Sodium supplement with improved decomposition efficiency and preparation method and application thereof

By recombining sodium orthosilicate with conductive carbon, reducing the decomposition voltage and improving the decomposition efficiency, the problem of low decomposition efficiency of sodium supplementary materials in sodium ion batteries is solved, and the battery performance with high energy density is achieved.

CN119009191APending Publication Date: 2024-11-22NORTHWESTERN POLYTECHNICAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411341348.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The decomposition efficiency of sodium supplementary materials in existing sodium ion batteries is low, resulting in a reduced energy density and cannot meet the needs of efficient pre-sodium.

Method used

Sodium orthosilicate is compounded with conductive carbon, mixed in an oxygen-free environment by ball milling to form a conductive network, reduce the decomposition voltage and improve the decomposition efficiency, and prepare a high specific capacity sodium supplement agent.

Benefits of technology

It effectively improves the decomposition efficiency of sodium supplementation agent, so that it irreversibly removes active sodium ions at a lower voltage, improves the energy density of the battery, and is suitable for large-scale industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009191A_ABST
    Figure CN119009191A_ABST
Patent Text Reader

Abstract

The invention discloses a sodium supplement with improved decomposition efficiency and a preparation method and application thereof, belongs to the technical field of sodium ion batteries, and solves the problem of low decomposition efficiency of a sodium supplement material in the prior art. The sodium supplementing agent with improved decomposition efficiency provided by the invention comprises conductive carbon and sodium orthosilicate in a mass ratio of 1: (2-10). The sodium orthosilicate and the conductive carbon are compounded, so that the decomposition voltage of the sodium orthosilicate is reduced, and the sodium orthosilicate, which is a sodium-rich material with high specific capacity, can be effectively applied to the field of sodium pre-treatment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sodium ion batteries, and more specifically to a sodium supplement with improved decomposition efficiency, and a preparation method and application thereof. Background Art

[0002] Sodium resources are abundant and evenly distributed, and sodium-ion batteries are expected to become the technology with the most potential for application in the field of large-scale electrochemical energy storage. With the in-depth research of sodium-ion batteries by researchers in recent years, the energy density of sodium-ion batteries has been further improved. However, in the initial stage of the cycle, due to the common problem of low initial coulombic efficiency in batteries, the formation of the solid electrolyte interface (SEI) at the negative electrode and other factors will consume a large amount of active sodium ions from the positive electrode, resulting in a decrease in the overall energy density of the battery. The problem of active sodium ion loss has hindered the large-scale application of sodium-ion batteries.

[0003] In order to solve the above problems, pre-sodiumization technology is currently widely used to supplement active sodium ions. In sodium-ion batteries without a pre-sodiumization process, all sodium ion losses come from the positive electrode active materials. The negative electrode with low initial coulombic efficiency requires heavier positive electrode materials to provide more active sodium ions to make up for the irreversible consumption at the negative electrode, which leads to waste of active sodium ions and energy density attenuation. The pre-sodiumization process can introduce additional active sodium ions to make up for the loss of irreversible processes, thereby avoiding the waste of positive electrode active materials, which is beneficial to the improvement of energy density. Pre-sodiumization methods can be divided into pre-sodiumization on the positive electrode side and pre-sodiumization on the negative electrode side. The pre-sodium addition on the positive electrode side achieves the effect of pre-sodium addition on the positive electrode side by adding sodium-rich sodium supplement additives to the positive electrode material. This is a pre-sodium addition method that is more suitable for large-scale industrial production. During the first charge, the pre-sodium agent undergoes electrochemical oxidation and decomposition at a certain potential, releasing excess active sodium ions, which migrate irreversibly to the electrolyte and the negative electrode, thereby increasing the active sodium ion content during the cycle and improving the overall energy density of the battery. Existing sodium supplement additives include NaCrO2, Na2NiO2, Na2C4O4, Na2CO3, NaN3, etc. However, many existing sodium supplement materials currently have problems with insufficient sodium content and low specific capacity. For example, the sodium contents of NaCrO2 and Na2NiO2 are 21.5% and 33.6% respectively, and the theoretical specific capacities are 251mAh / g and 391mAh / g respectively. However, in actual use, the decomposition is incomplete, and the specific capacities of the materials are only 229mAh / g and 277mAh / g respectively, which are far lower than the theoretical specific capacities and are difficult to meet the demand for efficient pre-sodium (J.Phys.Chem.C 2015, 119, 1, 166–175, Chem.Mater.2015, 27, 19, 6682-6688). Many sodium supplement materials reported in patents also have the problem of low theoretical capacity. It is urgent to find a new sodium-rich additive with high specific capacity.

