Preparation method of zwitter-ion modified PVDF (Polyvinylidene Fluoride) polymer electrolyte

By using pyridine propane sulfonate salt as PVDF electrolyte additive in lithium metal batteries, the low ion conductivity and electrochemical stability of polymer solid electrolytes are solved. The cycle stability and performance of lithium metal batteries have been significantly improved.

CN119009093AActive Publication Date: 2024-11-22SICHUAN CHENGKEGUO RENEWABLE ENERGY CO LTD

Patent Information

Application Number
CN202410984911.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-22
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

The existing polymer solid electrolytes have low ionic conductivity and insufficient electrochemical stability, resulting in limited safety and cyclic stability of lithium metal batteries, especially because PVDF is in the -H and -F positions during lithium ion transport. Point contact leads to a dehydrogenation and defluorination reaction, reducing the stability of the battery.

Method used

Pyridine propane sulfonate salt (PPS) is used as the PVDF electrolyte additive, and lithium ions and polar solvents are adsorbed through its N+ and SO3-sites to reduce the contact between lithium ions and the -H and -F sites of PVDF, and inhibit dehydrogenation and defluorescence. Reactions to improve the stability and ionic conductivity of the lithium anode and battery.

Benefits of technology

While improving the ionic conductivity of lithium metal batteries, it can enhance the stability of lithium negative electrodes and batteries, extend the cycle life of lithium symmetric button batteries, lithium-ternary batteries and lithium-iron phosphate batteries, significantly improving the cycle of batteries Stability and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009093A_ABST
    Figure CN119009093A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a zwitter-ion modified PVDF polymer electrolyte, and belongs to the technical field of lithium metal batteries, and the preparation method specifically comprises the following steps: mixing PVDF particles, a lithium salt, pyridinium propane sulfonate and a polar organic solvent, stirring to obtain a uniform viscous solution, covering the surface of a substrate with the uniform viscous solution, and carrying out vacuum drying to obtain the zwitter-ion modified PVDF polymer electrolyte; wherein the concentration of the PVDF particles in the uniform viscous solution is 80-120 g / L, the concentration of the lithium salt in the uniform viscous solution is 10-120 g / L, and the concentration of the pyridinium propane sulfonate in the uniform viscous solution is 5-60 g / L. The pyridinium propane sulfonate is adopted as a PVDF electrolyte additive, so that ion transmission is promoted, the stability of PVDF and a lithium negative electrode is considered, dehydrogenation and defluorination side reactions are inhibited, and the stability of the lithium negative electrode and the performance and cycling stability of the polymer electrolyte-based lithium metal battery are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium metal batteries, and in particular relates to a method for preparing a zwitterion-modified PVDF polymer electrolyte. Background Art

[0002] Due to the high reactivity between the lithium negative electrode and the electrolyte, the lithium metal battery (LMB) of the liquid electrolyte system is prone to thermal failure problems such as short circuit and combustion. This phenomenon is more prominent and serious in the application fields where the energy density / capacity released by the LMB is required to be high, the test conditions are relatively strict, and the quality of the battery active materials is high. Compared with the liquid battery system, the solid (SSE) / quasi-solid electrolyte system contains fewer or trace organic plasticizer / solvent molecules, so it has a higher battery safety factor than the liquid electrolyte system, and also has higher mechanical strength to resist dendrite growth. Therefore, in order to solve the high risk of safety in the liquid electrolyte system LMB, the solid / quasi-solid electrolyte system LMB has received intensive attention and research in recent years. Among them, the polymer (quasi) solid electrolyte LMB has great development and application advantages due to its simpler preparation method, higher flexibility, and lower sensitivity to air and water oxygen than inorganic solid electrolytes. However, the polymer electrolyte (PESSE) has low ionic conductivity and narrow electrochemical stability window, which limits its further development and application. Therefore, improving the ionic conductivity and electrochemical stability of PESSE is an important strategy to enhance PESSE-based LMBs.

