Separator, electrochemical device, and electronic device

By designing the convex bonded particles of 20nm to 100nm on the membrane of the electrochemical device, the cyclic performance and low-temperature performance of the electrochemical device are improved, and the insufficient performance of the electrochemical device in the prior art under low temperature conditions is solved.

CN119009360APending Publication Date: 2024-11-22NINGDE AMPEREX TECHNOLOGY LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411388898.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The insufficient cycling performance of existing electrochemical devices under low temperature conditions affects their application in the field of new energy.

Method used

A diaphragm is designed, including a substrate layer, an inorganic coating and an adhesive layer. The surface of the bonded particles has a protrusion of 20nm to 100nm, which increases the contact site and adhesion between the bonded layer and the electrode sheet, and enhances the Cycling and low-temperature performance of electrochemical devices.

Benefits of technology

By increasing the interface bonding force between the adhesive layer and the electrode sheet and the liquid retention ability of the electrolyte, the circulation performance, low-temperature performance and rate performance of the electrochemical device are significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009360A_ABST
    Figure CN119009360A_ABST
Patent Text Reader

Abstract

The invention provides a diaphragm, an electrochemical device and an electronic device, the diaphragm comprises a base material layer, an inorganic coating and a bonding layer, the inorganic coating is arranged between the base material layer and the bonding layer, the bonding coating contains a plurality of bonding particles, the surface of each bonding particle contains a plurality of bulges, and the average diameter of the bulges is 20-100 nm. The diaphragm provided by the invention is beneficial to improving the cycle performance, the low-temperature performance and the rate capability of the electrochemical device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of electrochemical energy storage, and in particular to a diaphragm, an electrochemical device using the diaphragm, and an electronic device using the electrochemical device. Background Art

[0002] As portable chemical energy sources, electrochemical devices (such as lithium-ion batteries) are widely used in consumer electronics (such as mobile phones, notebooks, cameras, etc.), energy storage products (such as home energy storage, energy storage power stations, UPS power supplies, etc.) and new energy vehicles due to their high energy density, high operating voltage platform, low self-discharge, long service life and environmental friendliness.

[0003] With the development of the new energy industry, the requirements for electrochemical devices are getting higher and higher. The diaphragm is an important component of the electrochemical device, which affects the transmission and interface structure of the electrolyte of the electrochemical device and is related to the low temperature performance and cycle performance of the electrochemical device. Therefore, it is necessary to provide a diaphragm that can simultaneously improve the low temperature performance and cycle performance of the electrochemical device. Summary of the invention

[0004] The present application provides a diaphragm, an electrochemical device and an electronic device.

[0005] The first aspect of the present application provides a diaphragm, including a substrate layer, an inorganic coating and a bonding layer, wherein the inorganic coating is disposed between the substrate layer and the bonding layer, the bonding coating contains a plurality of bonding particles, the surface of each bonding particle comprises a plurality of protrusions, and the average diameter of the protrusions is 20nm to 100nm.

[0006] The membrane in the present application includes a plurality of protrusions on the surface of the bonding particles, and the formation of the protrusions increases the contact sites between the bonding layer and the positive electrode sheet or the negative electrode sheet, which is beneficial to increase the interfacial bonding force between the bonding layer and the electrode sheet; and the protrusions can also be embedded in the positive electrode active material layer or the negative electrode active material layer, further improving the bonding force between the bonding layer and the electrode sheet, thereby helping to improve the cycle performance and energy density of the electrochemical device; the bonding particles include a plurality of protrusions, and the protrusions increase the volume of the bonding particles, which is beneficial to improve the electrolyte retention capacity of the membrane, improve the conduction of lithium ions, and improve the cycle performance and low temperature performance of the electrochemical device. Moreover, the average diameter of the protrusions is within the above range, so that the protrusions can fully contact the active material layer in the electrode sheet, maintain good bonding force, and also help to improve the transmission of the electrolyte between the bonding layer and the active material layer in the electrode sheet, which is beneficial to improve the conduction of active ions, thereby improving the cycle performance, low temperature performance and rate performance of the electrochemical device. More preferably, the average diameter of the protrusions is 40 nm to 100 nm, which can further improve the cycle performance, low temperature performance and rate performance of the electrochemical device.

[0007] Based on the first aspect, in some embodiments, some adjacent bonding particles are interconnected, and the number of interconnected bonding particles accounts for more than 50% of the total number of bonding particles. Some bonding particles are connected to form a mesh structure, which can improve the interface bonding force between the positive electrode sheet and the negative electrode sheet when bonding with the positive electrode sheet or the negative electrode sheet, thereby improving the cycle performance of the electrochemical device.

[0008] Based on the first aspect, in some embodiments, the infrared spectrum of the bonding layer is between 1680 and 1750 cm -1 There is a -COOH group absorption peak, and the transmittance of the absorption peak is 50% to 95%. There is a carboxyl absorption peak in the bonding layer, and the carboxyl group has polarity, which is beneficial to increase the wettability of the electrolyte to the diaphragm and also to improve the bonding force of the bonding layer. When the transmittance of the absorption peak is within the above range, so that the bonding layer contains a suitable number of protrusions, the bonding layer has good bonding force and is also beneficial to improve the wettability of the electrolyte to the diaphragm, thereby improving the cycle performance and rate performance of the electrochemical device.

[0009] Based on the first aspect, in some embodiments, the scanning electron microscope of the diaphragm is 10 4 In the 11.6 μm×7.6 μm photo, the number of bonding particles in the area of ​​11.6 μm×7.6 μm is 10 to 60. The number of bonding particles is within the above range, so that the bonding layer has good bonding force and is also conducive to improving the wettability of the electrolyte to the separator, thereby improving the cycle performance and rate performance of the electrochemical device.

[0010] Based on the first aspect, in some embodiments, each of the bonding particles comprises 5 to 50 protrusions. When the protrusions on the surface of the bonding layer meet the appropriate number in the above region, the contact points between the bonding particles and the positive and negative electrode sheets are increased, and the bonding force between the bonding particles and the positive and negative electrode sheets is increased; when the number of protrusions is within the above range, it is beneficial to further improve the bonding force between the bonding particles and the positive electrode sheet or the negative electrode sheet and the electrolyte retention capacity of the diaphragm, thereby improving the cycle performance and kinetic performance of the electrochemical device.

[0011] Based on the first aspect, in some embodiments, the inorganic coating includes inorganic particles and a binder, and the inorganic particles include at least one of aluminum oxide, aluminum oxide, silicon dioxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zirconium oxide, zinc oxide, calcium oxide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide or barium sulfate. Based on the mass of the inorganic coating, the mass percentage of the inorganic particles is 85% to 95%. The above-mentioned inorganic particles can improve the mechanical strength of the diaphragm, and at the same time, it is also beneficial to improve the wetting effect of the electrolyte on the diaphragm and improve the cycle performance of the electrochemical device.

[0012] Based on the first aspect, in some embodiments, the binder includes at least one of acrylic acid, methyl methacrylate, butyl acrylate, octyl acrylate, isooctyl acrylate, butadiene or acrylonitrile. The above binder is beneficial to improve the bonding force between inorganic particles in the inorganic coating and the bonding force between the inorganic coating and the substrate layer, and is beneficial to improve the interface bonding force between the inorganic coating and the substrate layer, which is beneficial to lithium ion transmission and improves the cycle performance of the electrochemical device.