[0004] Sodium orthosilicate (Na4SiO4) is an ideal sodium-rich material with a sodium content of up to 50wt% and a theoretical specific capacity of 583mAh / g. It is the silicate material with the highest sodium content in the binary system. However, in the actual application of sodium orthosilicate, it was found that the decomposition voltage of pure sodium orthosilicate material is too high and the decomposition efficiency is low, making it difficult to directly use it as a sodium supplement in positive electrode materials. Summary of the invention

[0005] The invention provides a sodium supplement with improved decomposition efficiency and a preparation method and application thereof, so as to solve the problem of low decomposition efficiency of sodium supplement materials in the prior art.

[0006] In a first aspect, the present invention provides a sodium supplement with improved decomposition efficiency, comprising conductive carbon and sodium orthosilicate in a mass ratio of 1:2 to 10.

[0007] As a possible implementation manner, the conductive carbon is one or a combination of Super P, acetylene black, Ketjen black, carbon nanotubes, conductive graphite, redox graphene, and ordered mesoporous carbon.

[0008] In a second aspect, the present invention provides a method for preparing the sodium supplement described in any possible implementation of the first aspect, comprising the following steps: mixing the raw material components in proportion according to the formula components contained in the sodium supplement described in any possible implementation of the first aspect, grinding in an anaerobic environment, to obtain the sodium supplement with improved decomposition efficiency.

[0009] As a possible implementation, the oxygen-free environment is achieved by introducing an inert gas; and / or the grinding is performed by adding ball milling beads to a ball milling jar for ball milling.

[0010] As a possible implementation method, the ball milling condition is: a rotation speed of 300 to 700 rpm·min -1 , duration 10 to 60 hours.

[0011] In a third aspect, the present invention provides a use of the sodium supplement described in any possible implementation of the first aspect or the sodium supplement prepared by the preparation method described in any possible implementation of the second aspect in a sodium ion battery.

[0012] As a possible implementation method, the sodium supplement participates in constituting the positive electrode active material of the sodium ion battery.

[0013] As a possible implementation manner, the proportion of the sodium supplement in the positive electrode active material is 0.1 wt % to 20 wt %.

[0014] In a fourth aspect, the present invention provides a sodium ion battery, wherein the positive electrode active material of the sodium ion battery comprises the sodium supplement described in any possible implementation of the first aspect or the sodium supplement prepared by the preparation method described in any possible implementation of the second aspect.

[0015] As a possible implementation, the positive electrode active material further includes any one of polyanions, Prussian blue or layered oxides; and / or, the negative electrode is any one of Sn, hard carbon or soft carbon materials.

[0016] The sodium supplement provided by the present invention uses a sodium-rich material, sodium orthosilicate (Na4SiO4). Na4SiO4 has a high sodium content and can release four sodium ions after complete decomposition. The theoretical specific capacity is as high as 583mAh / g, which is higher than most of the sodium supplements currently available and is an ideal sodium supplement material. The composite sodium supplement material based on sodium orthosilicate has a high theoretical specific capacity, can effectively replenish the active sodium ions lost at the beginning of the cycle, and improve the energy density of the battery. The present invention composites sodium orthosilicate with conductive carbon, reduces the decomposition voltage of sodium orthosilicate, and enables sodium orthosilicate, a sodium-rich material with a high specific capacity, to be effectively applied to the pre-sodium field.

[0017] However, the inherent low conductivity of sodium orthosilicate exposes problems such as high decomposition voltage and extremely low decomposition efficiency that are not conducive to direct application in actual use. The present invention combines sodium orthosilicate with conductive carbon to construct a conductive network between sodium orthosilicate particles, thereby reducing the decomposition voltage and improving the decomposition efficiency, so that more active sodium ions can be irreversibly released at a lower voltage during the first charging process, effectively playing the role of pre-sodium.

[0018] The invention has simple process, is easy to operate, uses environmentally friendly and pollution-free materials, and is suitable for large-scale use. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0020] Figure 1 This is the XRD diagram of the sodium supplement B provided in the embodiment of the present invention.

