Zn-Fe bimetal MOFs material modified diaphragm and preparation method thereof

Through the preparation of Zn-Fe bimetallic MOFs material modified separators, the problem of degradation of lithium-sulfur batteries in high temperature and corrosive environments is solved, and the cycle stability and energy efficiency are achieved, and the production cost is reduced. Mass production.

CN119009363AActive Publication Date: 2024-11-22SHAANXI UNIV OF SCI & TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411076730.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-22
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

The performance of existing lithium-sulfur batteries in high temperature or corrosive environments has decreased, the pore structure complexity and performance optimization of MOFs materials are limited, the synthesis process is complex and costly, which affects the cycle stability and large-scale production of the battery.

Method used

The preparation method of Zn-Fe bimetallic MOFs material modified separator is mixed with FeCl2·4H2O, 2,2'-bipyridine-5,5'-dicarboxylic acid and deionized water, and tetraazole and zinc salt Reacted in N,N-dimethylacetamide, conductive carbon black and binder are added to form a slurry, scraped onto the PP membrane and dried in vacuo to form a modified membrane with a double-channel structure.

Benefits of technology

It improves the transmission efficiency of lithium ions, reduces the shuttle effect, enhances the cycle stability and energy efficiency of the battery, is suitable for high-temperature and corrosive environments, and is simple in preparation process and low in cost, which is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009363A_ABST
    Figure CN119009363A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of lithium-sulfur batteries, and particularly relates to a Zn-Fe bimetal MOFs material modified diaphragm and a preparation method thereof. Comprising the following steps: preparing an MOFs material from FeCl2. 4H2O, 2, 2 '-bipyridine-5, 5'-dicarboxylic acid, tetrazole, tetrapropylammonium hydroxide and zinc salt through a solvothermal method; preparing the MOFs material into slurry; and blade-coating and drying to obtain the modified diaphragm. The method is suitable for being applied to a high-temperature or corrosive environment, the purity of the MOFs is high, the production cost is low, and the preparation process is simple. The prepared diaphragm can effectively induce transmission of lithium ions and also can adsorb LiPS, high catalytic activity sites accelerate kinetics of a redox reaction and promote proceeding of the reaction, the specific capacity of the first circle can reach 1587.6 mAh.g <-1 > under the rated capacitance of 0.1 C, the specific capacity is 695.3 mAh.g <-1 > after 70 cycles, and the coulombic efficiency is still close to 100%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium-sulfur batteries, and specifically relates to a Zn-Fe bimetallic MOFs material modified diaphragm and a preparation method thereof. Background Art

[0002] As a promising energy storage system, lithium-sulfur batteries have attracted much attention due to their high theoretical energy density and low cost. However, lithium-sulfur batteries face some challenges in practical applications, especially when the batteries work in high temperature or corrosive environments, these problems become more prominent. Traditional lithium-sulfur batteries are prone to performance degradation under high temperature conditions, mainly due to the aggravated sulfide shuttle effect, as well as the instability and corrosion of the internal components of the battery. In addition, the metal organic framework (MOFs) materials used in existing lithium-sulfur battery technology are often limited by purity and performance, which directly affects the cycle stability and overall performance of the battery. At the same time, the synthesis cost of some MOFs materials is high and the preparation process is complicated, making it difficult to meet the needs of large-scale production and commercial applications.

