Preparation and application of ethylene glycol diester additive

By using ethylene glycol-based diester additives in lithium-ion batteries to form an interface film of moderate thickness, the problem of reduced battery discharge capacity of lithium-ion batteries at low temperatures is solved, high-temperature circulation and storage performance are improved, and internal battery Obstacle.

CN119009117APending Publication Date: 2024-11-22ZHEJIANG LANTIAN ENVIRONMENTAL PROTECTION HI TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310603735.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-22
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The problem of the reduction of battery discharge capacity of existing lithium-ion batteries in low temperature environments. The chemical film formed by existing film-forming additives at high temperatures has strong ion resistance, affecting battery performance.

Method used

The additive is synthesized by a specific preparation method using an ethylene glycol-based diester additive containing a sulfate and carbonate group, and used in lithium-ion battery electrolyte to form an interface film of moderate thickness, reducing electrodes and Resistance between electrolytes.

Benefits of technology

It improves high-temperature circulation and storage performance, while also having low-temperature performance, maintains battery capacity at low temperatures, suppresses the growth of battery internal resistance, and improves the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009117A_ABST
    Figure CN119009117A_ABST
Patent Text Reader

Abstract

The invention discloses an ethylene glycol diester additive for a battery electrolyte, the structure of the ethylene glycol diester additive is as shown in the following formula (I): in the # imgabs0 # formula, R1 and R2 are independently selected from C1-C6 alkyl, C1-C6 halogenated alkyl, C2-C6 alkenyl, C2-C6 halogenated alkenyl, aryl or halogenated aryl. The ethylene glycol diester additive disclosed by the invention has low-temperature performance while improving the high-temperature circulating storage performance, and can keep the battery capacity at low temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a lithium ion battery electrolyte, and in particular to the preparation of a new ethylene glycol-based diester additive and its application in a lithium ion battery electrolyte. Background Art

[0002] With the rapid development of new energy vehicles, people have put forward higher requirements for the cycle life, battery capacity, battery performance in high and low temperature weather, and safety of lithium-ion batteries. In order to improve the electrochemical performance of the battery, different film-forming additives are usually added to the electrolyte to form a dense and stable chemical film on the electrode surface through the film-forming additives, thereby reducing the side reactions between the electrode and the electrolyte, slowing down the aging of the battery and extending the battery life.

[0003] Cyclic sulfate or sulfonate is a commonly used film-forming additive in lithium-ion batteries, which can improve the cycle life of the battery and the stability under high temperature and high voltage. However, because the chemical film is not a perfect ion channel but has a certain resistance, and the chemical film formed after adding cyclic sulfate or sulfonate is thicker, the resistance to ions is stronger. At room temperature or high temperature, lithium ions have enough energy to overcome the resistance, so the impact on battery performance is not obvious; however, at low temperature, the resistance caused by the chemical film cannot be ignored, which will lead to a decrease in the discharge capacity of the battery.

[0004] Patent CN103107355A of Ningde New Energy Technology Co., Ltd. discloses a lithium-ion battery and its electrolyte, which uses unbranched cyclic sulfate and branched cyclic sulfate as additives. This combination of additives can slightly reduce the problem of increased battery internal resistance caused by using cyclic sulfate alone while ensuring high-temperature cycle performance, but the effect is not obvious.

[0005] Therefore, it is of great practical significance to develop an electrolyte additive that improves high-temperature cycle storage performance while also having low-temperature performance. Summary of the invention

[0006] In order to solve the above technical problems, the present invention proposes an ethylene glycol-based diester additive that improves high-temperature cycle and storage performance while also having low-temperature performance, and a preparation method and application thereof.

[0007] The objective of the present invention is achieved through the following technical solutions:

[0008] An ethylene glycol-based diester additive for battery electrolyte, the structure of which is shown in the following formula (I):

[0009]

[0010] In the formula, R1 and R2 are independently selected from C1-C6 alkyl, C1-C6 haloalkyl, C2-C6 alkenyl, C2-C6 haloalkenyl, aryl or halogenated aryl; preferably, R1 and R2 are independently selected from C1-C3 alkyl, C1-C3 haloalkyl, C2-C3 alkenyl or C2-C3 haloalkenyl; further preferably, R1 and R2 are independently selected from methyl, ethyl, fluoromethyl or fluoroethyl. More preferably, R1 and R2 are independently selected from methyl or ethyl.

