Battery coating, battery, battery pack and electric equipment
By using modified inorganic materials and polymer materials in the lithium battery coating, combined with organic fibers, the adsorption capacity of transition metal ions is enhanced, and the problem of transition metal ions diffusion in lithium batteries is solved, and the battery life is extended. Improves stability and safety.
Patent Information
- Application Number
- CN202411496659.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-25
- Publication Date
- 2024-11-22
AI Technical Summary
The side reaction of the positive electrode material in lithium batteries causes the dissolution of transition metal ions to diffuse to the negative electrode surface, destroying the stability of the SEI film, affecting the battery capacity and safety performance, and the existing coating adsorption capacity is insufficient, affecting the battery service life.
Using the dual modification technology of matrix material and bonding material, the adsorption ability of transition metal ions is enhanced by using modified inorganic materials and polymer materials in the battery coating and combining organic fibers to prevent them from diffusing to the negative electrode surface. .
It significantly extends the service life of the battery, improves cycle stability and battery pack stability, reduces battery impedance, and enhances safety performance.
Smart Images

Figure CN119009374A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of batteries, and in particular to a battery coating, a battery, a battery pack, and an electrical device. Background Art
[0002] In lithium batteries, there are some side reactions on the surface of positive electrode materials such as nickel cobalt manganese oxide, nickel cobalt aluminum oxide, lithium manganese oxide, lithium iron manganese phosphate, and lithium-rich manganese, which will cause a small amount of transition metal to dissolve. In addition, during repeated charge and discharge, the structural changes of the positive electrode materials will also cause a small amount of transition metal to dissolve. The dissolved transition metal ions will diffuse to the surface of the negative electrode, destroy the stability of the SEI film on the surface of the negative electrode, cause irreversible decay of the battery capacity, and seriously affect the electrochemical performance and safety performance of the battery.
[0003] At present, by coating the surface of the diaphragm with a coating that adsorbs transition metal ions, the content of free transition metal ions in the electrolyte can be reduced and the diffusion of transition metal ions to the negative electrode surface can be restricted. However, the current coating has a weak ability to adsorb transition metals, and the dissolved transition metal ions will still slowly diffuse to the negative electrode surface, affecting the service life of the battery. Summary of the invention
[0004] The present invention provides a battery coating, in which the surfaces of a base material and a bonding material are simultaneously modified with adsorption groups, which can effectively improve the coating's ability to adsorb transition metals, prevent dissolved transition metal ions from slowly diffusing to the negative electrode surface, and thus extend the battery's service life.
[0005] The present invention also provides a battery comprising the battery coating, and the battery has excellent cycle stability.
[0006] The present invention also provides a battery pack comprising the battery, which has the advantages of good stability and long cycle life.
[0007] The present invention also provides an electrical device. Since the electrical device comprises the battery or battery pack, the service life of the electrical device is relatively long.
[0008] In a first aspect, the present invention provides a battery coating, comprising a base material modified by a first group and a bonding material modified by a second group, wherein the base material is an inorganic material and / or a high molecular polymer material, and the bonding material comprises organic fibers; the first group and the second group are used to adsorb transition metal ions.
[0009] Furthermore, the transition metal ion is at least one of nickel ion, cobalt ion and manganese ion.
[0010] Furthermore, the first group and the second group are each independently one or more of -OH, -CN, -NO2, -NH2, -COOH, -COOLi, -H2PO4, -LiHPO4, -LiHPO4, -SO3H, -SO3Li.
[0011] Furthermore, the first group accounts for 0.1wt%-1wt% of the mass of the matrix material; and the second group accounts for 0.1wt%-1wt% of the mass of the bonding material.
[0012] Furthermore, the material of the organic fiber is one or more of cellulose, chitin, polyimide, polyacrylonitrile, poly(p-phenylene benzobisoxazole), para-aramid, and meta-aramid; And / or, the inorganic material is one or more of alumina, boehmite, boron nitride, silicon carbide, silicon nitride, zinc oxide, titanium dioxide, silicon dioxide, and zirconium dioxide.
[0013] Furthermore, the organic fiber has a diameter of 2nm~100nm and a length of 1μm~100μm; And / or, the inorganic material is in granular form, and its particle size is 0.2 μm to 2 μm; And / or, the organic material is in at least one of a linear, fibrous, and rod-like shape, with a diameter of 10 nm to 1000 nm and a length of 1 μm to 100 μm; And / or, the specific surface area of the inorganic material is 0.5m 2 / g~1000m 2 / g.
[0014] Furthermore, the high molecular polymer includes one or more of polystyrene, polymethyl methacrylate, polyethylene, and polypropylene.
