is reduced, thereby inhibiting side reaction of the electrolyte at a high temperature, improving the oxidation stability of the electrolyte and further improving the use stability of a battery in a high-temperature environment; and the service life of the battery is prolonged. Besides, the size of an ion-solvent aggregate in the electrolyte can be reduced by forming an ion-solvent coordination structure, so that the conductivity of ions in the electrolyte is improved, and the usability of the battery is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to an electrolyte, a battery, a battery pack and an electrical device. Background Art

[0002] In a high temperature environment, heat easily accumulates inside the battery, so the internal temperature of the battery can reach above 60°C. The high temperature inside the battery will accelerate the dissolution of the electrode-electrolyte interface layer, seriously destroy the structure and composition of the electrode-electrolyte interface layer, aggravate the side reactions inside the battery, cause the battery to fail prematurely, and reduce the battery life. In addition, high temperature will also bring problems such as uneven metal deposition, and uneven metal deposition will produce dendrites that pierce the diaphragm, causing a short circuit inside the battery, further inducing battery safety and other problems.

[0003] In the related art, film-forming additives are often added to the electrolyte of the battery to construct a stable electrode-electrolyte interface layer, thereby inhibiting the contact between the electrode and the electrolyte. However, the above solution is difficult to reduce the side reactions between the electrolyte and the electrode, and the improvement effect on the battery is not significant. Summary of the invention

[0004] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the first object of the present invention is to provide an electrolyte that can improve the use stability of a battery in a high temperature environment.

[0005] A second object of the present invention is to provide a battery.

[0006] A third objective of the present invention is to provide a battery pack.

[0007] A fourth object of the present invention is to provide an electrical device.

[0008] The electrolyte according to the first embodiment of the present invention includes: 1,3-bis(2-fluoroethoxy)propane and an electrolyte salt, wherein the electrolyte salt includes a lithium salt.

[0009] According to the electrolyte of the embodiment of the present invention, 1,3-bis(2-fluoroethoxy)propane is used as a solvent, which is conducive to adjusting the ion-solvent coordination structure, reducing the free solvent in the electrolyte, thereby inhibiting the side reaction of the electrolyte at high temperature, improving the oxidation stability of the electrolyte, and thus improving the stability of the battery in a high temperature environment, and extending the life of the battery. In addition, by forming an ion-solvent coordination structure, the size of the ion-solvent aggregates in the electrolyte can be reduced, thereby improving the conductivity of the ions in the electrolyte, thereby improving the usability of the battery.

[0010] According to some embodiments of the present invention, the electrolyte salt includes at least one of LiPF6, LiBF4, LiNO3, LiCF3SO3, Li(FSO2)2N, and F2LiNO4S2.

[0011] According to some embodiments of the present invention, the molar concentration of the electrolyte salt in the electrolyte is 0.4 mol / L to 2 mol / L.

[0012] According to some embodiments of the present invention, the weight percentage of 1,3-bis(2-fluoroethoxy)propane in the electrolyte is 0.01 wt % to 99 wt %.

[0013] According to some embodiments of the present invention, the electrolyte further includes a diluent, and the diluent and the 1,3-bis(2-fluoroethoxy)propane form a solution of the electrolyte.

[0014] According to some embodiments of the present invention, the solution comprises, by mass percentage, 68% to 91% of the diluent and 9% to 32% of the 1,3-bis(2-fluoroethoxy)propane.

[0015] According to some embodiments of the present invention, the diluent includes: at least one of 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, 1-(2,2,2-trifluoroethoxy)-1,1,2,2-tetrafluoroethane, 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, bis(2,2,2-trifluoroethyl) ether, tris(2,2,2-trifluoroethyl) orthoformate, 1H,1H,5H-octafluoropentyl acrylate-1,1,2,2-tetrafluoroethyl ether, fluorobenzene and 1,3,5-trifluorobenzene.

[0016] A battery according to an embodiment of the second aspect of the present invention comprises: a positive electrode sheet, a lithium metal negative electrode sheet, a separator and an electrolyte, wherein the electrolyte is the electrolyte according to the embodiment of the first aspect of the present invention.

[0017] According to some embodiments of the present invention, the positive electrode sheet includes at least one of lithium iron phosphate, a ternary positive electrode material, lithium cobalt oxide, lithium manganese oxide, and a lithium-rich manganese-based material.