[0011] The ethylene glycol diester additive of the present invention contains both sulfate groups and carbonate groups, so that it improves high-temperature cycle and storage performance while also having low-temperature performance.

[0012] The present invention also provides a method for preparing any of the above-mentioned ethylene glycol-based diester additives, the preparation method comprising:

[0013] (1) A step of reacting chloroformate and ethylene glycol to obtain an alkyl hydroxyethyl carbonate intermediate, wherein the reaction formula is as follows:

[0014]

[0015] (2) The step of reacting an alkyl hydroxyethyl carbonate intermediate with a chlorosulfonate to obtain an ethylene glycol diester additive, wherein the reaction formula is as follows:

[0016]

[0017] In the formula, R1 and R2 have the same definitions as above.

[0018] In step (1), the molar ratio of chloroformate to ethylene glycol is (0.2-2):1, and in order to completely react the chloroformate and reduce the formation of the by-product ethylene glycol carbonate diester, it is preferably (0.6-1):1;

[0019] In step (2), the molar ratio of the alkyl hydroxyethyl carbonate intermediate to the chlorosulfonate is (0.2-2):1, and in order to allow the alkyl hydroxyethyl carbonate intermediate to react completely, it is preferably (0.5-1.5):1.

[0020] In step (1), the reaction temperature is 5 to 60°C, and the reaction time is 0.2 to 24 hours; preferably, the reaction temperature is 20 to 45°C, and the reaction time is 1 to 6 hours;

[0021] In step (2), the reaction temperature is 5 to 60° C., and the reaction time is 0.2 to 24 h; preferably, the reaction temperature is 20 to 45° C., and the reaction time is 1 to 6 h.

[0022] Specifically, the preparation method comprises the following steps:

[0023] S1. reacting chloroformate and ethylene glycol in a reaction vessel to obtain an alkyl hydroxyethyl carbonate intermediate reaction solution, and removing the residual ethylene glycol in the reaction solution by atmospheric distillation or reduced pressure distillation;

[0024] S2. Continue to add chlorosulfonate to the reaction vessel to obtain a glycol diester reaction solution;

[0025] S3. Using atmospheric distillation or reduced pressure distillation to remove the residual chlorosulfonate and alkyl hydroxyethyl carbonate intermediates in the reaction solution to obtain an ethylene glycol diester additive having a structure shown in formula (I).

[0026] In step S1, the distillation temperature of atmospheric distillation or reduced pressure distillation is 100-200°C, and the distillation time is 0.1-5h; preferably, the distillation temperature is 130-170°C, and the preferred reaction time is 0.1-1h;

[0027] In step S3, the distillation temperature of atmospheric distillation or reduced pressure distillation is 150-250°C, and the distillation time is 0.1-5h; preferably, the distillation temperature is 170-210°C, and the preferred reaction time is 0.1-1h;

[0028] The present invention also provides the use of any of the above-mentioned ethylene glycol diester additives, wherein the ethylene glycol diester additive is used in lithium secondary battery electrolyte, and the addition amount accounts for 0.01-10% of the total mass of the electrolyte, preferably the addition amount accounts for 0.1-5.0% of the total mass of the electrolyte, and more preferably the addition amount accounts for 0.5-3.0% of the total mass of the electrolyte. After the ethylene glycol diester additive is used in the lithium secondary battery electrolyte, it can effectively form a film at the positive electrode, inhibit the oxidation of the electrolyte at the positive electrode, and improve the high temperature performance of the battery; it can also effectively form a film at the negative electrode, and the thickness of the interface film formed is moderate, thinner than that of cyclic sulfate or sulfonate, which can improve the problem of increasing the internal resistance of the battery when using cyclic sulfate or sulfonate.

[0029] The ethylene glycol diester additive of the present invention can be combined with cyclic sulfate and / or sulfonate for lithium secondary battery electrolyte, the amount of ethylene glycol diester additive added is 0.01-10% of the total mass of the electrolyte, and the amount of cyclic sulfate or sulfonate added is 0.01-10% of the total mass of the electrolyte; preferably, the amount of ethylene glycol diester additive added is 0.1-5.0% of the total mass of the electrolyte, and the amount of cyclic sulfate or sulfonate added is 0.1-5.0% of the total mass of the electrolyte; more preferably, the amount of ethylene glycol diester additive added is 0.5-3.0% of the total mass of the electrolyte, and the amount of cyclic sulfate or sulfonate added is 0.5-3.0% of the total mass of the electrolyte.