[0013] Based on the first aspect, in some embodiments, the bonding particles are selected from at least two of the following monomers: butadiene, methyl acrylate, methyl methacrylate, styrene, butyl methacrylate, isooctyl acrylate, ethylene, propylene or vinylidene fluoride. The bonding particles formed by the polymerization of the above monomers have good bonding force, so that the bonding layer can provide a certain bonding force. The bonding layer also includes at least one of acrylic acid, acrylonitrile and butadiene. The addition of the above substances can further improve the bonding force between the bonding layer and the inorganic coating, so that the bonding coating has good bonding force and the wettability of the electrolyte to the diaphragm, which is beneficial to improve the kinetic performance of the electrochemical device.

[0014] Based on the first aspect, in some embodiments, the thickness of the inorganic coating is 0.5 μm to 5 μm. The thickness of the inorganic coating is within the above range, so that the separator has good puncture resistance while maintaining good electrolyte storage capacity and wettability to the separator, which is beneficial to improving the transmission of the electrolyte, thereby improving the cycle performance of the electrochemical device.

[0015] Based on the first aspect, in some embodiments, the average diameter of the bonding particles is 600nm to 1000nm. The average diameter of the bonding particles is within the above range, which is beneficial to improving the bonding force between the bonding particles and the positive electrode sheet or the negative electrode sheet, and is also beneficial to the transmission of the electrolyte, further improving the cycle performance and low temperature performance of the electrochemical device.

[0016] Based on the first aspect, in some embodiments, the particle size Dv50 of the inorganic particles in the inorganic coating is 0.4 μm to 1 μm, and Dv90 is 0.8 μm to 4 μm. The particle sizes Dv50 and Dv90 of the inorganic particles meet the above ranges, which is beneficial to the transmission of the electrolyte and also helps to improve the mechanical strength of the diaphragm and improve the heat shrinkage resistance of the diaphragm, thereby further improving the cycle performance of the electrochemical device.

[0017] Based on the first aspect, in some embodiments, the thickness of the bonding layer is 0.5 μm to 2 μm. The thickness of the bonding layer is within the above-mentioned suitable range. While maintaining a good energy density of the electrochemical device, the wetting of the electrolyte along the thickness direction of the bonding layer and in the direction perpendicular to the plane of the bonding layer is improved, which is beneficial to improving the low temperature performance and cycle performance of the electrochemical device.

[0018] Based on the first aspect, in some embodiments, the coating weight per unit area of ​​the adhesive layer is 0.5 mg / 5000 mm 2 Up to 3mg / 5000mm 2 The coating weight per unit area of ​​the adhesive layer is within the above range. While maintaining good bonding between the adhesive layer and the positive and negative electrode sheets and between the adhesive layer and the inorganic coating, it is also beneficial for the electrolyte to infiltrate the diaphragm and improve the transmission of the electrolyte, thereby further improving the low temperature performance and cycle performance of the electrochemical device.

[0019] Based on the first aspect, in some embodiments, the thickness of the inorganic coating is d1, the thickness of the substrate layer is d2, and the separator satisfies: 0.05≤d1 / d2≤1. The thickness of the inorganic coating and the thickness of the substrate layer satisfy the above relationship, which not only satisfies the heat shrinkage resistance of the separator but also facilitates the transmission of the electrolyte, so that the electrochemical device maintains good cycle performance and low temperature performance.

[0020] Based on the first aspect, in some embodiments, the porosity of the separator is 30% to 50%. The porosity of the separator within the above range can not only improve the liquid retention capacity of the separator, but also reduce the transmission impedance of lithium ions and improve the transmission capacity of lithium ions, thereby improving the cycle performance of the electrochemical device.

[0021] The bonding particles are formed by swelling of polymer particles. At 60°C, the swelling degree of the polymer particles in carboxylic acid esters after 24 hours is 100% to 300%; the carboxylic acid esters include at least one of methyl formate, ethyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate or propyl propionate. The protrusions on the surface of the bonding particles can be formed by swelling of some polymer particles in the electrolyte and protruding from the surface. When the swelling degree of the polymer particles is within the above range, the bonding layer has good bonding force and is also conducive to the transmission of the electrolyte, and can also reduce the pore blockage of the substrate layer, which is conducive to further improving the cycle performance and low temperature performance of the electrochemical device.

[0022] The second aspect of the present application provides an electrochemical device, comprising an electrode assembly, the electrode assembly comprising a positive electrode sheet, a negative electrode sheet and a separator, the separator being located between the positive electrode sheet and the negative electrode sheet. The separator is conducive to improving the cycle performance and low temperature performance of the electrochemical device.

[0023] A third aspect of the present application provides an electronic device, which includes an electrochemical device. The electrochemical device includes a diaphragm, and the diaphragm improves the cycle performance and low-temperature performance of the electrochemical device, thereby facilitating the electronic device to have a good service life. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0025] Figure 1 This is a scanning electron microscope image of the diaphragm provided in Example 1 of the present application.

[0026] Figure 2 for Figure 1 Magnified scanning electron micrograph of area A. DETAILED DESCRIPTION

[0027] The technical scheme in the embodiment of the present application is described clearly and in detail below. Obviously, the described embodiment is a part of the embodiment of the present application, rather than all the embodiments. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present application. The terms used in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application.

[0028] As used herein, amounts, ratios and other numerical values ​​are sometimes presented herein in a range format. It should be understood that such a range format is used for convenience and brevity, and should be flexibly construed to include not only the values ​​explicitly specified as range limits, but also all individual values ​​or sub-ranges encompassed within the range, as if each value and sub-range were explicitly specified.

[0029] The present application provides a diaphragm, including a substrate layer, an inorganic coating and a bonding layer, wherein the inorganic coating is disposed between the substrate layer and the bonding layer, and the bonding coating comprises a plurality of bonding particles, wherein the surface of each bonding particle comprises a plurality of protrusions, and the average diameter of the protrusions is 20 nm to 100 nm.

[0030] The membrane in the present application, the surface of the bonding particles includes a plurality of protrusions, the formation of the protrusions increases the contact sites between the bonding layer and the positive electrode sheet or the negative electrode sheet, which is conducive to increasing the interfacial bonding force between the bonding layer and the electrode sheet; and the protrusions can also be embedded in the positive electrode active material layer or the negative electrode active material layer, further improving the bonding force between the bonding layer and the electrode sheet, thereby helping to improve the cycle performance and energy density of the electrochemical device; the bonding particles contain a plurality of protrusions, the setting of the protrusions increases the volume of the bonding particles, which is conducive to improving the electrolyte retention capacity of the membrane, and is conducive to improving the conduction of lithium ions, and improving the cycle performance and low temperature performance of the electrochemical device. Moreover, the average diameter of the protrusions is within the above range, so that the protrusions can fully contact the active material layer in the electrode sheet, maintain good bonding force, and also help to improve the transmission of the electrolyte between the bonding layer and the active material layer in the electrode sheet, which is conducive to improving the conduction of active ions, thereby improving the cycle performance, low temperature performance and rate performance of the electrochemical device.