[0003] The document with application number "No. 202410329533.8" discloses "a Zn-Fe oxide heterojunction nanocomposite material derived from MOFs and its application", which combines aminoterephthalic acid with FeCl 3 6H 2 O was dissolved in dimethylformamide solution; ethanol solution was added dropwise to the above solution, mixed and then transferred into a reactor, heated for reaction, centrifuged and washed, and dried to obtain Fe-MOF precursor; the precursor and PVP were dissolved in methanol solution, mixed and then Zn(NO 3 ) 2 6H 2 O is stirred evenly to obtain a precursor solution; terephthalic acid is dissolved in a mixed solution of dimethylformamide / dimethyl sulfoxide; it is added dropwise to the precursor solution, transferred into a reactor for heating and reaction, and the white product is collected, centrifuged, washed, dried and annealed to obtain a MOFs-derived Fe-Zn oxide gas-sensitive material. The existing problems are: 1. The use of aminoterephthalic acid as a ligand for constructing bimetallic MOFs limits the complexity of the pore structure and the performance optimization space of MOFs; in addition, the insufficient chemical and thermal stability of aminoterephthalic acid under extreme conditions will affect the application of MOFs in high temperature or corrosive environments; 2. During the synthesis process, the precise coordination between the ligand and the metal node requires high requirements, and improper synthesis conditions are prone to by-product formation or structural defects, which in turn affect the purity and performance of MOFs. 3. Complex synthesis steps are required, including precise control of pyrolysis conditions, which increases production costs and difficulties. Summary of the invention

[0004] The purpose of the present invention is to prepare a Zn-Fe bimetallic MOFs material modified diaphragm to solve the problems of the prior art that it is not suitable for application in high temperature or corrosive environments, affects the purity and performance of MOFs, and has high production costs and difficulty.

[0005] To achieve the above object, the technical solution adopted by the present invention is: a method for preparing a Zn-Fe bimetallic MOFs material modified diaphragm, comprising the following steps:

[0006] Step 1: FeCl 2 ·4H 2 O, 2,2'-bipyridine-5,5'-dicarboxylic acid and deionized water are mixed and stirred, filtered and washed to obtain a powder;

[0007] Step 2: Weigh the powder and tetrazole and dissolve them in N,N-dimethylacetamide. Stir the solution until it is uniform at room temperature. Add tetrapropylammonium hydroxide and zinc salt and continue stirring until dissolved. React in a reactor, cool to room temperature, wash with N,N-dimethylacetamide, and dry to obtain a Zn-Fe bimetallic MOFs material.

[0008] Step 3: Add the Zn-Fe bimetallic MOFs material, conductive carbon black and binder into a glass bottle, mix well, and then add an appropriate amount of N-methyl-2-pyrrolidone solution and stir to form a uniform viscous slurry;

[0009] Step 4: Use anhydrous ethanol to clean the cut PP diaphragm, and use a scraper to evenly scrape the slurry obtained in step 3 on the PP diaphragm with a scraper. Vacuum dry the coated diaphragm to obtain a uniform modified diaphragm.

[0010] Furthermore, in the above step 1, FeCl 2 ·4H 2 The molar ratio of O and 2,2'-bipyridine-5,5'-dicarboxylic acid is 1:1, and the stirring time is 24h to 60h.

[0011] Furthermore, in the above step 2, the zinc salt is zinc acetate, zinc nitrate or zinc chloride.

[0012] Furthermore, in the above step 2, the molar ratio of the powder, tetrazole, tetrapropylammonium hydroxide and zinc salt is 1:1:1:1.

[0013] Furthermore, in the above step 2, the reaction temperature is 100-140° C., and the reaction time is 48-72 h.

[0014] Furthermore, in the above step 3, the mass ratio of the Zn-Fe bimetallic MOFs material, the conductive carbon black and the binder is 50-90:5-25:5-25, and the stirring time is 9-15h.

[0015] Furthermore, the conductive carbon black in the above step 3 is Super P, Ketjen black or acetylene black; the binder is carboxymethyl cellulose (CMC), polyvinylidene fluoride (PVDF) or polytetrafluoroethylene (PTFE).

[0016] Furthermore, in the above step 4, the vacuum drying temperature is 40° C. to 70° C., and the time is 5 h to 8 h.