[0003] Since PESSE mainly relies on the movement of its internal domain chains to transport lithium ions Li + , its ionic conductivity mainly depends on the structure of polar groups with adsorptive properties in the polymer and the content of lithium salts and plasticizers. Therefore, adjusting the functional group structure of the polymer to improve adsorption, or increasing the content of lithium salts / plasticizers, can improve ionic conductivity to a certain extent. However, the regulation of polymer structure and the content of transmission media such as lithium salts to improve ionic conductivity are often accompanied by changes in the interaction / side reactions between molecules inside the polymer and the side reactions on the surface of the negative electrode, and the chemical reaction process between the polymer and the negative electrode surface will also affect its stability. Therefore, while regulating the ionic conductivity of the polymer, it is often necessary to take into account the regulation of its stability.

[0004] Polyvinylidene fluoride (PVDF) is a polymer that contains a large number of -H and -F sites. + In the process, Li +It is very easy to come into contact with -H and -F, which causes PVDF to undergo dehydrogenation and defluorination reactions, producing HF and LiF as side reaction products, which reduces the stability of PVDF. At the same time, HF will corrode the lithium negative electrode, reducing the stability of the lithium negative electrode. Therefore, in order to improve the ionic conductivity of PVDF while avoiding the reduction of its structural stability, it is necessary to consider Li + Contact with -H and -F sites during the transmission process, try to find a way to transfer Li + While avoiding Li + The material in contact with -H and -F achieves the effect of taking into account both the ionic conductivity and stability of PVDF. Summary of the invention

[0005] In view of the above-mentioned problems existing in the existing PVDF, the present invention provides a method for preparing a zwitterion-modified PVDF polymer electrolyte, which adopts propane pyridinium sulfonate (PPS) as a PVDF electrolyte additive to promote ion transport while taking into account the stability of PVDF and the lithium negative electrode, inhibiting the dehydrogenation and defluorination side reactions, and improving the stability of the lithium negative electrode and the performance and cycle stability of the PESSE-based LMB battery.

[0006] In order to achieve the above purpose, the technical method adopted by the present invention is as follows:

[0007] A method for preparing a zwitterion-modified PVDF polymer electrolyte, the specific process is:

[0008] PVDF particles, lithium salt, PPS and polar organic solvent are mixed and stirred to obtain a uniform viscous solution, the uniform viscous solution is coated on the surface of the substrate, and after vacuum drying, a zwitterion-modified PVDF polymer electrolyte is obtained;

[0009] The concentrations of PVDF particles, lithium salt and PPS in the uniform viscous solution are 80-120 g / L, 10-120 g / L and 5-60 g / L, respectively.

[0010] Furthermore, the lithium salt is lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiFSI) or lithium hexafluorophosphate (LiPF 6 ).

[0011] Furthermore, the polar organic solvent is N-methylpyrrolidone (NMP), N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO) or tetrahydrofuran (THF).

[0012] Furthermore, the stirring temperature is room temperature, and the stirring time is 12 to 36 hours.

[0013] Furthermore, the thickness of the uniform viscous solution on the surface of the substrate is 500-1000 μm.

[0014] Furthermore, the vacuum drying is carried out at a temperature of 60 to 80° C. and for a period of 24 to 48 hours.

[0015] The invention also proposes the application of the obtained zwitterion-modified PVDF polymer electrolyte in a quasi-solid-state lithium metal battery.

[0016] Furthermore, the quasi-solid-state lithium metal battery is a lithium symmetric button cell, a lithium-ternary (NCM) full cell, a lithium-lithium iron phosphate (LFP) full cell, etc.