[0031] See also Figure 1 and Figure 2 A plurality of bonding particles N are formed on the surface of the diaphragm, the bonding particles N are convexly arranged on the surface of the diaphragm, and a plurality of protrusions T (such as Figure 2 A plurality of protrusions T are formed and cover the entire surface of the bonding particle N.

[0032] If the average diameter of the protrusion T is small, such as less than 20nm, the contact area between the protrusion T and the positive electrode sheet or the negative electrode sheet will be reduced, and the bonding force between the bonding layer and the electrode sheet will be reduced. If the average diameter of the protrusion T is too small, the number of protrusions T will be indirectly increased, affecting the transmission of the electrolyte in the plane direction perpendicular to the bonding layer, thereby affecting the cycle performance and low temperature performance of the electrochemical device. If the average diameter of the protrusion T is large, such as greater than 100nm, the contact site with the positive electrode sheet or the negative electrode sheet will be reduced, affecting the interfacial bonding force between the bonding layer and the positive electrode sheet or the negative electrode sheet. In some embodiments, the average diameter of the protrusion T can be 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, or any value within the range composed of any two of the above values.

[0033] In some embodiments, the average diameter of the protrusions may be 40 nm to 100 nm, and further, the average diameter of the protrusions may be 40 nm to 80 nm, which can further improve the cycle performance, low temperature performance and rate performance of the electrochemical device.

[0034] In some embodiments, some adjacent bonding particles are interconnected, and the number of interconnected bonding particles accounts for more than 50% of the total number of bonding particles. Some bonding particles are connected to form a mesh structure, which can improve the interfacial bonding force between the positive electrode sheet and the negative electrode sheet when bonded to the positive electrode sheet or the negative electrode sheet, thereby improving the cycle performance of the electrochemical device. In some embodiments, the number of interconnected bonding particles accounts for 50%, 60%, 70%, 80%, 90%, 95% of the total number of bonding particles, or any value within the range of any two of the above values.

[0035] In some embodiments, the number of interconnected bonding particles is between 50% and 100% of the total number of bonding particles.

[0036] In some embodiments, the infrared spectrum of the bonding layer is between 1680 and 1750 cm -1There is a -CO OH group absorption peak, and the transmittance of the absorption peak is 50% to 95%. There is a carboxyl absorption peak in the bonding layer, and the carboxyl group has polarity, which is beneficial to increase the wettability of the electrolyte to the diaphragm and also to improve the bonding force of the bonding layer. When the transmittance of the absorption peak is within the above range, so that the bonding layer contains an appropriate number of protrusions, the bonding layer has good bonding force, and it is also beneficial to improve the wettability of the electrolyte to the diaphragm, thereby improving the cycle performance and rate performance of the electrochemical device. If the transmittance of the absorption peak is small, such as less than 50%, the bonding layer contains more protrusions, which may affect the transmission of the electrolyte and affect the cycle performance and rate performance of the electrochemical device; if the transmittance of the absorption peak is large, such as greater than 95%, the bonding layer contains fewer protrusions, which reduces the bonding force of the bonding layer and affects the cycle performance of the electrochemical device. In some embodiments, the transmittance of the -COOH absorption peak can be 50%, 60%, 70%, 80%, 90%, 95% or any value within the range composed of any two of the above values.

[0037] In some embodiments, scanning electron microscopy of the membrane 10 4 In the photo taken 2x, in the area of ​​11.6μm×7.6μm, the number of bonding particles is 10 to 60. The number of bonding particles is within the above range, so that the bonding layer has good bonding force, while also helping to improve the wettability of the electrolyte to the diaphragm, thereby improving the cycle performance and rate performance of the electrochemical device. If the number of bonding particles is small, the bonding force between the bonding layer and the positive electrode sheet and the negative electrode sheet will be reduced. If there are more bonding particles, the rate performance and low temperature performance of the electrochemical device may be reduced. In some embodiments, the number of bonding particles is 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60 or any value within the range composed of any two of the above values.

[0038] In some embodiments, each bonding particle includes 5 to 50 protrusions. When the protrusions on the surface of the bonding layer meet the appropriate number in the above region, the contact sites between the bonding particles and the positive and negative electrode sheets are increased, and the bonding force between the bonding particles and the positive and negative electrode sheets is increased; within the above range of the number of protrusions, it is more conducive to embedding the bonding particles into the active material layer of the positive electrode sheet or the negative electrode sheet, further improving the bonding force between the bonding particles and the positive electrode sheet or the negative electrode sheet, thereby facilitating the improvement of the cycle performance and energy density of the electrochemical device; at the same time, within the above range of the number of protrusions, it is also more conducive to improving the electrolyte retention capacity of the diaphragm, improving the conduction of lithium ions, and improving the cycle performance and kinetic performance of the electrochemical device. In some embodiments, within an area of ​​11.6 μm×7.6 μm, the number of protrusions can be 5, 8, 10, 12, 14, 16, 18, 20, 24, 28, 30, 32, 34, 38, 40, 44, 48, 50 or any value within the range formed by any two of the above values.

[0039] In some embodiments, the inorganic coating includes inorganic particles and a binder, and the inorganic particles include at least one of aluminum oxide, aluminum oxide, silicon dioxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zirconium oxide, zinc oxide, calcium oxide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide, or barium sulfate. The above-mentioned inorganic particles can improve the mechanical strength of the diaphragm, and are also conducive to improving the wetting effect of the electrolyte on the diaphragm, thereby improving the cycle performance of the electrochemical device.

[0040] The binder includes at least one of acrylic acid, methyl methacrylate, butyl acrylate, octyl acrylate, isooctyl acrylate, butadiene or acrylonitrile. The above-mentioned binder is beneficial to improve the bonding force between the inorganic particles in the inorganic coating and the bonding force between the inorganic coating and the substrate layer, which is beneficial to improve the interfacial bonding force between the inorganic coating and the substrate layer, which is beneficial to lithium ion transmission and improves the cycle performance of the electrochemical device. Based on the mass of the inorganic coating, the mass percentage of the inorganic particles is 85% to 95%. The mass percentage of the inorganic particles within the above range can enable the electrochemical device to improve the thermal safety of the electrochemical device on the basis of having good kinetic performance. In some embodiments, based on the mass of the inorganic coating, the mass percentage of the inorganic particles can be 85%, 87%, 89%, 90%, 92%, 93%, 94%, 95% or any value within the range composed of any two of the above values.

[0041] Based on the mass of the inorganic coating, the mass percentage of the binder is 5% to 15%. The mass percentage of the binder within the above range can provide good adhesion between the inorganic coating and the substrate layer. In some embodiments, based on the mass of the inorganic coating, the mass percentage of the binder can be 5%, 7%, 8%, 9%, 10%, 12%, 13%, 14%, 15%, or any value within the range formed by any two of the above values.

[0042] In some embodiments, the bonding particles are selected from at least two of the following monomers: butadiene, methyl acrylate, methyl methacrylate, styrene, butyl methacrylate, isooctyl acrylate, ethylene, propylene or vinylidene fluoride. The bonding particles formed by the polymerization of the above monomers have good bonding force and electrolyte wettability to the bonding layer, so that the bonding layer can provide a certain bonding force.

[0043] The bonding particles also include at least one of acrylic acid, acrylonitrile and butadiene. The addition of the above substances can further improve the bonding force between the bonding layer and the inorganic coating, so that the bonding coating has good bonding force, which is beneficial to improving the cycle performance of the electrochemical device.