[0017] Furthermore, the Zn-Fe bimetallic MOFs material modified diaphragm prepared by the above preparation method.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] (1) Zn-Fe bimetallic MOFs material has a one-dimensional columnar crystal structure: The present invention uses Zn-Fe bimetallic MOFs material to prepare a modified diaphragm. Zn-Fe bimetallic MOFs has a regular triangle and regular hexagonal double-channel nanoflower structure. The two independent channels can optimize the transmission paths of electrons and ions, promote faster charge transfer and diffusion of lithium ions, avoid the formation of lithium dendrites, and improve the rate performance and charge and discharge speed of the battery. In addition, the double-channel structure provides more surface and internal sites, which can more effectively adsorb and fix polysulfides, reduce their dissolution and migration in the electrolyte, thereby greatly reducing the shuttle effect and improving the cycle stability and energy efficiency of the battery; its crystal skeleton has high porosity and large double channels, which is Li + The transport of lithium ions provides a uniform and orderly channel, which can effectively induce the transport of lithium ions and avoid Li + Agglomeration occurs to prevent the growth of negative electrode lithium dendrites.

[0020] (2) Zn-Fe bimetallic MOFs materials have a double-channel crystal structure: Since the bipyridine structure can provide an additional conjugated π electron system, which helps to stabilize the entire molecular structure, the present invention selects 2,2'-bipyridine-5,5'-dicarboxylic acid and tetrazole to coordinate with metal ions to form a one-dimensional ordered double-channel nanoflower-shaped Zn-Fe bimetallic MOFs material. On the one hand, the larger pores can allow Li + On the other hand, the smaller pores can effectively block the shuttling of LiPS, especially medium to high-order LiPS (such as Li 2 S 4 -Li 2 S 8 ), these substances can easily shuttle through traditional separators, causing battery capacity decay.

[0021] (3) Zn-Fe bimetallic MOFs materials have catalytic conversion function: by 2+By precisely anchoring on 2,2'-bipyridine-5,5'-dicarboxylic acid, we successfully achieved Fe 2+ Precise positioning of Fe in Zn-Fe bimetallic MOFs 2+ and Zn 2+ The bimetallic MOFs with abundant catalytic active sites are composed of Fe 2+ It has a strong catalytic effect on LiPS conversion and effectively captures and converts dissolved LiPS through physical adsorption, inhibits the dissolution of LiPS, slows down the shuttle effect, and Zn 2+ The introduction of further regulates the catalytic center and synergistically enhances the catalytic effect. It prevents LiPS from shuttling to the negative electrode, thereby protecting the lithium metal negative electrode, reducing capacity attenuation, and improving the cycle stability and efficiency of the battery.

[0022] (4) The Zn-Fe bimetallic MOFs material can withstand a certain degree of thermal expansion without losing its integrity due to its ordered double-pore structure. The bimetallic combination of zinc and iron can optimize the electron distribution, which helps to reduce the local corrosion phenomenon inside the battery. Therefore, the present invention is suitable for application in high temperature or corrosive environments; due to the use of higher purity metal salts and ligands, the introduction of impurities can be reduced by optimizing the chemical structure and synthesis conditions, so that MOFs have higher purity, thereby significantly improving the purity of the material and enhancing the overall performance of the battery.

[0023] (5) The Zn-Fe bimetallic MOFs material provided by the present invention is prepared by a solvothermal method, which has mild reaction conditions, simple preparation process, low production cost, and is suitable for large-scale production. These characteristics make the material a potential ideal candidate material, which can significantly improve the applicability and economy of lithium-sulfur batteries in high temperature and corrosive environments, and open up a new path for the development of high-performance lithium-sulfur batteries in the future. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 is a preparation flow chart of Example 1;

[0025] Figure 2 is a morphology of the Zn-Fe bimetallic MOFs material prepared in Example 1 under an optical microscope;

[0026] Figure 3 This is a characterization diagram of the flexibility of the Zn-Fe bimetallic MOFs material modified diaphragm prepared in Example 1;

[0027] Figure 4 is a graph showing the relationship between current density and potential (CV) of the lithium-sulfur battery prepared in Example 1;

[0028] Figure 5 is the electrochemical impedance spectroscopy (EIS) of the lithium-sulfur battery prepared in Example 1;

[0029] Figure 6 This is a rate performance diagram of the lithium-sulfur battery prepared in Example 1 at different currents;

[0030] Figure 7 This is a relationship diagram between efficiency and specific capacity of the lithium-sulfur battery prepared in Example 1 after 70 cycles at a rated capacity of 0.1C;

[0031] like Figure 8 It is the conductivity of the lithium-sulfur battery prepared in Implementation Case 1-5 at room temperature. DETAILED DESCRIPTION

[0032] The present invention will be further described below in conjunction with specific embodiments.