[0015] Furthermore, the specific surface area of the polymer material is 0.5 m 2 / g~1000m 2 / g; And / or, the polymer material is in granular form, and its particle size is 0.2 μm to 2 μm; And / or, the high molecular polymer material is at least one of linear, fibrous, and rod-shaped, with a diameter of 10 nm to 1000 nm and a length of 1 μm to 100 μm.
[0016] Furthermore, the mass ratio of the inorganic material, the high molecular polymer material and the organic fiber is 0~100:0~100:1~10; wherein the masses of the inorganic material and the high molecular polymer material are not 0 at the same time.
[0017] Further, the battery coating is disposed on at least one surface of the positive electrode, and / or, on at least one surface of the negative electrode, and / or, on at least one surface of the separator.
[0018] Furthermore, the battery coating has a thickness of 0.5 μm to 5 μm.
[0019] In a second aspect, the present invention provides a battery comprising the coating of the battery of the first aspect.
[0020] In a third aspect, the present invention provides a battery pack comprising the battery described in the second aspect.
[0021] In a fourth aspect, the present invention provides an electrical device, comprising the battery described in the second aspect or the battery pack described in the third aspect.
[0022] The battery coating of the present invention has excellent ability to adsorb transition metal ions, which can prevent the dissolved transition metal ions from slowly diffusing to the negative electrode surface, thereby extending the service life of the battery. In addition, the battery coating has a low swelling rate in the electrolyte, which can reduce the impact on the battery impedance. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the technical solutions in the embodiments of the present invention or related technologies, the following briefly introduces the drawings required for use in the embodiments of the present invention or related technologies. Obviously, the drawings described below are only some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0024] Figure 1 This is a schematic diagram of the adsorption of transition metal ions by a battery coating according to a specific embodiment of the present invention. DETAILED DESCRIPTION
[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] In a first aspect, the present invention provides a battery coating, comprising a base material modified by a first group and a bonding material modified by a second group, wherein the base material is an inorganic material and / or a high molecular polymer material, and the bonding material comprises organic fibers, and the first group and the second group are used to adsorb transition metal ions.
[0027] The battery coating of the present invention has excellent ability to adsorb transition metal ions, which can prevent the dissolved transition metal ions from slowly diffusing to the negative electrode surface, thereby extending the service life of the battery. In addition, the battery coating has a low swelling rate in the electrolyte, which can reduce the impact on the battery impedance. The main reasons include: on the one hand, the existing battery coating is usually composed of inorganic materials, dispersants, and binders, and common binders are easily coated on the surface of inorganic materials, such as polyvinyl pyrrolidone, polyacrylic acid, polyvinylidene fluoride, etc., thereby covering the groups on the surface of the inorganic material that play an adsorption role, weakening the overall adsorption capacity of the coating, and the patent uses organic fibers to replace conventional binders in batteries, which can effectively prevent the groups on the surface of the base material from being covered. At the same time, since the organic fiber is modified by the second group, it can adsorb transition metal ions together with the base material, thereby providing double protection to prevent the dissolved transition metal ions from diffusing to the surface of the negative electrode; on the other hand, the existing binder may swell in the electrolyte, which will reduce the porosity of the battery coating during the long cycle of the battery, thereby affecting the migration of lithium ions between the positive and negative electrodes, resulting in an increase in the battery impedance, and the organic fiber of the present invention has a lower swelling rate in the electrolyte, is not easy to be transformed into a gel in the electrolyte, and the porosity of the battery coating does not change much during the long cycle of the battery, so the impact on the ion migration between the positive and negative electrodes is smaller, which can avoid the increase in battery impedance to a certain extent.
[0028] In some embodiments, the transition metal ion is at least one of a nickel ion, a cobalt ion, and a manganese ion.
[0029] The battery coating as described above can adsorb at least one of Ni ions, Co ions and Mn ions, so at least part of the transition metal will be adsorbed by the adsorption coating and cannot reach the surface of the negative electrode sheet, thereby reducing the content of transition metal deposited on the negative electrode sheet when the battery is overcharged, reducing the degree of reaction between the transition metal and the electrolyte and the battery temperature, thereby improving the stability and safety of the battery.
[0030] It should be noted that when the matrix material includes both an inorganic material and a high molecular polymer material, the first groups modified by the two materials may be the same or different.
[0031] In some embodiments, the first group and the second group are each independently one or more of -OH, -CN, -NO2, -NH2, -COOH, -COOLi, -H2PO4, -LiHPO4, -LiHPO4, -SO3H, -SO3Li. When the battery coating includes the first group and the second group as described above, the ability of the battery coating to adsorb transition metal ions can be further improved.