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] 1. The present invention proposes a method for preparing a zwitterion-modified PVDF polymer electrolyte, using PPS as a PVDF electrolyte additive to promote ion transport while taking into account the stability of PVDF and lithium negative electrodes, inhibiting the dehydrogenation and defluorination side reactions, and improving the stability of the lithium negative electrode and the performance and cycle stability of the PESSE-based LMB battery;

[0019] 2. Specifically, PPS contains N + and SO 3 - sites, which can be used as amphoteric adsorption sites to TFSI - and Li + Adsorbed, becoming a transport site for LiTFSI, increasing Li + The transfer efficiency is improved, while avoiding the contact and reaction between LiTFSI and the -H / F sites of PVDF, thereby inhibiting the dehydrogenation and defluorination of PVDF, improving the stability of PVDF, reducing the generation of HF side reaction products, and thus reducing the corrosion of the lithium negative electrode, and comprehensively improving the stability of the lithium negative electrode, PVDF and the battery;

[0020] 3. When the zwitterion-modified PVDF polymer electrolyte obtained in the present invention is applied to lithium symmetric button cells, a 0.2 mA cm -2 , 0.1mAh cm -2 The cycle stability can reach 1000 h under low temperature and 1.5 mg cm-2 can be achieved when applied to lithium-ternary button cells. -2 NCM811 has a cycling stability of 145 cycles under load and 0.2C current; when used in lithium-iron phosphate button batteries, it can achieve 1C and 1.5mg cm -2 Cycle 500 times stably under load. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0022] Figure 1 The SEM (scanning electron microscope) microscopic morphology structures of the PVDF polymer electrolyte membranes obtained in Example 1 and Comparative Example 1; wherein (a) and (b) are the morphology structures of Comparative Example 1, and (c) and (d) are the morphology structures of Example 1;

[0023] Figure 2 The XRD (X-ray diffraction) patterns of the PVDF polymer electrolyte membranes obtained in Example 1 and Comparative Example 1;

[0024] Figure 3 The electrochemical impedance spectra of lithium-lithium symmetrical batteries assembled using the PVDF polymer electrolyte membranes obtained in Example 1 and Comparative Example 1; wherein (a) is Comparative Example 1, and (b) is Example 1;

[0025] Figure 4 The electrochemical stability linear scanning voltammetry (LSV) curve of the lithium-stainless steel battery assembled with the PVDF polymer electrolyte membrane obtained in Example 1 and Comparative Example 1;

[0026] Figure 5 The lithium-lithium symmetrical battery assembled with the PVDF polymer electrolyte membrane obtained in Example 1 and Comparative Example 1 is 0.1-1 mA cm -2 The rate cycle curve below;

[0027] Figure 6 The lithium-lithium symmetrical battery assembled with the PVDF polymer electrolyte membrane obtained in Example 1 and Comparative Example 1 was -2 , 0.1mAh cm -2 The long cycle curve below;

[0028] Figure 7 The lithium-ternary full battery assembled with the PVDF polymer electrolyte membrane obtained in Example 1 and Comparative Example 1 was tested at 0.2C and 1.5 mg cm -2 Long cycle curve under load.

[0029] Figure 8 The lithium-lithium iron phosphate full battery assembled with the PVDF polymer electrolyte membrane obtained in Example 1 and Comparative Example 1 was tested at 1C and 1.5 mg cm -2 Long cycle curve under load. DETAILED DESCRIPTION

[0030] In order to further understand the present invention, the preferred embodiments of the present invention are described below in conjunction with the examples, but it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the invention. All raw materials of the present invention are not particularly limited in their sources, and can be purchased on the market or prepared according to conventional methods well known to those skilled in the art.

[0031] Example 1

[0032] This embodiment proposes a method for preparing a zwitterion-modified PVDF polymer electrolyte, and the specific process is as follows:

[0033] Powdered PVDF particles, LiTFSI, PPS and NMP solvent were mixed and stirred at room temperature for 24 hours to form a uniform viscous solution. The uniform viscous solution was then coated on a glass plate with a 750 μm thick scraper and vacuum dried at 60°C for 24 hours to obtain a zwitterion-modified PVDF polymer electrolyte membrane, which was stored in an Ar gas atmosphere glove box for use. The concentrations of PVDF particles, LiTFSI and PPS in the uniform viscous solution were 100 g / L, 70 g / L and 30 g / L, respectively.