[0018] A battery pack according to an embodiment of a third aspect of the present invention comprises at least one battery according to an embodiment of the second aspect of the present invention.

[0019] An electric device according to an embodiment of a fourth aspect of the present invention comprises at least one battery pack according to an embodiment of the third aspect of the present invention.

[0020] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0022] Figure 1 is a schematic diagram of the reaction mechanism of 1,3-bis(2-fluoroethoxy)propane and lithium ions according to an embodiment of the present invention;

[0023] Figure 2 2 is a graph of high temperature lithium metal coulombic efficiency according to Example 1 of the present invention and Comparative Example 1;

[0024] Figure 3 It is the long cycle performance of the lithium metal||NMC811 battery at high temperature (50° C.) in Example 1 of the present invention and Comparative Example 1;

[0025] Figure 4 is the gas production of the first cycle of the Li||NMC811 battery in Example 1 and Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0026] Reference below Figure 1-Figure 4 An electrolyte according to an embodiment of the present invention is described.

[0027] The electrolyte according to an embodiment of the present invention includes 1,3-bis(2-fluoroethoxy)propane and an electrolyte salt. Among them, 1,3-bis(2-fluoroethoxy)propane has a strong solvating ability, which is conducive to adjusting the ion-solvent coordination structure, reducing the free solvent in the electrolyte, thereby inhibiting the side reaction of the electrolyte at high temperature, improving the oxidation stability of the electrolyte, improving the stability of the battery when used in a high temperature environment, and extending the life of the battery. In addition, by forming an ion-solvent coordination structure, the size of the ion-solvent aggregates in the electrolyte can be reduced, thereby improving the conductivity of the ions in the electrolyte, which is conducive to improving the safety of the battery.

[0028] Specifically, in the electrolyte, after the electrolyte salt is dissolved in 1,3-bis(2-fluoroethoxy)propane, it can dissociate into cations and anions. Under the action of the electric field, the above cations and anions can move in 1,3-bis(2-fluoroethoxy)propane, so that the charge can be conducted between the positive and negative electrodes of the battery to realize the charging and discharging process.

[0029] The structural formula of 1,3-bis(2-fluoroethoxy)propane is relatively simple. For example, there is no substituent on the main chain that forms the six-membered ring, which is conducive to reducing the steric hindrance effect, thereby reducing the steric hindrance between 1,3-bis(2-fluoroethoxy)propane and lithium ions, and promoting the lithium ions to coordinate with two oxygen atoms, which is conducive to forming a stable six-membered ring structure. Furthermore, the end group is a methyl group substituted with a single F atom, and the F atom is used to derive the LiF interface layer, while avoiding the end group selected from difluoro or trifluoro, which causes F to coordinate with lithium ions due to the large electronegativity of F, making it difficult to form a six-membered ring. Therefore, 1,3-bis(2-fluoroethoxy)propane, through a simple main chain structure and a single fluorine end group, enables the solvent molecule to derive the LiF interface layer and form a stable six-membered ring structure with lithium ions, thereby reducing the size of the ion-solvent aggregate, thereby improving the ionic conductivity of the electrolyte.

[0030] The electrolyte salt includes a lithium salt. The lithium salt has good ionic conductivity, moderate solvation ability and high electrochemical stability. Therefore, the lithium salt has good solubility in 1,3-bis(2-fluoroethoxy)propane and is conducive to coordination with 1,3-bis(2-fluoroethoxy)propane to reduce the size of ion-solvent aggregates, thereby improving the ionic conductivity of the electrolyte.

[0031] For example, refer to Figure 1 , lithium ions react with 1,3-bis(2-fluoroethoxy)propane to form a six-membered cyclic compound, that is, the coordination structure of lithium ions and 1,3-bis(2-fluoroethoxy)propane is realized. The free solvent in the electrolyte is reduced, and the six-membered ring is stable and not easy to decompose at high temperatures, thereby inhibiting the side reactions of the electrolyte at high temperatures, improving the oxidation stability of the electrolyte, improving the stability of the battery in high temperature environments, and extending the battery life.