[0030] After the ethylene glycol diester additive and the cyclic sulfate or sulfonate additive are used together, the ethylene glycol diester additive and the cyclic sulfate or sulfonate additive jointly participate in the chemical film formation process on the negative electrode surface. The two ions containing -O-SO2- or -O-SO2-O- groups have diverse structures when participating in film formation and can form a cross-shaped and network structure. Compared with the chemical film formed by adding cyclic sulfate or sulfonate alone, it is more fluffy and contains more ion holes.

[0031] The cyclic sulfate and / or sulfonate is selected from at least one of vinyl sulfate, propylene sulfate, 1,3-propane sultone and 1,4-butane sultone.

[0032] The present invention also provides a lithium-ion secondary battery, comprising a positive electrode, a negative electrode, a separator and an electrolyte, in particular, the electrolyte comprises any of the above-mentioned ethylene glycol-based diester additives, or the electrolyte comprises a combination of any of the above-mentioned ethylene glycol-based diester additives and any of the above-mentioned cyclic sulfates and / or sulfonates.

[0033] The active material of the positive electrode is selected from a nickel-cobalt-manganese ternary material, a nickel-cobalt-aluminum ternary material, a lithium cobalt oxide material, or a lithium iron phosphate material; wherein the nickel-cobalt-manganese ternary material is Li(Ni x Co y Mn z )O2, x≥0.5, y>0, z>0, x+y+z=1; the nickel-cobalt-aluminum ternary material is Li(Ni)O2, x≥0.8, y>0, z>0, x+y+z=1.

[0034] The active material of the negative electrode is graphite, silicon dioxide, silicon, metallic lithium or a composite material thereof.

[0035] The separator is selected from separators commonly used in lithium-ion batteries.

[0036] The electrolyte also includes a main lithium salt and a non-aqueous solvent;

[0037] The main lithium salt is selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(fluorosulfonyl)imide and lithium bis(trifluoromethylsulfonyl)imide, and its molar concentration is 0.1 to 4.0 mol / L, more preferably 0.8 to 1.5 mol / L.

[0038] The non-aqueous solvent can be an organic solvent commonly used in electrolytes. Preferably, the organic solvent is selected from at least one of ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, γ-butyrolactone, methyl acetate, methyl propionate, methyl butyrate, ethyl acetate, ethyl propionate, ethyl butyrate, propyl acetate, propyl propionate, sulfolane, dimethyl sulfoxide, dimethyl sulfone, diethyl sulfone, triethylene glycol dimethyl ether or tetraethylene glycol dimethyl ether.

[0039] Compared with the prior art, the present invention has the following beneficial effects:

[0040] The ethylene glycol-based diester additive of the present invention contains both sulfate and carbonate groups, so that it improves high-temperature cycle and storage performance while also having low-temperature performance, thereby maintaining battery capacity at low temperatures. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 This is the GC-MS spectrum of the ethylene glycol diester additive prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0042] The present invention is further described below in conjunction with specific embodiments, but the present invention is not limited to these specific embodiments. Those skilled in the art should recognize that the present invention covers all possible alternatives, improvements and equivalents within the scope of the claims.

[0043] Example 1

[0044] This embodiment provides a method for preparing an ethylene glycol-based diester additive, which specifically comprises the following steps:

[0045] S1. In a dry room with a dew point of -40°C, add 1 mol of ethylene glycol to the reaction flask and start stirring; then add 0.8 mol of methyl chloroformate to the reaction flask and react at 50°C for 1 hour; remove the residual unreacted ethylene glycol in the reaction solution by vacuum distillation at a distillation temperature of 150°C for 0.5 hours;

[0046] S2. After distillation, 0.8 mol of methyl chlorosulfonate was added to the reaction flask and reacted at 50 ° C for 1 h to obtain a glycol diester reaction solution;

[0047] S3. The residual methyl chlorosulfonate and methyl hydroxyethyl carbonate intermediates in the reaction solution were removed by vacuum distillation at a temperature of 180° C. for 0.5 h to obtain an ethylene glycol methyl sulfate methyl carbonate additive, which was recorded as additive #1.

[0048] Attached Figure 1 The GC-MS spectrum of additive #1 is given, and the instrument method is as follows: injection port temperature: 280°C; carrier gas: helium, flow rate 1mL / min; column temperature: program temperature rise, 40°C for 5min, and then rise to 230°C at 10°C / min; detector: MSD; ionization mode: electron impact ionization (EI), ionization energy 70eV; scanning mode: full scan. Through spectrum analysis, it is confirmed that additive #1 is ethylene glycol methyl sulfate methyl carbonate, and the purity of additive #1 is calculated to be about 92.7%.