[0044] In some embodiments, the thickness of the inorganic coating is 0.5 μm to 5 μm. The thickness of the inorganic coating is within the above range, so that the diaphragm has good puncture resistance while maintaining good storage capacity for the electrolyte and wettability of the electrolyte to the diaphragm, which is beneficial to improve the transmission of the electrolyte, thereby improving the cycle performance of the electrochemical device. In some embodiments, the thickness of the inorganic coating can be 0.5 μm, 0.8 μm, 1 μm, 1.5 μm, 1.8 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm or any value within the range of any two of the above values.

[0045] In some embodiments, the average diameter of the bonding particles is 600nm to 1000nm. The average diameter of the bonding particles is within the above range, which is conducive to improving the bonding force between the bonding particles and the positive electrode sheet or the negative electrode sheet, and is also conducive to the transmission of the electrolyte, further improving the cycle performance and low temperature performance of the electrochemical device. If the average diameter of the bonding particles is small, such as less than 600nm, the number of protrusions contained therein is small, which is not conducive to improving the bonding force of the bonding layer; if the average diameter of the bonding particles is large, such as greater than 1000nm, it will affect the transmission of the electrolyte and is not conducive to improving the low temperature performance of the electrochemical device. In some embodiments, the average diameter of the bonding particles is 600nm, 650nm, 700nm, 800nm, 850nm, 900nm, 950nm, 1000nm or any value within the range composed of any two of the above values.

[0046] In some embodiments, the particle size Dv10 of the inorganic particles in the inorganic coating is 0.2 μm to 0.6 μm, Dv50 is 0.4 μm to 1 μm, and Dv90 is 0.8 μm to 4 μm. The particle sizes Dv10, Dv50 and Dv90 of the inorganic particles meet the above ranges, which is beneficial to the transmission of the electrolyte and also helps to improve the mechanical strength of the diaphragm and improve the heat shrinkage resistance of the diaphragm, thereby further improving the cycle performance of the electrochemical device. In some embodiments, the particle size Dv10 of the inorganic particles can be 0.2 μm, 0.3 μm, 0.4 μm, 0.5 μm, 0.6 μm or any value within the range of any two of the above values. The particle size Dv50 of the inorganic particles can be 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1 μm or any value within the range of any two of the above values. The particle size Dv90 of the inorganic particles can be 0.8 μm, 1 μm, 1.2 μm, 1.5 μm, 1.8 μm, 2.3 μm, 2.7 μm, 3.2 μm, 3.7 μm, 4 μm or any value within the range formed by any two of the above values.

[0047] In some embodiments, the thickness of the bonding layer is 0.5 μm to 2 μm. The thickness of the bonding layer is within the above-mentioned suitable range. Under the condition that the electrochemical device maintains a good energy density, the electrolyte infiltration along the thickness direction of the bonding layer and perpendicular to the plane direction of the bonding layer is improved, which is beneficial to improve the low temperature performance and cycle performance of the electrochemical device. In some embodiments, the thickness of the bonding layer can be 0.5 μm, 0.8 μm, 1 μm, 1.2 μm, 1.5 μm, 1.8 μm, 2 μm, or any value within the range formed by any two of the above values.

[0048] In some embodiments, the coating weight per unit area of ​​the adhesive layer is 0.5 mg / 5000 mm 2 Up to 3mg / 5000mm 2 The coating weight per unit area of ​​the adhesive layer is within the above range. While maintaining good adhesion between the adhesive layer and the positive and negative electrode sheets and between the adhesive layer and the inorganic coating, it is also beneficial for the electrolyte to infiltrate the adhesive layer, improve the transmission of the electrolyte, and thus further improve the low temperature performance and cycle performance of the electrochemical device. In some embodiments, the coating weight per unit area of ​​the adhesive layer is 0.5 mg / 5000 mm 2 , 1mg / 5000mm 2 , 1.5mg / 5000mm 2 , 2mg / 5000mm 2 , 2.5mg / 5000mm 2 、3mg / 5000mm 2 Or any value within the range formed by any two of the above values.

[0049] In some embodiments, the thickness of the inorganic coating is d1, the thickness of the substrate layer is d2, and the separator satisfies: 0.05≤d1 / d2≤1. The thickness of the inorganic coating and the thickness of the substrate layer satisfy the above relationship, which not only satisfies the heat shrinkage resistance of the separator, but also helps to improve the transmission of the electrolyte, so that the electrochemical device maintains good cycle performance and low temperature performance. In some embodiments, the ratio of d1 / d2 can be 0.05, 0.1, 0.2, 0.3, 0.5, 0.8, 1 or any value within the range of any two of the above values.

[0050] In some embodiments, the porosity of the diaphragm is 30% to 50%. The porosity of the diaphragm within the above range can not only improve the liquid retention capacity of the diaphragm, but also reduce the transmission impedance of lithium ions and improve the transmission capacity of lithium ions, thereby improving the cycle performance of the electrochemical device. In some embodiments, the porosity of the diaphragm can be 30%, 32%, 35%, 38%, 40%, 42%, 45%, 48%, 50% or any value within the range composed of any two of the above values. Preferably, the porosity of the diaphragm is 35% to 45%.

[0051] The bonding particles are formed by the swelling of polymer particles. At 60°C, the swelling degree of the polymer particles in carboxylic acid esters after 24 hours is 100% to 300%; the carboxylic acid esters include at least one of methyl formate, ethyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate or propyl propionate. The protrusions on the surface of the bonding particles can be formed by the swelling of some polymer particles in the electrolyte and protruding from the surface. When the swelling degree of the polymer particles is within the above range, the bonding layer has good bonding force and is also conducive to the transmission of the electrolyte, and can also reduce the pore blocking of the substrate layer, which is conducive to further improving the cycle performance and low temperature performance of the electrochemical device. In some embodiments, the swelling degree of the polymer particles in the carboxylic acid ester after 24 hours can be 100%, 120%, 150%, 200%, 220%, 250%, 300% or any value within the range composed of any two of the above values.

[0052] In some embodiments, the diaphragm includes two adhesive layers, one adhesive layer is located on the surface of the inorganic coating layer away from the substrate layer, and the other adhesive layer is located on the surface of the substrate layer away from the inorganic coating layer. The adhesive layer containing the inorganic coating layer is close to the positive electrode sheet, and the inorganic coating layer can prevent the damage to the diaphragm caused by crystallization on the positive electrode sheet, thereby improving the safety of the electrochemical device. Adhesive layers are included on both sides of the diaphragm to improve the bonding force between the diaphragm and the positive electrode sheet and the negative electrode sheet, reduce the possibility of deformation of the electrochemical device during the cycle, and improve the cycle performance of the electrochemical device.

[0053] In the present application, the type of monomer selected from the bonding particles, the content of acrylates, the content of linear esters in the electrolyte, and the immersion time and temperature of the polymer particles will affect the average diameter of the protrusions on the surface of the bonding particles. If the content of acrylates in the monomer polymerization is greater or the content of linear esters in the electrolyte is greater, the average diameter of the protrusions will increase. The longer the temperature and / or time that the polymer particles are immersed in the electrolyte containing carboxylic acid esters, the greater the average diameter of the protrusions. The suitable immersion time of the diaphragm in the electrolyte can be 8h to 24h, and the immersion temperature can be 60°C to 80°C.