[0032] According to the electrolyte of the embodiment of the present invention, 1,3-bis(2-fluoroethoxy)propane is used as a solvent, which is conducive to adjusting the ion-solvent coordination structure, reducing the free solvent in the electrolyte, thereby inhibiting the side reaction of the electrolyte at high temperature, improving the oxidation stability of the electrolyte, and then improving the stability of the battery when used in a high temperature environment, thereby extending the life of the battery. In addition, by forming an ion-solvent coordination structure, the size of the ion-solvent aggregates in the electrolyte can be reduced, thereby improving the conductivity of the ions in the electrolyte, thereby improving the usability of the battery. For example, the battery can be kept at a capacity retention rate of 86% after 100 cycles at high temperature (50°C).

[0033] According to some embodiments of the present invention, the electrolyte salt includes at least one of LiPF6, LiBF4, LiNO3, LiCF3SO3, Li(FSO2)2N, and F2LiNO4S2. The above lithium salts (i.e., LiPF6, LiBF4, LiNO3, LiCF3SO3, Li(FSO2)2N, and F2LiNO4S2) all have good thermal stability and electrochemical stability, so selecting at least one of the above lithium salts as the electrolyte salt is conducive to reducing the risk of thermal runaway, allowing the electrolyte to maintain good stability during the battery charge and discharge cycle, and improving the safety of the electrolyte.

[0034] According to some specific embodiments of the present invention, the molar concentration of the electrolyte salt in the electrolyte is 0.4mol / L to 2mol / L. When the molar concentration of the electrolyte salt in the electrolyte is less than 0.4mol / L, the electrolyte salt is less, so the ion-solvent interaction is small, the content of the free solvent in the electrolyte is increased, and it is difficult to suppress the parasitic reaction between the electrolyte and the electrode; when the molar concentration of the electrolyte salt in the electrolyte is greater than 2mol / L, the electrolyte salt is more, so it is difficult to ensure that all the electrolyte salts are dissolved, the fluidity of the electrolyte is reduced, and it is difficult to give full play to the role of the electrolyte. Therefore, by setting the molar concentration of the electrolyte salt in the electrolyte to: 0.4mol / L to 2mol / L, the electrolyte salt is fully dissolved, and the ion-solvent interaction is ensured, the content of the free solvent in the electrolyte is reduced, and the reaction between the electrolyte and the electrode is suppressed as much as possible to extend the life of the battery.

[0035] According to some embodiments of the present invention, the weight percentage of 1,3-bis(2-fluoroethoxy)propane in the electrolyte is: 0.01wt% to 99wt%. When the weight percentage of 1,3-bis(2-fluoroethoxy)propane in the electrolyte is less than 0.01wt%, the electrolyte is easy to react with the electrode, and the ion-solvent interaction between 1,3-bis(2-fluoroethoxy)propane and ions is difficult to meet the needs of the battery. When the weight percentage of 1,3-bis(2-fluoroethoxy)propane in the electrolyte is greater than 99wt%, 1,3-bis(2-fluoroethoxy)propane is more, which reduces the mass percentage of electrolyte salts in the electrolyte, making it difficult to give full play to the role of the electrolyte.

[0036] Thus, the weight percentage of 1,3-bis(2-fluoroethoxy)propane in the electrolyte is set to 0.01wt% to 99wt%, giving full play to the interaction between ions and solvents, and suppressing the reaction between the electrolyte and the electrode as much as possible to extend the life of the battery. Optionally, the weight percentage of 1,3-bis(2-fluoroethoxy)propane in the electrolyte is 0.01%, 0.1%, 1%, 10%, 50% or 99wt%. No specific limitation is made here.

[0037] According to some embodiments of the present invention, the electrolyte further includes a diluent, and the diluent and 1,3-bis(2-fluoroethoxy)propane form a solution of the electrolyte. The diluent can reduce the viscosity of the electrolyte, facilitate the diffusion and conduction of the electrolyte salt, increase the migration rate of ions, and improve the conductivity, thereby improving the charge and discharge performance of the battery. The diluent can also adjust the solvation environment of the electrolyte salt to enhance the stability of the electrolyte salt in 1,3-bis(2-fluoroethoxy)propane and improve the cycle life and safety performance of the battery. In lithium metal batteries, the diluent can control the formation of SEI (solid electrolyte interface), that is, the diluent promotes the formation of SEI rich in inorganic components by enhancing the interaction between anions and Li+. The SEI is relatively stable, which is beneficial to inhibit the growth of lithium dendrites and improve the safety of the battery.