[0049] Example 2

[0050] The operation of this embodiment is the same as that of Embodiment 1, except that: in step S1, methyl chloroformate is replaced by ethyl chloroformate, and the amount used remains unchanged; in step S2, methyl chlorosulfonate is replaced by ethyl chlorosulfonate, and the obtained additive is recorded as 2# additive.

[0051] The GC-MS spectrum confirmed that the 2# additive was ethylene glycol ethyl sulfate ethyl carbonate, and the purity of the 2# additive was calculated to be about 85.1%.

[0052] Example 3

[0053] The operation of this embodiment is the same as that of Embodiment 1, except that the content of methyl chloroformate added in step S1 is increased to 1.2 mol, and the obtained additive is recorded as additive #3.

[0054] The GC-MS spectrum confirmed that the 3# additive was ethylene glycol methyl sulfate methyl carbonate, and the purity of the 3# additive was calculated to be about 71.3%, and the main impurity was ethylene glycol dimethyl carbonate.

[0055] Example 4

[0056] The operation of this embodiment is the same as that of Embodiment 1, except that the content of methyl chlorosulfonate added in step S2 is increased to 1.2 mol, and other operations remain unchanged. The obtained additive is recorded as 4# additive.

[0057] The GC-MS spectrum confirmed that the 4# additive was ethylene glycol methyl sulfate methyl carbonate, and the purity of the 4# additive was calculated to be about 72.5%, and the main impurity was ethylene glycol dimethyl sulfate.

[0058] Example 5

[0059] The operation of this embodiment is the same as that of Embodiment 1, except that the content of methyl chlorosulfonate added in step S2 is reduced to 0.5 mol, and other operations remain unchanged. The obtained additive is recorded as 5# additive.

[0060] The GC-MS spectrum confirmed that the 5# additive was ethylene glycol methyl sulfate methyl carbonate, and the purity of the 5# additive was calculated to be about 84.8%.

[0061] Example 6

[0062] The operation of this embodiment is the same as that of Embodiment 1, except that the distillation temperature in step S1 is lowered to 130° C., and other operations remain unchanged. The obtained additive is recorded as additive #6.

[0063] The GC-MS spectrum confirmed that the 6# additive was ethylene glycol methyl sulfate methyl carbonate, and the purity of the 6# additive was calculated to be about 70.1%. The reduction in distillation temperature made it impossible to completely remove ethylene glycol from the reaction solution, resulting in the generation of a variety of by-products, which had a significant impact on the purity of the product.

[0064] Example 7

[0065] The operation of this embodiment is the same as that of Embodiment 1, except that the distillation temperature in step S1 is increased to 170° C., and other operations remain unchanged. The obtained additive is recorded as additive #7.

[0066] The GC-MS spectrum confirmed that the 7# additive was ethylene glycol methyl sulfate methyl carbonate, and the purity of the 7# additive was calculated to be about 90.3%.

[0067] Application Example 1

[0068] This application example provides the preparation of an electrolyte.

[0069] In a glove box filled with argon (water content <5ppm, oxygen content <10ppm), ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were uniformly mixed at a mass ratio of EC:EMC:DEC=3:5:2, and lithium hexafluorophosphate (LiPF6) was slowly added to the mixed solution until the molar concentration of LiPF6 was 1.2mol / L to obtain a basic electrolyte. Ethylene glycol methyl sulfate methyl carbonate (1# additive) was slowly added to the basic electrolyte until the mass fraction was 1.0%, and the electrolyte of this application example was obtained.

[0070] Application Example 2

[0071] The operation of this application example is the same as that of application example 1, except that ethylene glycol methyl sulfate methyl carbonate (additive #1) is slowly added to the base electrolyte to a mass fraction of 0.5% to obtain the electrolyte of this application example.

[0072] Application Example 3

[0073] The operation of this application example is the same as that of application example 1, except that ethylene glycol methyl sulfate methyl carbonate (additive #1) is slowly added to the base electrolyte to a mass fraction of 2.0% to obtain the electrolyte of this application example.

[0074] Application Example 4

[0075] The operation of this application example is the same as that of application example 1, except that ethylene glycol methyl sulfate methyl carbonate (additive #1) is slowly added to the base electrolyte to a mass fraction of 3.0% to obtain the electrolyte of this application example.