[0054] The number of bonding particles, average diameter and number of protrusions in the bonding layer are all affected by the coating weight per unit area of ​​the bonding layer, the synthesis process steps, the swelling degree of the polymer particles and the type of monomer polymerization from which the bonding particles are selected.

[0055] The ratio of the number of interconnected bonding particles is affected by the coating weight per unit area, the type of monomer from which the bonding particles are selected, the average diameter of the bonding particles, and the swelling degree.

[0056] In the present application, the thickness of the bonding layer and the inorganic coating layer can be regulated by changing the average diameter of the bonding particles, the particle size of the inorganic particles and the coating amount per unit area. The particle size of the inorganic particles can be regulated by regulating the stirring rate, stirring time and stirring rate.

[0057] In one embodiment of the present application, an electrochemical device is also provided, including a housing, an electrode assembly, and an electrolyte, wherein the battery cell and the electrolyte are located in the housing. The housing may be a packaging bag obtained by packaging with a packaging film (such as an aluminum-plastic film), such as when the electrochemical device is a soft-pack secondary battery. In other embodiments, the electrochemical device may also be a steel shell battery, an aluminum shell battery, and the like.

[0058] The electrode assembly includes a positive electrode sheet, a negative electrode sheet and a separator, wherein the separator is located between the positive electrode sheet and the negative electrode sheet. The electrode assembly may be a laminated structure, which is formed by stacking the positive electrode sheet, the separator and the negative electrode sheet. In other embodiments, the electrode assembly may also be a wound structure, which is formed by stacking the positive electrode sheet, the separator and the negative electrode sheet and then winding them.

[0059] Positive electrode

[0060] The positive electrode plate includes a positive current collector and a positive active layer disposed on the positive current collector. The positive current collector may be aluminum foil or nickel foil, etc., or may be any composite current collector disclosed in the prior art, such as but not limited to the current collector formed by combining the aforementioned conductive foil and the polymer substrate. The positive active layer contains a positive active material, and the positive active material includes a compound that reversibly embeds and deintercalates lithium ions (i.e., a lithiated intercalation compound). In some embodiments, the positive active material may include a lithium transition metal composite oxide. The lithium transition metal composite oxide contains lithium and at least one element selected from cobalt, manganese and nickel. In some embodiments, the positive active material may include but is not limited to lithium cobaltate, lithium nickel manganese cobaltate, lithium nickel manganese aluminum, lithium iron phosphate, lithium vanadium phosphate, lithium cobalt phosphate, lithium manganese phosphate, lithium manganese iron phosphate, lithium iron silicate, lithium vanadium silicate, lithium cobalt silicate, lithium manganese silicate, spinel lithium manganese oxide, spinel lithium nickel manganese oxide and lithium titanate.

[0061] The positive electrode active layer also includes a binder to bond the positive electrode active material particles to facilitate the formation of a film layer, and at the same time, it can also improve the bonding force between the positive electrode active layer and the positive electrode current collector. In some embodiments, the binder may include but is not limited to polyvinyl alcohol, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene butadiene rubber, acrylic (ester) styrene butadiene rubber, epoxy resin or nylon, etc. At least one of the above.

[0062] The positive electrode active layer may also include a conductive material, including but not limited to a carbon-based material, a metal-based material, a conductive polymer, or any combination thereof. In some embodiments, the carbon-based material may include but is not limited to natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, or any combination thereof. In some embodiments, the metal-based material may include but is not limited to metal powder or metal fiber, such as copper, nickel, aluminum, or silver. In some embodiments, the conductive polymer may be a polyphenylene derivative.

[0063] Diaphragm

[0064] The material and shape of the diaphragm used in the electrochemical device of the present application are not particularly limited, and it can be any technology disclosed in the prior art. In some embodiments, the diaphragm includes a polymer or inorganic substance formed of a material that is stable to the electrolyte of the present application. In the present application, the diaphragm described above is used.

[0065] For example, the substrate layer is a non-woven fabric, film or composite film with a porous structure, and the material of the substrate layer is selected from at least one of polyethylene, polypropylene, polyethylene terephthalate and polyimide. Specifically, polypropylene porous film, polyethylene porous film, polypropylene non-woven fabric, polyethylene non-woven fabric or polypropylene-polyethylene-polypropylene porous composite film can be selected.

[0066] Electrolyte

[0067] According to some embodiments of the present application, the electrolyte includes an organic solvent, a lithium salt, and optional additives.

[0068] The organic solvent in the electrolyte of the present application may be any organic solvent known in the prior art that can be used as a solvent for the electrolyte. The electrolyte used in the electrolyte according to the present application is not limited, and it can be any electrolyte known in the prior art. The additive of the electrolyte according to the present application can be any additive known in the prior art that can be used as an electrolyte additive. In some embodiments, the organic solvent includes, but is not limited to: ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC) or ethyl propionate.

[0069] In some embodiments, the organic solvent includes an ether solvent, for example, at least one of 1,3-dioxolane (DOL) and ethylene glycol dimethyl ether (DME). In some embodiments, the lithium salt includes at least one of an organic lithium salt or an inorganic lithium salt. In some embodiments, the lithium salt includes, but is not limited to: lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium difluorophosphate (LiPO2F2), bistrifluoromethanesulfonyl imide lithium LiN(CF3 SO2)2 (LiTF SI), bis(fluorosulfonyl)imide lithium Li(N(SO2F)2)(LiF SI), lithium bis(oxalate borate) LiB(C2O4)2 (LiB OB) or lithium difluorooxalate borate LiBF2(C2O4) (LiDFOB). In some embodiments, the additive includes at least one of fluoroethylene carbonate and adiponitrile.

[0070] According to some embodiments of the present application, the electrochemical device of the present application includes, but is not limited to: a lithium-ion battery.

[0071] The present application also applies the electrochemical device to the electronic device, and the electrochemical device supplies power to the load of the electronic device. In the above electronic device, the electrochemical device has good low temperature performance and cycle performance, which is conducive to improving the service life and low temperature universality of the electronic device.

[0072] Among them, electronic devices may include but are not limited to laptop computers, pen-input computers, mobile computers, e-book players, portable phones, portable fax machines, portable copiers, portable printers, head-mounted stereo headphones, video recorders, LCD televisions, portable cleaners, portable CD players, mini CDs, transceivers, electronic notepads, calculators, memory cards, portable recorders, radios, backup power supplies, motors, cars, motorcycles, power-assisted bicycles, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, flashlights, cameras, large household batteries and lithium-ion capacitors, etc.

[0073] The present application is described below by specific examples and comparative examples. Those skilled in the art should understand that the preparation methods described in the present application are only examples, and any other suitable preparation methods are within the scope of the present application.

[0074] Example 1

[0075] <Preparation of battery separator>

[0076] Inorganic boehmite particles with a Dv50 of 1 μm and polyacrylate were mixed in a mass ratio of 90:10 and dissolved in deionized water to form an inorganic coating slurry with a solid content of 50%. The inorganic coating slurry was then evenly coated on one side of a polyethylene (PE) substrate layer using a micro-concave coating method, and dried in an oven to obtain an inorganic ceramic coating. The particle size Dv 10 of the inorganic particles was 0.84 μm, Dv50 was 1.09 μm, Dv90 was 1.91 μm, and the thickness of the inorganic coating was 2 μm.