[0021] Figure 2 This is the XRD diagram of the sodium supplement G provided in an embodiment of the present invention.

[0022] Figure 3These are SEM images of sodium supplementer G and sodium supplementer H provided in embodiments of the present invention, wherein the left image is the SEM image of sodium supplementer G, and the right image is the SEM image of sodium supplementer H.

[0023] Figure 4 This is the charge and discharge curve of the sodium supplement agent B provided in the embodiment of the present invention. DETAILED DESCRIPTION

[0024] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] In order to solve the problem of low decomposition efficiency of sodium supplement materials in the prior art, the present invention provides a preparation experiment of a sodium supplement with improved decomposition efficiency. Figure 1 The XRD pattern shown shows the crystal structure of sodium supplement A.

[0026] The sodium supplement provided by the present invention uses a sodium-rich material, sodium orthosilicate (Na4SiO4). Na4SiO4 has a high sodium content and can release four sodium ions after complete decomposition. The theoretical specific capacity is as high as 583mAh / g, which is higher than most of the sodium supplements currently available and is an ideal sodium supplement material. The composite sodium supplement material based on sodium orthosilicate has a high theoretical specific capacity, can effectively replenish the active sodium ions lost at the beginning of the cycle, and improve the energy density of the battery. The present invention composites sodium orthosilicate with conductive carbon, reduces the decomposition voltage of sodium orthosilicate, and enables sodium orthosilicate, a sodium-rich material with a high specific capacity, to be effectively applied to the pre-sodium field.

[0027] Furthermore, an electrochemical performance test experiment of a sodium supplementer with improved decomposition efficiency is provided in an embodiment of the present invention, which proves that the sodium supplementer provided by the present invention has better electrochemical performance and better sodium supplementation effect than sodium orthosilicate alone.

[0028] Furthermore, the embodiment of the present invention provides an application performance test experiment of a sodium supplement with improved decomposition efficiency, which proves that the sodium supplement provided by the present invention has better application performance than single sodium orthosilicate.

[0029] The technical solution of the present invention will be further described below in conjunction with specific embodiments.

[0030] Example 1

[0031] This embodiment provides an experiment for preparing a sodium supplement with improved decomposition efficiency.

[0032] Sodium orthosilicate and Ketjen black in a mass ratio of 10:1 were mixed and placed in a ball mill. After adding ball mill beads, an inert gas was introduced. The ball mill was sealed and milled at 300 rpm / min. -1 The mixture was ball milled at a speed of 20 h to obtain sodium supplement agent A.

[0033] Sodium orthosilicate and Ketjen black in a mass ratio of 6:1 were mixed and placed in a ball mill. After adding ball mill beads, an inert gas was introduced. The ball mill was sealed and milled at 300 rpm / min. -1 The sodium supplement B was ball-milled at a speed of 20 h to obtain the sodium supplement B. The sodium supplement B was subjected to X-ray diffraction analysis and the following Figure 1 XRD pattern shown.

[0034] Sodium orthosilicate and Ketjen black in a mass ratio of 2:1 were mixed and placed in a ball mill. After adding ball mill beads, an inert gas was introduced. The ball mill was sealed and milled at 300 rpm / min. -1 The mixture was ball milled at a speed of 20 h to obtain sodium supplement agent C.

[0035] Sodium orthosilicate and Super P in a mass ratio of 6:1 were mixed and placed in a ball mill. After adding ball mill beads, inert gas was introduced. The ball mill was sealed and milled at 300 rpm / min. -1 The mixture was ball milled at a speed of 20 h to obtain sodium supplement agent D.

[0036] Sodium orthosilicate and Ketjen black in a mass ratio of 6:1 were mixed and placed in a ball mill. After adding ball mill beads, an inert gas was introduced. The ball mill was sealed and milled at 200 rpm / min. -1 The mixture was ball milled at a speed of 10 h to obtain sodium supplement agent E.

[0037] Sodium orthosilicate and Ketjen black in a mass ratio of 6:1 were mixed and placed in a ball mill. After adding ball mill beads, an inert gas was introduced. The ball mill was sealed and milled at 700 rpm / min. -1 The mixture was ball milled at a speed of 60 h to obtain sodium supplement agent F.

[0038] Sodium orthosilicate was placed in a ball mill, ball mill beads were added, inert gas was introduced, the ball mill was sealed, and the mill was heated at 300 rpm / min. -1 The sodium supplement G was ball-milled at a speed of 20 h to obtain the sodium supplement G. The sodium supplement G was subjected to X-ray diffraction analysis and the following results were obtained: Figure 2 XRD pattern shown.