[0033] Example 1: See Figure 1 , a method for preparing a Zn-Fe bimetallic MOFs material modified diaphragm comprises the following steps:

[0034] Step 1: Weigh 0.61 g of FeCl 2 ·4H 2 O, 0.5 g of 2,2'-bipyridine-5,5'-dicarboxylic acid and 50 mL of deionized water were added into a beaker and stirred for 24 h. The solution was filtered and washed with deionized water to obtain a pink powder;

[0035] Step 2: Weigh 0.172 g of powder and 0.04 g of tetrazole and dissolve them in 9 mL of N,N-dimethylacetamide. Stir the solution in a polytetrafluoroethylene reactor at room temperature until it is uniform. Then add 0.12 g of tetrapropylammonium hydroxide and 0.076 g of zinc acetate and continue stirring until dissolved. React at 120 ° C in the reactor for 2 days, cool to room temperature, wash three times with N,N-dimethylacetamide, and dry to obtain Zn-Fe bimetallic MOFs material;

[0036] Step 3: Weigh 0.07 g, 0.02 g and 0.01 g of the Zn-Fe bimetallic MOFs material, conductive carbon black (SuperP) and binder (PVDF) obtained in step 2, respectively, and add them into a glass bottle, mix them evenly, then add 1 mL of N-methyl-2-pyrrolidone solution and stir for 9 h to form a uniform viscous black slurry;

[0037] Step 4: Use anhydrous ethanol to clean the cut PP diaphragm, and use the scraping method to evenly scrape the black slurry obtained in step 3 on the surface of the PP diaphragm with a thickness of 75 μm. Transfer the coated diaphragm to a vacuum drying oven and dry it at 60°C for 12 hours to obtain a uniform black modified diaphragm.

[0038] Example 2: A method for preparing a Zn-Fe bimetallic MOFs material modified diaphragm, comprising the following steps:

[0039] Step 1: Weigh 0.61 g of FeCl 2 ·4H 2 O, 0.5 g of 2,2'-bipyridine-5,5'-dicarboxylic acid and 50 mL of deionized water were added into a beaker and stirred for 30 h. The solution was filtered and washed with deionized water to obtain a pink powder;

[0040] Step 2: Weigh 0.172 g of powder and 0.04 g of tetrazole and dissolve them in 12 mL of N, N-dimethylacetamide. In a polytetrafluoroethylene reactor, stir the solution at room temperature until it is uniform, then add 0.12 g of tetrapropylammonium hydroxide and 0.076 g of zinc acetate and continue stirring until dissolved. React at 120 ° C in the reactor for 2 days, cool to room temperature, wash three times with N, N-dimethylacetamide, and dry to obtain Zn-Fe bimetallic MOFs material;

[0041] Step 3: Weigh 0.08 g, 0.01 g and 0.01 g of the Zn-Fe bimetallic MOFs material, conductive carbon black (SuperP) and binder (PVDF) obtained in step 2 respectively and add them into a glass bottle, mix them evenly, then add 1 mL of N-methyl-2-pyrrolidone solution and stir for 10 h to form a uniform viscous black slurry;

[0042] Step 4: Use anhydrous ethanol to clean the cut PP diaphragm, and use the scraping method to evenly scrape the black slurry obtained in step 3 on the surface of the PP diaphragm with a thickness of 75 μm. Transfer the coated diaphragm to a vacuum drying oven and dry it at 50°C for 12 hours to obtain a uniform black modified diaphragm.