[0077] Add 90g of polymer particles (weight average molecular weight of 600,000, polymer monomers include 5% by weight of methyl acrylate, 78% by weight of styrene, 2% by weight of butadiene and 15% by weight of isobutyl acrylate) into a blender, add 10g of sodium carboxymethyl cellulose, stir and mix evenly, add 5g of wetting agent dimethylsiloxane, then add deionized water and stir, adjust the viscosity of the slurry to 2000mPa·s~5000mPa·s, solid content 5%, and obtain a bonding layer slurry. Then, the bonding layer slurry is evenly coated on the surface of the inorganic ceramic coating and the substrate layer by screen printing, with a coating weight of 1mg / 5000mm 2 , and then dried in an oven to form a bonding layer to obtain a diaphragm. The average diameter of the bonding particles in the bonding layer is 0.6 μm, and the porosity of the diaphragm is 42.5%.

[0078] <Preparation of negative electrode sheet>

[0079] The negative electrode active materials artificial graphite, acetylene black, styrene-butadiene rubber and sodium carboxymethyl cellulose are mixed in a mass ratio of 96:1:1.5:1.5, and then deionized water is added as a solvent to prepare a negative electrode slurry with a solid content of 70%, and then a vacuum mixer is used to stir evenly. The negative electrode slurry is evenly coated on one surface of a copper foil with a thickness of 8 μm, dried at 110°C, and cold pressed to obtain a negative electrode sheet coated with a 150 μm negative electrode active material layer on one side, and then the above coating steps are repeated on the other surface of the negative electrode sheet to obtain a negative electrode sheet coated with a negative electrode active material layer on both sides. The negative electrode sheet is cut into a specification of 74 mm × 867 mm and welded to the pole ear for standby use.

[0080] <Preparation of positive electrode sheet>

[0081] The positive electrode active materials lithium cobalt oxide, acetylene black, and polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 94:3:3, and then N-methylpyrrolidone (NMP) is added as a solvent to prepare a positive electrode slurry with a solid content of 75%, and then a vacuum mixer is used to stir evenly. The positive electrode slurry is evenly coated on one surface of an aluminum foil with a thickness of 12μm, dried at 90°C, and cold pressed to obtain a positive electrode sheet coated with a 100μm thick positive electrode active material layer on one side, and then the above steps are repeated on the other surface of the positive electrode sheet to obtain a positive electrode sheet coated with a positive electrode active material layer on both sides. The positive electrode sheet is cut into a specification of 74mm×867mm and welded to the pole ear for standby use.

[0082] <Preparation of Electrolyte>

[0083] In an environment with a water content of less than 10ppm, non-aqueous organic solvents of ethylene carbonate (EC), diethyl carbonate (DEC), propylene carbonate (PC), propyl propionate (PP), and vinylene carbonate (VC) are mixed in a mass ratio of 20:30:20:28:2, and then lithium hexafluorophosphate (LiPF6) is added to the non-aqueous organic solvent to dissolve and mix evenly to obtain an electrolyte. Based on the total mass of the electrolyte, the mass content of LiPF6 is 8%.

[0084] <Preparation of Secondary Battery>

[0085] The positive electrode sheet, battery separator and negative electrode sheet prepared above are stacked in order, and the separator is located between the positive electrode sheet and the negative electrode sheet to play a role of isolation, wherein a surface of the separator containing an inorganic ceramic coating faces the positive electrode sheet and contacts the positive electrode sheet, the negative electrode sheet contacts another adhesive layer, and the positive electrode tab is located on the extension line of at least part of the linear adhesive and then wound to obtain an electrode assembly. The electrode assembly is placed in an aluminum-plastic film packaging bag, and the moisture is removed at 80°C, and the prepared electrolyte is injected. After vacuum packaging, standing, formation, shaping and other processes, a secondary battery is obtained. At 60°C, the swelling degree of the polymer particles in the electrolyte after 24 hours is 150%.

[0086] Performance testing method:

[0087] (1) Average diameter of bonding particles

[0088] In the scanning electron microscope of the diaphragm, the image statistics method is used to count the particle size of the bonding particles in the area of ​​11.6μm×7.6μm, and the particle size of the single particle is used as the standard, excluding the secondary particles formed by multiple particles. The polymer is spherical or quasi-spherical. 32 particles are randomly selected and tested, and the average value is the average diameter of the bonding particles.

[0089] (2) Number of bonding particles

[0090] In the scanning electron microscope of the diaphragm, at 10 4 At a magnification of times, the image statistics method was used to count the number of bonded particles in the area of ​​11.6μm×7.6μm, and the particle size of single particles was taken as the standard, excluding secondary particles formed by multiple particles. The polymer was spherical or quasi-spherical. The data of bonded particles in the above 32 diaphragm areas were counted, and the average value was the number of bonded particles.

[0091] (3) Average diameter of protrusions

[0092] In the scanning electron microscope of the diaphragm, the image statistics method was used to count the number of protrusions on the bonding particles in the area of ​​11.6μm×7.6μm, and the particle size of the single bonding particles was used as the standard to exclude the secondary particle shapes formed by multiple particles. The diameters of the particle protrusions on 32 bonding particles were tested, and the average value was calculated to be the average diameter of the protrusions.

[0093] (4) Number of protrusions

[0094] In the scanning electron microscope of the diaphragm, the image statistics method was used to count the number of protrusions on the bonding particles in the area of ​​11.6μm×7.6μm, and the particle size of the single bonding particles was used as the standard. The secondary particle shape formed by multiple particles was excluded. The number of particle protrusions on 32 bonding particles was counted and the average value was calculated to be the number of protrusions.

[0095] (5) Particle size Dv 10, Dv50 and Dv90 of inorganic particles

[0096] Use laser particle size analyzer Malvern 3000 for measurement. Add 50ml water to the beaker, add about 2g of material (inorganic particles), stir the solution to fully disperse the material; after the equipment is cleaned, add more than 2 / 3 of DI water, and adjust the speed to 2800±50. Click "Initialize Instrument" to wait for the instrument to complete initialization, click "Measure Background", the laser intensity must be higher than 70%, and the background light intensity must be lower than 100. After the background test is completed, add the test sample, wait for the laser shading to reach the specified range of 10-12%, wait for 5-8S, click "Test Sample" to automatically generate the value after the test is completed, and record the three sets of test data Dv 10, Dv50, Dv90; equipment parameter settings: refractive index 1.765, absorptivity 0.1, density 1.05.

[0097] (6) Thickness of bonding layer, inorganic coating and diaphragm

[0098] The test was conducted using a VL 500,000 caliper, including: pressing the "▼" button to make the measuring head close to the test platform, and pressing the "zero" button to reset the thickness gauge. Press the "▲" button to raise the measuring head, pick up the diaphragm and place it flat on the test platform, so that the diaphragm at the measuring position remains flat on the test platform and the measuring position is aligned with the measuring head. Press the "▼" button until the measuring head is stationary. When the data remains stable, record the data in a table; measure 16 points evenly in the horizontal direction (1 point is tested every 20 mm; measure 16 points evenly in the width, and then calculate the average value of a total of 32 points in the horizontal and width directions. Similarly, the bonding layer and inorganic coating are measured in the same way.