[0038] Furthermore, the solution includes, by mass percentage, 68% to 91% of a diluent and 9% to 32% of 1,3-bis(2-fluoroethoxy)propane. By setting a more reasonable molar ratio of the electrolyte salt to the diluent, it is beneficial to improve the conductivity of the electrolyte, thereby improving the charge and discharge performance of the battery.

[0039] According to some embodiments of the present invention, the diluent includes at least one of: 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, 1-(2,2,2-trifluoroethoxy)-1,1,2,2-tetrafluoroethane, 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, bis(2,2,2-trifluoroethyl) ether, tris(2,2,2-trifluoroethyl) orthoformate, 1H,1H,5H-octafluoropentyl acrylate-1,1,2,2-tetrafluoroethyl ether, fluorobenzene and 1,3,5-trifluorobenzene. The above diluents all have a high boiling point and high oxidation stability. Using at least one of the above diluents is conducive to making the electrolyte suitable for use at a higher operating temperature and is conducive to forming a stable SEI film on the electrode. The SEI film has a high ionic conductivity, which is conducive to protecting the battery electrode, reducing the side reaction between the electrode and the electrolyte, and improving the cycle life of the battery.

[0040] Optionally, the molar ratio of the electrolyte salt to the diluent is 1:0.01, 1:0.05, 1:0.1, 1:0.5, 1:1, 1:0.5 or 1:10, which is not specifically limited here.

[0041] The battery according to the second embodiment of the present invention comprises: a positive electrode sheet, a lithium metal negative electrode sheet, a separator and an electrolyte, wherein the electrolyte is the electrolyte according to the first embodiment of the present invention.

[0042] The battery according to the embodiment of the present invention includes a positive electrode sheet, a lithium metal negative electrode sheet, a separator and the above-mentioned electrolyte, which is conducive to improving the charging and discharging performance of the battery, extending the life of the battery in a high temperature environment, and improving the market competitiveness of the battery.

[0043] According to some embodiments of the present invention, the positive electrode sheet includes at least one of lithium iron phosphate, ternary positive electrode material, lithium cobalt oxide, lithium manganese oxide, and lithium-rich manganese-based material. The above inorganic substances all have good thermal stability. The positive electrode sheet uses the above inorganic substances, which is conducive to improving the safety of the positive electrode sheet, reducing the risk of thermal runaway of the positive electrode sheet, and extending the service life of the positive electrode sheet.

[0044] A battery pack according to an embodiment of a third aspect of the present invention comprises at least one battery according to an embodiment of the second aspect of the present invention.

[0045] The battery pack according to the embodiment of the present invention is conducive to improving the charging and discharging performance of the battery pack in a high temperature environment and extending the use stability of the battery pack in a high temperature environment.

[0046] An electric device according to an embodiment of a fourth aspect of the present invention comprises at least one battery pack according to an embodiment of the third aspect of the present invention.

[0047] The electric device according to the embodiment of the present invention enriches the use conditions of the electric device, which is conducive to improving the operation stability of the electric device and improving the user experience of the electric device.

[0048] The embodiments of the present invention are described in detail below. It should be noted that the embodiments described below are exemplary and are only used to explain the present invention, and cannot be interpreted as limiting the present invention. In addition, if not explicitly stated, all reagents used in the following embodiments are commercially available, or can be synthesized according to this article or known methods, and the reaction conditions not listed are also easily available to those skilled in the art.

[0049] Example 1

[0050] In this embodiment, the electrolyte is composed of an ether solvent, an electrolyte salt and a diluent, wherein the solvent is 1,3-bis(2-fluoroethoxy)propane, the electrolyte salt is lithium bis(fluorosulfonyl)imide, and the diluent is 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether.

[0051] Lithium bis(fluorosulfonyl)imide, 1,3-bis(2-fluoroethoxy)propane, and a diluent are weighed to prepare a local high-concentration ether electrolyte, wherein the mass percentage of the ether solvent in the solution is 23%, the mass percentage of the diluent is 77%, and the concentration of the electrolyte salt in the electrolyte is about 1M.

[0052] Example 2

[0053] The difference between Example 2 and Example 1 is that the mass percentage of the ether solvent in the solution is 9%, and the mass percentage of the diluent is 91%.