[0034] Example 2

[0035] This embodiment proposes a method for preparing a zwitterion-modified PVDF polymer electrolyte, and the specific process is as follows:

[0036] Powdered PVDF particles, LiTFSI, PPS and NMP solvent were mixed, stirred and reacted at room temperature for 24 hours to form a uniform viscous solution, and then the uniform viscous solution was scraped on a glass plate with a 1000 μm thick scraper and vacuum dried at 60°C for 24 hours to obtain a zwitterion-modified PVDF polymer electrolyte membrane, which was stored in an Ar gas atmosphere glove box for use; wherein the concentrations of PVDF particles, LiTFSI and PPS in the uniform viscous solution were 100 g / L, 70 g / L and 5 g / L, respectively.

[0037] Example 3

[0038] This embodiment proposes a method for preparing a zwitterion-modified PVDF polymer electrolyte, and the specific process is as follows:

[0039] Powdered PVDF particles, LiTFSI, PPS and NMP solvent were mixed and stirred at room temperature for 24 hours to form a uniform viscous solution. The uniform viscous solution was then coated on a glass plate with a 500 μm thick scraper and vacuum dried at 60°C for 24 hours to obtain a zwitterion-modified PVDF polymer electrolyte membrane, which was stored in an Ar gas atmosphere glove box for later use. The concentrations of PVDF particles, LiTFSI and PPS in the uniform viscous solution were 100 g / L, 70 g / L and 60 g / L, respectively.

[0040] Example 4

[0041] This embodiment proposes a method for preparing a zwitterion-modified PVDF polymer electrolyte, and the specific process is as follows:

[0042] Powdered PVDF particles, LiFSI, PPS and NMP solvent were mixed and stirred at room temperature for 24 hours to form a uniform viscous solution. The uniform viscous solution was then coated on a glass plate with a 500 μm thick scraper and vacuum dried at 60°C for 24 hours to obtain a zwitterion-modified PVDF polymer electrolyte membrane, which was stored in an Ar gas atmosphere glove box for later use. The concentrations of PVDF particles, LiFSI and PPS in the uniform viscous solution were 120 g / L, 120 g / L and 60 g / L, respectively.

[0043] Example 5

[0044] This embodiment proposes a method for preparing a zwitterion-modified PVDF polymer electrolyte, and the specific process is as follows:

[0045] Powdered PVDF particles, LiPF 6 , PPS and NMP solvent were mixed, stirred and reacted at room temperature for 24 hours to form a uniform viscous solution, and then the uniform viscous solution was scraped on a glass plate with a 500 μm thick scraper, and vacuum dried at 60 ° C for 24 hours to obtain a zwitterion-modified PVDF polymer electrolyte membrane, which was stored in an Ar gas atmosphere glove box for standby use; wherein, PVDF particles, LiPF 6 The concentrations of PEG and PPS were 80 g / L, 30 g / L and 60 g / L, respectively.

[0046] Comparative Example 1

[0047] This comparative example proposes a method for preparing an unmodified PVDF polymer electrolyte, and the specific process is as follows:

[0048] Powdered PVDF particles, LiTFSI and NMP solvent were mixed, stirred and reacted at room temperature for 24 hours to form a uniform viscous solution, and then the uniform viscous solution was scraped on a glass plate with a 750 μm thick scraper and vacuum dried at 60°C for 24 hours to obtain an unmodified PVDF polymer electrolyte membrane, which was stored in an Ar gas atmosphere glove box for use; wherein the concentrations of PVDF particles and LiTFSI in the uniform viscous solution were 100 g / L and 70 g / L, respectively.

[0049] The characterization and performance of the zwitterion-modified PVDF polymer electrolyte membrane obtained in Example 1 and the unmodified PVDF polymer electrolyte membrane obtained in Comparative Example 1 are compared and analyzed below.