[0076] Application Example 5

[0077] The operation of this application example is the same as that of application example 1, except that ethylene glycol ethyl sulfate ethyl carbonate (additive #2) is slowly added to the base electrolyte to a mass fraction of 1.0% to obtain the electrolyte of this application example.

[0078] Application Example 6

[0079] The operation of this application example is the same as that of application example 1, except that ethylene glycol ethyl sulfate ethyl carbonate (additive #2) is slowly added to the base electrolyte to a mass fraction of 2.0% to obtain the electrolyte of this application example.

[0080] Application Example 7

[0081] The operation of this application example is the same as that of application example 1, except that ethylene glycol ethyl sulfate ethyl carbonate (additive #2) is slowly added to the base electrolyte to a mass fraction of 3.0% to obtain the electrolyte of this application example.

[0082] Application Example 8

[0083] The operation of this application example is the same as that of application example 1, with the only difference being that, on the basis of application example 1, 1.0% diethyl sulfate (DTD) is added to obtain the electrolyte of this application example.

[0084] Application Example 9

[0085] The operation of this application example is the same as that of application example 1, except that: on the basis of application example 1, 1.0% of 1,3-propane sultone (PS) is added to obtain the electrolyte of this application example.

[0086] Comparative application example 1

[0087] The electrolyte of this comparative application example adopts the basic electrolyte in Application Example 1 without adding the ethylene glycol-based diester additive.

[0088] Comparative Application Example 2

[0089] The operation of this comparative application example is the same as that of application example 1, with the only difference being that ethylene glycol methyl sulfate methyl carbonate is replaced with diethylene sulfate (DTD) to obtain the electrolyte of this comparative application example.

[0090] Comparative Application Example 3

[0091] The operation of this comparative application example is the same as that of application example 1, except that ethylene glycol methyl sulfate methyl carbonate is replaced with 1,3-propane sultone (PS) to obtain the electrolyte of this comparative application example.

[0092] The electrolytes of the above-mentioned embodiments and comparative examples are respectively made into soft-pack lithium-ion batteries with a capacity of 1260 mAh, wherein the lithium-ion batteries include a positive electrode sheet, a negative electrode sheet, a separator, an electrolyte, and battery auxiliary materials, wherein the positive electrode active material is a nickel-cobalt-manganese ternary material, and the negative electrode active material is a graphite-silicon mixture. The preparation process is as follows: the positive electrode sheet, the separator, and the negative electrode sheet are wound together into a winding core, sealed with an aluminum-plastic film, and then baked so that the electrode moisture meets the requirements, and the battery cell is injected with electrolyte after baking, and the finished soft-pack battery cell is obtained through the processes of standing, forming, volume separation, and aging.

[0093] The prepared lithium-ion power battery (soft-pack battery cell) was subjected to performance testing. The specific test items and methods are as follows:

[0094] (1) 60°C high temperature storage test: The battery was charged to 100% SOC and stored in a 60±2°C oven for 28 days. The volume before and after storage was measured to obtain the volume expansion rate of the single battery before and after 60°C storage. The DCR value after storage was measured at room temperature, and the percentage value of the initial DCR was calculated and recorded as the discharge DCR change rate.

[0095] (2) 25°C room temperature cycle test: The battery is cycled at 25±1°C in an oven at a charge and discharge current of 1C / 1C. The discharge capacity per week is calculated. The cycle is stopped after 500 cycles, and the capacity retention rate after the cycle is calculated.

[0096] (3) -20℃ low-temperature discharge: The battery is discharged in a -20±1℃ oven at a discharge current of 1C to 80% of the lower limit voltage. The low-temperature discharge capacity is taken as the percentage of the 1C discharge capacity at 25℃, which is recorded as the low-temperature discharge capacity retention rate.

[0097] The test results are shown in Table 1 below:

[0098] Table 1 Electrochemical performance test results

[0099]

[0100] According to Table 1 above, adding ethylene glycol diester additives to the electrolyte can reduce the initial impedance of the battery and improve the low-temperature discharge performance, inhibit the gas production and impedance growth of the battery during high-temperature storage, and improve the cycle performance, thereby achieving the effect of taking into account both high and low temperature performance.