[0054] Example 3

[0055] The difference between Example 3 and Example 1 is that the mass percentage of the ether solvent in the solution is 32%, and the mass percentage of the diluent is 68%.

[0056] Example 4

[0057] Example 4 differs from Example 1 in that no diluent is included.

[0058] Example 5

[0059] The difference between Example 5 and Example 2 is that the concentration of the electrolyte salt in the electrolyte is about 0.4M.

[0060] Example 6

[0061] The difference between Example 6 and Example 3 is that the concentration of the electrolyte salt in the electrolyte is about 1.5M.

[0062] Comparative Example 1

[0063] The electrolyte of Comparative Example 1 is composed of an electrolyte salt and a solvent, wherein the electrolyte salt is lithium hexafluorophosphate, and the solvent is dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate. The volume ratio of the solvents of different components is 1:1:1, and the concentration of the electrolyte is 1M.

[0064] Comparative Example 2

[0065] Comparative Example 2 is substantially the same as Comparative Example 1, except that 10% of fluoroethylene carbonate (FEC) is further added.

[0066] Table 1 Data of Examples 1 to 6 of the present invention and Comparative Examples 1 to 2

[0067]

[0068]

[0069] Performance Testing

[0070] 1. Coulomb efficiency test:

[0071] Assemble Li||Cu half-cells to measure the coulombic efficiency of lithium metal in electrolyte.

[0072] Preparation is as follows: 450 μm thick lithium metal sheet is cut into a sheet with a diameter of 16 mm and used as the negative electrode of the half-cell, 9 μm thick Cu foil is cut into a sheet with a diameter of 19 mm and used as the positive electrode of the half-cell. Celgard separator (2500) is cut into a sheet with a diameter of 19 mm and used as the separator of the half-cell.

[0073] Test: The assembled Li||Cu half-cell was tested for zinc metal coulombic efficiency at room temperature (25°C). 2 After the current is discharged to 0.005V, it is then discharged at 1mA / cm 2 The current is charged to 1V. This is considered a cycle, and the cycle is repeated 100 times. The data after each cycle is recorded by a blue electricity tester (model CT3002A). The average coulomb efficiency of 100 cycles is taken as the average coulomb efficiency. The test results are as follows Figure 2 shown.

[0074] 2. Long cycle test

[0075] Assemble Li||NMC811 batteries to measure the long-term cycle stability of the batteries.

[0076] The preparation is as follows: a 450 μm thick lithium metal sheet is cut into a 16 mm diameter sheet and used as a half-cell negative electrode, with an active material loading of 22 mg / cm 2 NMC811 was used as the positive electrode. Celgard separator (2500) was cut into a diameter of 19 mm and used as the separator of the half-cell.

[0077] Test: Charge the assembled Li||NMC811 battery from the open circuit potential to 4.6V at a rate of 0.1C at room temperature (50°C), and then discharge it to 2.8V at a rate of 0.1C. This is considered a cycle, and the battery is activated after 3 cycles. Subsequently, increase the charge and discharge current density, charge from the open circuit potential to 4.6V at a rate of 1 / 3C, and then discharge it to 2.8V at a rate of 1 / 3C. This is considered a cycle, and after 100 cycles, take the average coulombic efficiency and capacity retention rate. The data after each cycle is recorded using a blue electricity tester (model CT3002A). The specific test results are as follows: Figure 3 shown.

[0078] 3. The electrolyte in the embodiment was selected as the research object, and the comparative example was used as the control group. After the Li||NMC811 battery was assembled, the gas production of the battery during the cycle was measured by in-situ differential electrochemical mass spectrometry. The test cutoff potential was 2.8-4.6V, and the test temperature was 50°C. The specific test results are as follows Figure 4 shown.

[0079] Table 2 Test results of Examples 1 to 6 of the present invention and Comparative Examples 1 to 2

[0080] Average Coulombic efficiency Capacity retention rate <![CDATA[Gas production μmol / m 2 > Example 1 99.70% 86% 124 Example 2 99.2% 78% 221 Example 3 99.5% 81% 174 Example 4 89.00% 55% 392 Example 5 99.20% 78% 221 Example 6 99.50% 81% 174 Comparative Example 1 82.40% 20% 643 Comparative Example 2 88.50% 46% 466

[0081] Test Results

[0082] Combining Table 1 and Figure 2 In Comparative Example 1, the high-temperature lithium metal coulombic efficiency is only 82.4%, which is due to the strong reactivity of the carbonate electrolyte to lithium metal, resulting in low lithium metal coulombic efficiency, and the side reaction between lithium metal and the electrolyte is aggravated at high temperature. In contrast, the lithium metal coulombic efficiency in Example 1 is 99.5%, which is mainly due to the fact that the electrolyte with strong solvation ability can inhibit the side reaction between the free solvent and the negative electrode, thereby improving the high-temperature performance of the lithium metal negative electrode.