[0043] Example 3: A method for preparing a Zn-Fe bimetallic MOFs material modified diaphragm, comprising the following steps:

[0044] Step 1: Weigh 0.61 g of FeCl 2 ·4H 2 O, 0.5 g of 2,2'-bipyridine-5,5'-dicarboxylic acid and 50 mL of deionized water were added into a beaker and stirred for 35 h. The solution was filtered and washed with deionized water to obtain a pink powder;

[0045] Step 2: 0.172 g of powder and 0.04 g of tetrazole were dissolved in 9 mL of N, N-dimethylformamide. The solution was stirred at room temperature in a polytetrafluoroethylene reactor until uniform. 0.12 g of tetrapropylammonium hydroxide and 0.076 g of zinc acetate were added and continued to stir until dissolved. The mixture was reacted at 120 ° C in the reactor for 2 days, cooled to room temperature, washed three times with N, N-dimethylformamide, and dried to obtain a Zn-Fe bimetallic MOFs material.

[0046] Step 3: 0.07 g, 0.02 g and 0.01 g of the Zn-Fe bimetallic MOFs material, conductive carbon black (Ketjen black) and binder (PVDF) obtained in step 2 were weighed respectively and added into a glass bottle, mixed evenly, and then 1 mL of N-methyl-2-pyrrolidone solution was added and stirred for 11 h to form a uniform viscous black slurry;

[0047] Step 4: Use anhydrous ethanol to clean the cut PP diaphragm, and use the scraping method to evenly scrape the black slurry obtained in step 3 on the surface of the PP diaphragm with a thickness of 75 μm. Transfer the coated diaphragm to a vacuum drying oven and dry it at 60°C for 10 hours to obtain a uniform black modified diaphragm.

[0048] Example 4: A method for preparing a Zn-Fe bimetallic MOFs material modified diaphragm, comprising the following steps:

[0049] Step 1: Weigh 0.61 g of FeCl 2 ·4H 2 O, 0.5 g of 2,2'-bipyridine-5,5'-dicarboxylic acid and 50 mL of deionized water were added into a beaker and stirred for 24 h. The solution was filtered and washed with deionized water to obtain a pink powder;

[0050] Step 2: Weigh 0.172 g of powder and 0.04 g of tetrazole and dissolve them in 9 mL of N,N-dimethylacetamide. Stir the solution in a polytetrafluoroethylene reactor at room temperature until it is uniform. Then add 0.12 g of tetrapropylammonium hydroxide and 0.076 g of zinc acetate and continue stirring until dissolved. React at 120 ° C in the reactor for 3 days, cool to room temperature, wash three times with N,N-dimethylacetamide, and dry to obtain Zn-Fe bimetallic MOFs material;

[0051] Step 3: 0.07 g, 0.02 g and 0.01 g of the Zn-Fe bimetallic MOFs material, conductive carbon black (SuperP) and carboxymethyl cellulose (CMC) obtained in step 2 were weighed respectively and added into a glass bottle, mixed evenly, and then 1 mL of N-methyl-2-pyrrolidone solution was added and stirred for 9 h to form a uniform viscous black slurry;

[0052] Step 4: Use anhydrous ethanol to clean the cut PP diaphragm, and use the scraping method to evenly scrape the black slurry obtained in step 3 on the surface of the PP diaphragm with a thickness of 100 μm. Transfer the coated diaphragm to a vacuum drying oven and dry it at 70°C for 12 hours to obtain a uniform black modified diaphragm.

[0053] Example 5: A method for preparing a Zn-Fe bimetallic MOFs material modified diaphragm, comprising the following steps:

[0054] Step 1: Weigh 0.61 g of FeCl 2 ·4H 2 O, 0.5 g of 2,2'-bipyridine-5,5'-dicarboxylic acid and 50 mL of deionized water were added into a beaker and stirred for 50 h. The solution was filtered and washed with deionized water to obtain a pink powder;

[0055] Step 2: Weigh 0.172 g of powder and 0.04 g of tetrazole and dissolve them in 9 mL of N,N-dimethylformamide. Stir the solution in a polytetrafluoroethylene reactor at room temperature until it is uniform. Then add 0.12 g of tetrapropylammonium hydroxide and 0.076 g of zinc acetate and continue stirring until dissolved. React at 100 ° C in the reactor for 3 days, cool to room temperature, wash three times with N,N-dimethylformamide, and dry to obtain Zn-Fe bimetallic MOFs material;