[0039] Sodium orthosilicate was used as sodium supplement H. Scanning electron microscope analysis of sodium supplement G and sodium supplement H revealed the following results: Figure 3 SEM images shown.

[0040] Depend on Figure 1 and Figure 2 By comparison, it can be seen that ball milling with conductive carbon did not change the crystal structure of sodium orthosilicate, but the crystallinity of sodium orthosilicate decreased. Figure 3 It can be seen that the particle diameter of sodium orthosilicate is significantly reduced after ball milling, from about 1000 μm to about 5 μm.

[0041] Example 2

[0042] This example provides an electrochemical performance test experiment of a sodium supplement.

[0043] The sodium supplement agent, conductive agent and binder to be tested were ground and mixed in a mass ratio of 8:1:1, and a solvent was added and stirred to form a uniform slurry. The slurry was coated on the current collector and dried in a vacuum drying oven for 12 hours to obtain a sodium supplement material electrode. The sodium supplement material electrode was cut into a disc with a diameter of 12 mm as the electrode to be tested; the electrode to be tested was used as the positive electrode, the metal sodium as the negative electrode, the glass fiber as the separator, and 1 mol·L -1 NaClO4 (EC:PC=1:1, with 5% FEC) was used as the electrolyte and button cells were assembled.

[0044] In this example, KB was used as a conductive agent, PVDF was used as a binder, NMP was used as a solvent, and aluminum foil was used as a current collector. The sodium supplement agents A to G prepared in Example 1 were used as the sodium supplement agents to be tested, respectively, to prepare button batteries A to G. In the voltage range of 2.0 to 4.6 V, 58 mA g -1 The current density was used for charge and discharge test, and the results are shown in Table 1 and Figure 2 Results shown.

[0045] Table 1 Performance test results of button batteries A to G

[0046]

[0047] From Table 1 and Figure 4 It can be seen that mixing conductive carbon and sodium orthosilicate can effectively promote the electrochemical decomposition of sodium orthosilicate and reduce the decomposition voltage of sodium orthosilicate. Therefore, the sodium supplement exhibits a higher capacity during the first cycle of charging. Sodium supplements A to F can irreversibly release more active sodium ions in the first cycle, which can effectively play the role of sodium supplement.

[0048] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0049] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A sodium supplement with improved decomposition efficiency, characterized in that: It comprises conductive carbon and sodium orthosilicate in a mass ratio of 1:2 to 10.

2. The sodium supplement according to claim 1, characterized in that The conductive carbon is one or a combination of SuperP, acetylene black, Ketjen black, carbon nanotubes, conductive graphite, redox graphene, and ordered mesoporous carbon.

3. A method for preparing the sodium supplement according to any one of claims 1 to 2, characterized in that: The following steps are involved: According to the formula components contained in the sodium supplement according to any one of claims 1 to 2, the raw material components are mixed in proportion and ground in an anaerobic environment to obtain the sodium supplement with improved decomposition efficiency.

4. The preparation method according to claim 3, characterized in that: The oxygen-free environment is achieved by introducing an inert gas; And / or, the grinding is performed by adding ball milling beads into a ball milling jar for ball milling.

5. The preparation method according to claim 4, characterized in that: The ball milling conditions are: rotation speed 300-700 rpm·min -1 , duration 10 to 60 hours.

6. Use of the sodium supplement according to any one of claims 1 to 2 or the sodium supplement prepared by the preparation method according to any one of claims 3 to 5 in sodium ion batteries.

7. The use according to claim 6, characterized in that: The sodium supplement is involved in constituting the positive electrode active material of the sodium ion battery.

8. The use according to claim 7, characterized in that: The ratio of the sodium supplement in the positive electrode active material is 0.1 wt % to 20 wt %.

9. A sodium ion battery, characterized in that: The positive electrode active material of the sodium ion battery comprises the sodium supplement according to any one of claims 1 to 2 or the sodium supplement prepared by the preparation method according to any one of claims 3 to 5.

10. The sodium ion battery according to claim 9, characterized in that: The positive electrode active material also includes any one of polyanion, Prussian blue or layered oxide; And / or, the negative electrode is any one of Sn, hard carbon or soft carbon material.