[0099] (7) Coating weight per unit area of ​​adhesive layer

[0100] The samples before and after the substrate layer is coated with the adhesive layer are punched into strips of 50*100mm, and the weight is measured with a 4-decimal electronic balance. m1 and m2 are recorded. Six test points are taken before and after coating to find the average value and calculate the coating weight per unit area.

[0101] (8) Porosity of the diaphragm

[0102] Cut the membrane sample into discs with a diameter of 10 mm, and put the punched membrane sample into the sample cup. Place the membrane sample cup into the sample chamber, close the sample chamber, and use the gas exchange method of the true density meter to test. Record the test results, and test each membrane sample 3 times to get the average value.

[0103] (9)-COOH absorption peak test

[0104] Take out 1-2 mg of sample and put it into an agate mortar, add ~150 mg of potassium bromide powder, and grind it thoroughly; put the ground powder into a mold and press it into tablets using a tablet press. Place the pressed sample tablets into the sample chamber and use infrared equipment for testing, with a wave number of 400-4000cm -1 . Plot the test results with the horizontal axis being the wave number cm -1 , the vertical axis is absorbance %; the -COOH absorption peak appears at a wave number of 1680-1750cm -1 interval.

[0105] (10) Swelling test

[0106] Cut the prepared membrane into strips of about 2g with scissors, and make 3 parallel samples for each membrane. Weigh the membrane strips separately, record the initial weight M1, put them into a vial, label the sample name, add the test electrolyte (the electrolyte in the above lithium-ion battery), exceed the film by 3cm, seal the vial, put it in an oven and bake at 60℃ for 24h. Take out the membrane, wipe it clean with dust-free paper, and record the weight M2 of each membrane.

[0107] Swelling degree (%) = (M2-M1) / M1×100%, and the average of the swelling degrees of three parallel samples is taken as the final swelling degree.

[0108] Performance test of lithium-ion battery:

[0109] Adhesion test between diaphragm and electrode plate:

[0110] The national standard GB / T 2790-1995, i.e., the 180° peel test standard, was adopted to test the bonding force between the diaphragm and the positive electrode sheet or the negative electrode sheet. The diaphragm and the positive electrode sheet or the negative electrode sheet were cut into 54.2 mm × 72.5 mm samples. The diaphragm and the positive electrode sheet or the negative electrode sheet were compounded and hot pressed using a hot press. The hot pressing conditions were: temperature 85°C, pressure 1 MPa, and hot pressing time 85 s (seconds). The compounded samples were cut into 15 mm × 54.2 mm strips. The bonding force between the diaphragm and the positive electrode sheet or the negative electrode sheet was tested according to the 180° peel test standard.

[0111] Low temperature capacity retention test:

[0112] At 25°C, the lithium-ion battery is charged to 4.53V at 0.5C constant current, charged to 0.02C at constant voltage, and then discharged to 2.5V at 0.2C at constant current, and the discharge capacity of the lithium-ion battery at 25°C is recorded; then, the lithium-ion battery is charged to 4.53V at 0.5C constant current, charged to 0.02C at constant voltage, and then the lithium-ion battery is placed at -20°C and discharged to 2.5V at 0.2C constant current, and the discharge capacity of the lithium-ion battery at -20°C is recorded. Calculate the capacity retention rate of the lithium-ion battery at -20°C, low temperature capacity retention rate = (final discharge capacity of the secondary battery at -20°C / discharge capacity of the first cycle of the secondary battery at 25°C) × 100%.

[0113] Cycle performance test:

[0114] At 25°C, the lithium-ion battery is charged to 4.35V at 3C constant current and to 1.8C at constant voltage, and then discharged to 3.0V at 0.7C to complete a cycle, which is recorded as the first cycle. Then, the above steps are repeated for 800 cycles, and the capacity retention rate after 800 cycles is calculated. The capacity retention rate after 800 cycles = (discharge capacity after 800 cycles / discharge capacity after the first cycle) × 100%.

[0115] Rate performance test:

[0116] At 25°C, the lithium-ion battery is charged to 4.47V at 0.5C constant current, and charged to 0.05C at constant voltage, and then rested for 5 minutes, and then discharged to 3.0V at 0.2C constant current, and then rested for 5 minutes, and then charged to 4.47V at 0.5C constant current, and then charged to 0.05C at constant voltage, and then rested for 5 minutes, and then discharged to 3.0V at 0.5C constant current, and recorded capacity D1, and then rested for 5 minutes, and then discharged to 3.0V at 2C constant current, and recorded capacity D2. Rate performance = D 2 / D 1*100%.

[0117] Embodiment 0, Embodiment 2 to 5

[0118] The time for which the diaphragm in the lithium-ion battery is immersed in the electrolyte is changed, and the average diameter of the protrusions on the diaphragm surface is adjusted to obtain the relevant parameters in Table 1 and Table 2. The remaining steps are the same as in Example 1.

[0119] Comparative Examples 1 to 3

[0120] The types of polymer monomers were changed to obtain the relevant parameters in Table 1 and Table 2, and the rest were the same as in Example 1.

[0121] Examples 6 to 12

[0122] The temperature at which the separator in the lithium-ion battery is immersed in the electrolyte is changed to obtain the relevant parameters in Table 3, and the rest is the same as in Example 1.

[0123] Examples 13 to 18

[0124] The coating weight per unit area of ​​the adhesive layer was changed to obtain the relevant parameters in Table 4, and the rest was the same as in Example 4.

[0125] Examples 19 to 23

[0126] The thickness of the inorganic coating was changed to obtain the relevant parameters in Table 5, and the rest was the same as in Example 1.

[0127] Examples 24 to 27

[0128] The process of synthesizing the bonding particles was changed, and the average diameter of the bonding particles was adjusted to obtain the relevant parameters in Table 6. The rest was the same as in Example 1.

[0129] Examples 28 to 31

[0130] The mass proportion of isobutyl acrylate in the polymer monomer was changed, and the content of the interconnected bonding particles was adjusted to obtain the relevant parameters in Table 7. The rest was the same as in Example 1.

[0131] Examples 32 to 33

[0132] The porosity of the diaphragm was changed to obtain the relevant parameters in Table 8, and the rest was the same as in Example 1.

[0133] Examples 34 to 36

[0134] The transmittance of the bonding layer was changed to obtain the relevant parameters in Table 9, and the rest was the same as in Example 1.

[0135] Examples 37 to 41

[0136] By changing the ratio of d1 / d2, the relevant parameters in Table 10 are obtained, and the rest are the same as in Example 1.

[0137] Examples 42 to 43

[0138] The types and proportions of the polymer monomers forming the bonded particles were changed to obtain the relevant parameters in Table 11, and the rest were the same as in Example 1.

[0139] Table 1

[0140]

[0141]

[0142] Table 2

[0143]

[0144] As can be seen from Tables 1 and 2, by adjusting the average diameter of the protrusions on the surface of the bonding particles, the average diameter of the protrusions is within an appropriate range, which improves the bonding force between the separator and the positive electrode sheet, and between the separator and the negative electrode sheet, and also significantly improves the cycle performance, low temperature performance and rate performance of the lithium-ion battery. In Comparative Example 1, no bonding particles and protrusions are formed.