[0101] By comparing application examples 1 to 4, it can be found that the battery with 1% content of 1# additive has the best comprehensive performance. When the addition amount is higher than 1%, as the amount of additive used increases, the inhibition of high-temperature gas production continues to improve, but the internal resistance of the battery increases slightly, and the low-temperature discharge capacity decreases. The regulation of the amount of additive used is of great significance for the high and low temperature performance of the battery. The preferred use range of the additive is 0.5-2.0%.

[0102] By comparing Application Example 1 and Application Example 8, it can be found that adding 1# additive and DTD to the electrolyte at the same time can further reduce the initial impedance and improve the high temperature storage performance and cycle performance; by comparing Application Example 1 and Application Example 9, it can be found that adding 1# additive and PS to the electrolyte at the same time can not only give play to the advantage of PS in significantly inhibiting the gas production of the battery during high temperature storage, but also avoid the defect of PS in increasing the initial impedance and deteriorating the low temperature performance. Therefore, the use of the ethylene glycol-based diester additive in combination with the cyclic sulfate or sulfonate of the present invention can not only further improve the high temperature performance, but also reduce the battery impedance and improve the low temperature discharge performance of the battery, so that the battery has both high and low temperature performance.

Claims

1. An ethylene glycol diester additive for battery electrolyte, the structure of which is shown in the following formula (I): In the formula, R1 and R2 are independently selected from C1-C6 alkyl, C1-C6 haloalkyl, C2-C6 alkenyl, C2-C6 haloalkenyl, aryl or halogenated aryl.

2. The ethylene glycol-based diester additive according to claim 1, characterized in that: R1 and R2 are independently selected from C1-C3 alkyl, C1-C3 haloalkyl, C2-C3 alkenyl or C2-C3 haloalkenyl.

3. The ethylene glycol-based diester additive according to claim 2, characterized in that: R1 and R2 are independently selected from methyl, ethyl, fluoromethyl or fluoroethyl.

4. A method for preparing the ethylene glycol diester additive according to any one of claims 1 to 3, characterized in that: The preparation method comprises: (1) A step of reacting chloroformate and ethylene glycol to obtain an alkyl hydroxyethyl carbonate intermediate, wherein the reaction formula is as follows: (2) The step of reacting an alkyl hydroxyethyl carbonate intermediate with a chlorosulfonate to obtain an ethylene glycol diester additive, wherein the reaction formula is as follows: Wherein, R1 and R2 are defined as in claim 1.

5. The method for preparing the ethylene glycol-based diester additive according to claim 4, characterized in that: In step (1), the molar ratio of chloroformate to ethylene glycol is (0.2-2):1; In step (2), the molar ratio of the alkyl hydroxyethyl carbonate intermediate to the chlorosulfonate is (0.2-2):

1.

6. The method for preparing the ethylene glycol-based diester additive according to claim 4, characterized in that: In step (1), the reaction temperature is 5 to 60° C. and the reaction time is 0.2 to 24 h; In step (2), the reaction temperature is 5 to 60° C. and the reaction time is 0.2 to 24 h.

7. The method for preparing the ethylene glycol-based diester additive according to any one of claims 4 to 6, characterized in that: The preparation method comprises the following steps: S1. reacting chloroformate and ethylene glycol in a reaction vessel to obtain an alkyl hydroxyethyl carbonate intermediate reaction solution, and removing the residual ethylene glycol in the reaction solution by atmospheric distillation or reduced pressure distillation; S2. Continue to add chlorosulfonate to the reaction vessel to obtain a glycol diester reaction solution; S3. Using atmospheric distillation or reduced pressure distillation to remove the residual chlorosulfonate and alkyl hydroxyethyl carbonate intermediates in the reaction solution to obtain an ethylene glycol diester additive having a structure shown in formula (I).

8. An application of the ethylene glycol diester additive according to any one of claims 1 to 3, characterized in that: The ethylene glycol diester additive is used in lithium secondary battery electrolyte, and the added amount accounts for 0.01-10% of the total mass of the electrolyte.

9. The use of the ethylene glycol diester additive according to claim 8, characterized in that: The ethylene glycol diester additive and the cyclic sulfate and / or sulfonate are combined for lithium secondary battery electrolyte, the ethylene glycol diester additive is added in an amount of 0.1-5.0% of the total mass of the electrolyte, and the cyclic sulfate and / or sulfonate is added in an amount of 0.1-5.0% of the total mass of the electrolyte.

10. A lithium ion secondary battery comprising a positive electrode, a negative electrode, a separator and an electrolyte, characterized in that: The electrolyte comprises the ethylene glycol-based diester additive according to any one of claims 1-3.