[0050] Figure 1 The SEM microstructures of the PVDF polymer electrolyte membranes obtained in Example 1 and Comparative Example 1 are shown in FIG. Figure 1 (a) and Figure 1 (b) is the morphology structure of Comparative Example 1, Figure 1 (c) and Figure 1 (d) is the morphology structure of Example 1. It can be seen that the morphology of both films is regular and flat, indicating that PPS modification has little effect on the morphology of the PVDF polymer membrane.

[0051] Figure 2 The XRD patterns of the PVDF polymer electrolyte membranes obtained in Example 1 and Comparative Example 1 are compared with the XRD patterns of pure PVDF powder. The sharp peak and the bun peak at around 20° are respectively attributed to the

[110] and

[020] crystal planes of PVDF, and the bun peak at around 39° is attributed to the γ-phase PVDF. It can be seen that the addition of PPS will increase the overall crystallinity of the PVDF polymer membrane to a certain extent without affecting the original PVDF structure, indicating that the introduction of the bipolar PPS molecules inside the PVDF polymer will enhance the dipole interaction.

[0052] Figure 3 The electrochemical impedance spectra of lithium-lithium symmetrical batteries assembled using the PVDF polymer electrolyte membranes obtained in Example 1 and Comparative Example 1 are shown in FIG. Figure 3 (a) is that of Comparative Example 1, Figure 3 (b) is that of Example 1; specifically, the impedance spectrum of the ionic conductivity of the PVDF polymer electrolyte membrane is calculated by the electrochemical test results of the lithium-lithium symmetrical battery, and the formula is σ=d / (R×S) (wherein, σ is the ionic conductivity; d is the thickness of the PVDF polymer electrolyte membrane, where the thickness of Comparative Example 1 is 40 μm, and the thickness of Example 1 is 88 μm; R is the impedance value, specifically the value of the intersection of the dotted curve and the abscissa in the figure; S is the area of ​​the PVDF polymer electrolyte membrane, where it is 1.12 cm 2 ).according to Figure 3 The ionic conductivity of Comparative Example 1 and Example 1 is 0.21 mS cm -1 、0.49mS cm -1 This indicates that PPS promotes the Li + transport, that is, improving ionic conductivity.

[0053] Figure 4 The electrochemical stability linear scanning LSV curve of the lithium-stainless steel battery assembled with the PVDF polymer electrolyte membrane obtained in Example 1 and Comparative Example 1 is shown. Specifically, the voltage threshold at which the current changes with the voltage and the value begins to increase sharply is used to obtain the withstand voltage of the polymer membrane, i.e., the electrochemical stability. Figure 4 The electrochemical stability windows of Comparative Example 1 and Example 1 are 4.2 V and 4.8 V, respectively, indicating that PPS avoids Li + The contact with the -H and -F sites of PVDF inhibits the occurrence of dehydrogenation and defluorination side reactions and improves the stability of the polymer structure and the lithium negative electrode interface.

[0054] Figure 5 The lithium-lithium symmetrical battery assembled with the PVDF polymer electrolyte membrane obtained in Example 1 and Comparative Example 1 is 0.1-1 mA cm -2 From the rate cycle curve under , it can be seen that the withstand current of Example 1 is significantly improved, and the overpotential value is small, and the overpotential jitter and attenuation phenomenon at high current that exist in Comparative Example 1 will not occur, indicating that PPS can improve the test withstand current density and rate performance of lithium-lithium symmetric batteries by improving ionic conductivity and stability.

[0055] Figure 6 The lithium-lithium symmetrical battery assembled with the PVDF polymer electrolyte membrane obtained in Example 1 and Comparative Example 1 was -2 , 0.1mAh cm -2 From the long cycle curve below, it can be seen that Example 1 can stably cycle for 1000h, while Comparative Example 1 has an obvious short circuit phenomenon at around 138h. This is because the stability and ionic conductivity of the polymer electrolyte are poor, resulting in excessive interface polarization, a thick dead lithium layer, and severe growth of dendrites, which eventually pierce the electrolyte. This shows that PPS can improve the stability of the battery, thereby improving the cycle performance of the battery.