[0145] Table 3

[0146]

[0147]

[0148] From Table 3 above, by changing the temperature at which the diaphragm is immersed in the electrolyte and adjusting the number of protrusions, when the number of protrusions is in the range of 5 to 50, the diaphragm and the positive electrode sheet, and the diaphragm and the negative electrode sheet have good adhesion, and the prepared lithium-ion battery has good cycle performance, low temperature performance and rate performance.

[0149] Table 4

[0150]

[0151] In Table 4, in Example 4 and Examples 13 to 18, the coating weight per unit area of ​​the bonding layer is adjusted. When the number of bonding particles is in the range of 10 to 60, while maintaining good bonding between the diaphragm and the positive electrode sheet and the negative electrode sheet, the prepared lithium-ion battery also has good cycle performance, low temperature performance and rate performance.

[0152] Table 5

[0153]

[0154] In the above Table 5, from Example 1 and Example 19 to Example 23, at different thicknesses of the inorganic coating, the separator maintains good adhesion with the positive electrode sheet and the negative electrode sheet, respectively, and the lithium-ion batteries prepared therefrom also have excellent cycle performance, low temperature performance and rate performance.

[0155] Table 6

[0156]

[0157]

[0158] In the above Table 6, from Example 1 and Example 24 to Example 27, when the bonding particles have different average diameters, the separator maintains good bonding with the positive electrode sheet and the negative electrode sheet, respectively, and the lithium-ion batteries prepared therefrom also have excellent cycle performance, low temperature performance and rate performance.

[0159] Table 7

[0160]

[0161]

[0162] In Table 7, in Example 1 and Examples 28 to 31, when the content of the interconnected bonding particles is within an appropriate range, the separator maintains good bonding with the positive electrode sheet and the negative electrode sheet, respectively, and the lithium-ion batteries prepared therefrom also have excellent cycle performance, low temperature performance and rate performance.

[0163] Table 8

[0164]

[0165] In Table 8, in Example 1 and Examples 32 and 33, when the porosity of the diaphragm is within an appropriate range, the diaphragm maintains good adhesion with the positive electrode sheet and the negative electrode sheet, respectively, and the lithium-ion batteries prepared therefrom also have excellent cycle performance, low temperature performance and rate performance.

[0166] Table 9

[0167]

[0168] In the above Table 9, the transmittance of the bonding layer is adjusted by adjusting the proportion of carboxyl groups grafted on the bonding particles in the bonding layer. When the transmittance is within an appropriate range, the diaphragm and the electrode maintain good adhesion, and the prepared lithium-ion battery also has excellent cycle performance, low temperature performance and rate performance.

[0169] Table 10

[0170]

[0171] In Table 10, in Example 1 and Examples 36 to 40, d1 / d2 is within the applicable range, the separator and the electrode maintain good adhesion, and the lithium ion batteries prepared therefrom also have excellent cycle performance, low temperature performance and rate performance.

[0172] Table 11

[0173]

[0174] In Table 11, in Example 1 and Example 42 to Example 43, the types and proportions of polymer monomers forming the bonding particles are changed, the diaphragm and the electrode maintain good bonding force, and the lithium-ion batteries prepared therefrom also have excellent cycle performance, low temperature performance and rate performance.

[0175] The above disclosure is only a preferred implementation mode of the present application, and certainly cannot be used to limit the present application. Therefore, equivalent changes made according to the present application are still within the scope covered by the present application.

Claims

1. A diaphragm, characterized in that: It includes a substrate layer, an inorganic coating layer and a bonding layer, wherein the inorganic coating layer is arranged between the substrate layer and the bonding layer, and the bonding layer contains a plurality of bonding particles, and the surface of each of the bonding particles contains a plurality of protrusions, and the average diameter of the protrusions is 20nm to 100nm.

2. The diaphragm according to claim 1, characterized in that The average diameter of the protrusions is 40 nm to 100 nm.

3. The diaphragm according to claim 1, characterized in that Some of the adjacent bonding particles are connected to each other, and the number of the bonding particles connected to each other accounts for 50% to 100% of the total number of the bonding particles.

4. The diaphragm according to claim 1, characterized in that The infrared spectrum of the bonding layer is between 1680 and 1750 cm -1 There is an absorption peak of a -COOH group, and the transmittance of the absorption peak is 50% to 95%.

5. The diaphragm according to claim 1, characterized in that In the scanning electron microscopy of the diaphragm 10 4 In the photo with a magnification of 1.5×1.2, in the area of ​​11.6 μm×7.6 μm, the separator satisfies at least one of the following conditions: (1) The number of the bonding particles is 10 to 60; (2) Each of the bonding particles comprises 5 to 50 protrusions.

6. The diaphragm according to claim 1, characterized in that The inorganic coating comprises inorganic particles and a binder, wherein the inorganic particles comprise at least one of aluminum oxide, aluminum oxide, silicon dioxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zirconium oxide, zinc oxide, calcium oxide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide or barium sulfate; The binder comprises at least one of acrylic acid, methyl methacrylate, butyl acrylate, octyl acrylate, isooctyl acrylate, butadiene or acrylonitrile; Based on the mass of the inorganic coating, the mass percentage of the inorganic particles is 85% to 95%.

7. The diaphragm according to claim 1, characterized in that The bonding particles are formed by polymerization of at least two monomers selected from the group consisting of butadiene, methyl acrylate, methyl methacrylate, styrene, butyl methacrylate, isooctyl acrylate, ethylene, propylene, and vinylidene fluoride.

8. The diaphragm according to any one of claims 1 to 7, characterized in that The diaphragm satisfies at least one of the following conditions: (1) The thickness of the inorganic coating is 0.5 μm to 5 μm; (2) The average diameter of the bonding particles is 600 nm to 1000 nm; (3) The particle size Dv50 of the inorganic particles in the inorganic coating is 0.4 μm to 1 μm, and Dv90 is 0.8 μm to 4 μm; (4) The thickness of the adhesive layer is 0.5 μm to 2 μm, and the coating weight per unit area of ​​the adhesive layer is 0.5 mg / 5000 mm 2 Up to 3mg / 5000mm 2 ; (5) The thickness of the inorganic coating layer is d1, the thickness of the substrate layer is d2, and the separator satisfies: 0.05≤d1 / d2≤1.0; (6) The adhesive layer further comprises at least one of acrylic acid, acrylonitrile and butadiene.

9. The diaphragm according to claim 1, characterized in that The porosity of the separator is 30% to 50%.

10. The diaphragm according to claim 1, characterized in that The bonding particles are formed by swelling of polymer particles, and at 60° C., the swelling degree of the polymer particles in carboxylic acid ester after 24 hours is 100% to 300%; The carboxylic acid ester includes at least one of methyl formate, ethyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate or propyl propionate.

11. An electrochemical device, comprising an electrode assembly, wherein the electrode assembly comprises a positive electrode sheet and a negative electrode sheet, characterized in that: The electrode assembly further comprises a separator as claimed in any one of claims 1 to 10, wherein the separator is located between the positive electrode sheet and the negative electrode sheet.

12. An electronic device, characterized in that: Comprising the electrochemical device as claimed in claim 11.