[0056] Step 3: Weigh 0.07 g, 0.02 g and 0.01 g of the Zn-Fe bimetallic MOFs material, conductive carbon black (SuperP) and binder (PTFE) obtained in step 2, respectively, and add them into a glass bottle, mix them evenly, and then add 1 mL of N-methyl-2-pyrrolidone solution and stir for 15 h to form a uniform viscous black slurry;

[0057] Step 4: Use anhydrous ethanol to clean the cut PP diaphragm, and use the scraping method to evenly scrape the black slurry obtained in step 3 on the surface of the PP diaphragm with a thickness of 75 μm. Transfer the coated diaphragm to a vacuum drying oven and dry it at 40°C for 12 hours to obtain a uniform black modified diaphragm.

[0058] The modified diaphragm obtained in the above Examples 1-5 was taken out and cut into a circle with a diameter of 18 mm using a punch to obtain a modified battery diaphragm; the battery diaphragm E was assembled with a sulfur-loaded graphene composite positive electrode material and a negative electrode material lithium sheet in an argon-filled glove box with a shrapnel and a gasket into a lithium-sulfur battery, and the rate performance (0.1C, 0.3C, 0.5C, 1C, 2C, 3C current), impedance (frequency of 0.01-1000000 Hz), CV (1.6V-2.8V, scanning rate of 0.0005V / s), and conductivity were tested at different currents.

[0059] See also Figure 2 The morphology of the Zn-Fe bimetallic MOFs diaphragm material obtained in Example 1 is dumbbell-shaped.

[0060] See also Figure 3 By folding the membrane twice and then restoring it, it was found that no slurry fell off the surface of the membrane, indicating that the Zn-Fe bimetallic MOFs material membrane obtained in Example 1 has good flexibility.

[0061] like Figure 4 As shown in the figure, the relationship between current density and potential of the lithium-sulfur battery assembled with the modified diaphragm of Zn-Fe bimetallic MOFs material at a scan rate of 0.0005V / s. It can be seen from the figure that it has obvious redox peaks (I, II and III), showing the redox reaction of sulfur during the charge and discharge process of the material. Peak I shows S 8 Reduced to Li 2 S 6 , peak II shows Li 2 S 6 Reducing to Li 2 S 2 / Li 2 S, peak III shows Li 2 S 2 / Li 2 S is oxidized to S 8 , indicating that the material has excellent catalytic performance and can accelerate the catalytic conversion of LiPS

[0062] like Figure 5 As shown, it is the electrochemical impedance diagram of the lithium-sulfur battery assembled with the Zn-Fe bimetallic MOFs material modified diaphragm of the present invention. The impedance curve is mainly composed of two parts. In the high-frequency region, the impedance curve corresponding to the high-frequency region on the complex plane diagram is a semicircle. It can be seen from the figure that the semicircle radius of the material is small, indicating a lower electrode polarization impedance, which means that it allows fast electron / ion transfer to achieve interfacial LiPS conversion.

[0063] like Figure 6 The figure shows the rate of the lithium-sulfur battery assembled with the Zn-Fe bimetallic MOFs material modified diaphragm of the present invention. The rate diagram can be used to obtain the specific capacity of the lithium-sulfur battery at different currents. The specific capacities at 0.1C, 0.3C, 0.5C, 1C, and 3C are 1166.1 mAh g -1 、751.1mAh g -1 、649.5mAh g -1 , 509.2mAh g -1 、397.9mAh g -1 、321.6mAh g -1 .

[0064] like Figure 7 As shown in the figure, the specific capacity long cycle diagram of the lithium-sulfur battery assembled with the Zn-Fe bimetallic MOFs material modified diaphragm of the present invention, the first cycle specific capacity can reach 1587.6 mAh g at 0.1C -1 After 70 cycles, the specific capacity is 695.3 mAh g -1 , the Coulombic efficiency is still close to 100%.