[0083] Combining Table 1 and Figure 3 The long cycle performance of the Li||NMC811 battery in Comparative Example 1 is significantly reduced, and the battery capacity retention rate is only about 20% after 20 cycles. However, the capacity retention rate of the Li||NMC811 battery in Example 1 is as high as 86% (after 100 cycles).

[0084] Combining Table 1 and the figure, in Comparative Example 1, Li||NMC811 has an ultra-high yield of 643 μmol / m during the first cycle. 2 This is mainly because the electrolyte reacts seriously with the electrode at high temperature and produces a lot of gas (CO2, H2), which causes the battery to fail prematurely. In contrast, the gas production of the electrolyte in Example 1 in the first cycle is only 124 μmol / m 2 The low gas production in Example 1 is attributed to the fact that the decomposition of the electrolyte is significantly suppressed.

[0085] Among them, lithium metal has an ultra-high coulombic efficiency of 99.7% at a high temperature of 50°C, and the capacity retention rate of the Li||NMC811 battery is 86% after 100 cycles at high temperature (50°C). That is, the lithium ion-1,3-bis(2-fluoroethoxy)propane coordination structure can effectively enhance the ion-solvent interaction, thereby reducing the content of free solvent in the electrolyte. In addition, the lithium ion-1,3-bis(2-fluoroethoxy)propane coordination structure can greatly reduce the size of ion-solvent aggregates, thereby improving the ionic conductivity of the electrolyte.

[0086] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example.

[0087] Although the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the claims and their equivalents.

Claims

1. An electrolyte, characterized in that: include: 1,3-bis(2-fluoroethoxy)propane and an electrolyte salt, Wherein, the electrolyte salt includes a lithium salt.

2. The electrolyte according to claim 1, characterized in that The electrolyte salt includes at least one of LiPF6, LiBF4, LiNO3, LiCF3SO3, Li(FSO2)2N, and F2LiNO4S2.

3. The electrolyte according to claim 1, characterized in that The molar concentration of the electrolyte salt in the electrolyte solution is 0.4 mol / L to 2 mol / L.

4. The electrolyte according to any one of claims 1 to 3, characterized in that The weight percentage of 1,3-bis(2-fluoroethoxy)propane in the electrolyte is 0.01wt% to 99wt%.

5. The electrolyte according to any one of claims 1 to 3, characterized in that Also includes: A diluent, wherein the diluent and the 1,3-bis(2-fluoroethoxy)propane form a solution of the electrolyte.

6. The electrolyte according to claim 5, characterized in that Calculated by mass percentage, the solution comprises: 68% to 91% of the diluent and 9% to 32% of the 1,3-bis(2-fluoroethoxy)propane.

7. The electrolyte according to claim 6, characterized in that The diluent includes: at least one of 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, 1-(2,2,2-trifluoroethoxy)-1,1,2,2-tetrafluoroethane, 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, bis(2,2,2-trifluoroethyl) ether, tris(2,2,2-trifluoroethyl) orthoformate, 1H,1H,5H-octafluoropentyl acrylate-1,1,2,2-tetrafluoroethyl ether, fluorobenzene and 1,3,5-trifluorobenzene.

8. A battery comprising: A positive electrode sheet, a lithium metal negative electrode sheet, a separator and an electrolyte, wherein the electrolyte is the electrolyte according to any one of claims 1 to 7.

9. The battery according to claim 8, characterized in that The positive electrode material includes at least one of lithium iron phosphate, ternary positive electrode material, lithium cobalt oxide, lithium manganese oxide, and lithium-rich manganese-based material.

10. A battery pack, characterized in that: Comprising at least one battery according to any one of claims 8-9.

11. An electrical device, characterized in that: Comprising at least one battery pack according to claim 10.