[0056] Figure 7 The lithium-ternary full battery assembled with the PVDF polymer electrolyte membrane obtained in Example 1 and Comparative Example 1 was tested at 0.2C and 1.5 mg cm -2From the long cycle curve under load, it can be seen that Example 1 can stably cycle for 145 cycles, while the capacity decay rate of Comparative Example 1 is relatively high after the start of the cycle, and the capacity retention after dozens of cycles is less than half of the first cycle, which further illustrates that PPS modification can significantly improve the cycle performance of the battery by improving ionic conductivity and polymer stability.

[0057] Figure 8 The lithium-lithium iron phosphate full battery assembled with the PVDF polymer electrolyte membrane obtained in Example 1 and Comparative Example 1 was tested at 1C and 1.5 mg cm -2 From the long cycle curve under load, it can be seen that Example 1 can stably cycle for 500 cycles, while the capacity attenuation rate of each cycle of Comparative Example 1 is relatively high since the beginning of the cycle, and the battery capacity drops sharply after less than fifty cycles, further illustrating that PPS modification can improve the cycle performance of lithium metal batteries.

[0058] The present invention uses specific examples to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core ideas, including the best mode, and also enables any technician in the field to practice the present invention, including making and using any device or system, and implementing any combined method. It should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, the present invention can also be improved and modified, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements that are not different from the text of the claims, or if they include equivalent structural elements that are not substantially different from the text of the claims, then these other embodiments should also be included in the scope of the claims.

Claims

1. A method for preparing a zwitterion-modified PVDF polymer electrolyte, characterized in that: The specific process is: PVDF particles, lithium salt, PPS and polar organic solvent are mixed and stirred to obtain a uniform viscous solution, which is coated on the surface of a substrate and vacuum dried to obtain a zwitterion-modified PVDF polymer electrolyte; The concentrations of PVDF particles, lithium salt and PPS in the uniform viscous solution are 80-120 g / L, 10-120 g / L and 5-60 g / L, respectively.

2. The method for preparing the zwitterion-modified PVDF polymer electrolyte according to claim 1, characterized in that: The lithium salt is lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate or lithium hexafluorophosphate.

3. The method for preparing the zwitterion-modified PVDF polymer electrolyte according to claim 1, characterized in that: The polar organic solvent is N-methylpyrrolidone, N,N-dimethylformamide, dimethyl sulfoxide or tetrahydrofuran.

4. The method for preparing the zwitterion-modified PVDF polymer electrolyte according to claim 1, characterized in that: The thickness of the uniform viscous solution on the surface of the substrate is 500-1000 μm.

5. The method for preparing the zwitterion-modified PVDF polymer electrolyte according to claim 1, characterized in that: The temperature of the vacuum drying is 60-80° C. and the duration is 24-48 hours.

6. Use of the zwitterion-modified PVDF polymer electrolyte obtained according to the preparation method according to any one of claims 1 to 5 in quasi-solid-state lithium metal batteries.

Citation Information

Patent Citations

  • Electrolyte containing 3-(1-Pyridinio)-1-propanesulfonate and battery using electrolyte

    CN106099183A

  • Preparation method of low-temperature flexible polymer solid electrolyte membrane and application of electrolyte membrane to low-temperature solid lithium ion battery

    CN109411809A

  • Gel polymer electrolyte with heterostructure and quasi-solid-state lithium metal battery

    CN114335708A

  • Solid polymer electrolyte and preparation method and application thereof

    CN116315119A

  • Lithium ion battery non-aqueous electrolyte additive capable of reducing internal resistance of battery and application of lithium ion battery non-aqueous electrolyte additive

    CN116646603A

Cited By

  • Composite positive electrode material and preparation method and application thereof

    CN121123238A