[0065] like Figure 8 As shown, the room temperature conductivity of the lithium-sulfur battery assembled with the Zn-Fe bimetallic MOFs material modified diaphragm under different examples of the present invention, the conductivity of Example 1 is 2.304 mS·cm -1 The conductivity of Example 2 is 1.414 mS·cm -1 The conductivity of Example 3 is 1.387 mS·cm -1 The conductivity of Example 4 is 0.955 mS·cm -1 The conductivity of Example 5 is 0.662 mS·cm -1 .

[0066] In summary, embodiment 1 is the best embodiment.

[0067] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention are still within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a Zn-Fe bimetallic MOFs material modified diaphragm, characterized in that: The following steps are involved: Step 1: FeCl2·4H2O, 2,2'-bipyridine-5,5'-dicarboxylic acid and deionized water are mixed and stirred, and then filtered and washed to obtain a powder; Step 2: Weigh the powder and tetrazole and dissolve them in N,N-dimethylacetamide. Stir the solution until it is uniform at room temperature. Add tetrapropylammonium hydroxide and zinc salt and continue stirring until dissolved. React in a reactor, cool to room temperature, wash with N,N-dimethylacetamide, and dry to obtain a Zn-Fe bimetallic MOFs material. Step 3: Add the Zn-Fe bimetallic MOFs material, conductive carbon black and binder into a glass bottle, mix well, and then add an appropriate amount of N-methyl-2-pyrrolidone solution and stir to form a uniform viscous slurry; Step 4: Use anhydrous ethanol to clean the cut PP diaphragm, and use a scraper to evenly scrape the slurry obtained in step 3 on the PP diaphragm with a scraper. Vacuum dry the coated diaphragm to obtain a uniform modified diaphragm.

2. The method for preparing a Zn-Fe bimetallic MOFs material modified diaphragm according to claim 1, characterized in that: In the step 1, the molar ratio of FeCl2·4H2O to 2,2'-bipyridine-5,5'-dicarboxylic acid is 1:1, and the stirring time is 24 h to 60 h.

3. The method for preparing a Zn-Fe bimetallic MOFs material modified diaphragm according to claim 2, characterized in that: In the step 2, the zinc salt is zinc acetate, zinc nitrate or zinc chloride.

4. The method for preparing a Zn-Fe bimetallic MOFs material modified diaphragm according to claim 3, characterized in that: In the step 2, the molar ratio of the powder, tetrazole, tetrapropylammonium hydroxide and zinc salt is 1:1:1:

1.

5. The method for preparing a Zn-Fe bimetallic MOFs material modified diaphragm according to claim 4, characterized in that: In the step 2, the reaction temperature is 100-140° C. and the reaction time is 48-72 hours.

6. The method for preparing a Zn-Fe bimetallic MOFs material modified diaphragm according to claim 5, characterized in that: In the step 3, the mass ratio of the Zn-Fe bimetallic MOFs material, the conductive carbon black and the binder is 50-90:5-25:5-25, and the stirring time is 9-15 hours.

7. The method for preparing a Zn-Fe bimetallic MOFs material modified diaphragm according to claim 6, characterized in that: The conductive carbon black in step 3 is Super P, Ketjen black or acetylene black; the binder is carboxymethyl cellulose, polyvinylidene fluoride or polytetrafluoroethylene.

8. The method for preparing a Zn-Fe bimetallic MOFs material modified diaphragm according to claim 7, characterized in that: The vacuum drying in step 4 is performed at a temperature of 40° C. to 70° C. and for a time of 5 h to 8 h.

9. The Zn-Fe bimetallic MOFs material modified diaphragm prepared according to the preparation method of claim 1.

Citation Information

Patent Citations

  • Diaphragm based on MOF with nitrogen-rich column layer structure as well as preparation method and application of diaphragm

    CN114069159A

  • Metal-organic complex polymer derived nano material as well as preparation and application thereof

    CN115418000A

  • Preparation method of Zn-based dual-MOF modified diaphragm for lithium-sulfur battery as well as product and application of Zn-based dual-MOF modified diaphragm

    CN115810865A

  • Preparation method of lithium-sulfur battery based on phosphorus-based anion framework polymer diaphragm coating

    CN116169429A

  • Diaphragm and lithium ion battery containing diaphragm

    CN117954784A