[0032] As for the matrix material modified by the first group and the organic fiber modified by the second group, they can be purchased directly from the market or prepared by referring to the existing technology. For example, they can be prepared by a method including the following process: mixing the matrix material with at least one strong oxidant such as concentrated sulfuric acid, concentrated nitric acid, hydrogen peroxide, potassium permanganate, etc., modifying the surface of the matrix material with -SO3H, -NO2, -OH, etc. by adjusting the reaction temperature and time, and then utilizing the reactive properties of the -SO3H, -NO2, -OH and other groups to obtain the matrix material modified with -CN, -NH2, -COOH, -COOLi, -H2PO4, -LiHPO4, -LiHPO4 through chemical reaction.
[0033] In one specific embodiment, the surface of the organic fiber is modified with -NH2 and -COOH, the bonding material is in a granular form, and the surface is modified with -OH and -COOH. The schematic diagram of the battery coating adsorbing transition metal (manganese) ions is shown in FIG. Figure 1 shown.
[0034] The present invention does not specifically limit the modification amount of the first group in the matrix material. In some embodiments, the amount of the first group in the matrix material is 0.1-1wt%; the present invention does not specifically limit the modification amount of the second group in the organic fiber. In some embodiments, the amount of the second group in the organic fiber is 0.1-1wt%.
[0035] In a specific embodiment, the first group includes at least one of -SO3H, -NO2, and -OH, and includes at least one of -CN, -NH2, -COOH, -COOLi, -H2PO4, -LiHPO4, and -LiHPO4.
[0036] Exemplarily, the mass content of the first group or the second group modified on the surface of the matrix material or the organic fiber can be tested by the following method: A certain mass of matrix material or organic fiber is taken and tested using a thermogravimetric analyzer. The test parameters are: in a nitrogen atmosphere, the temperature is increased from 30°C to 200°C at a rate of 10°C / min, and it is allowed to stand at 200°C for 10 minutes. The mass ratio of the first group or the second group on the surface to the matrix material or organic fiber is calculated based on the weight loss rate.
[0037] In some embodiments, the material of the organic fiber is one or more of cellulose, chitin, polyimide, polyacrylonitrile, poly(p-phenylene benzobisoxazole), para-aramid, and meta-aramid; And / or, the inorganic material is one or more of alumina, boehmite, boron nitride, silicon carbide, silicon nitride, zinc oxide, titanium dioxide, silicon dioxide, and zirconium dioxide. The organic fiber described above has a lower swelling rate in the electrolyte, which can further avoid the increase of battery impedance. The inorganic material described above has high mechanical strength and thermal stability, which can effectively block heat conduction, reduce the temperature gradient inside the battery, and prevent local overheating.
[0038] In some embodiments, the diameter of the organic fiber is 2 nm to 100 nm, and the length is 1 μm to 100 μm. The organic fiber of this size can further ensure that the groups on the surface of the matrix material are not covered.
[0039] Exemplarily, the diameter of the organic fiber is any value among 5 nm, 8 nm, 10 nm, 12 nm, 15 nm, 17 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, 55 nm, 60 nm, 65 nm, 70 nm, 75 nm, 80 nm, 85nm, 90 nm, 95 nm, etc., and the length of the organic fiber is any value among 1μm, 5μm, 10μm, 15μm, 2μm, 25μm, 30μm, 35μm, 40μm, 45μm, 50μm, 55μm, 60μm, 65μm, 70μm, 75μm, 80μm, 85μm, 90μm, 95μm, etc.
[0040] For example, the size of the fiber can generally be tested according to the fiber diameter by selecting an optical microscope, a scanning electron microscope, a transmission electron microscope, etc. Specifically, a microscopic morphology image of the fiber is first taken, and then a fiber diameter analysis software such as imagej, Simpleware, UV-TXW and other image analysis software is used to calculate the fiber diameter and length.
[0041] In some embodiments, the inorganic material is in a granular form, and its particle size is 0.2 μm to 2 μm; wherein, the granular inorganic material of this size can be more evenly distributed in the battery coating to form a dense and uniform structure.
[0042] Illustratively, the particle size of the granular inorganic material is 0.5 μm, 0.7 μm, 1 μm, 1.2 μm, 1.5 μm, 1.7 μm, 1.9 μm, etc.
[0043] In some embodiments, the inorganic material is at least one of linear, fibrous, and rod-shaped, with a diameter of 10nm~1000nm and a length of 1μm~100μm; wherein, linear, fibrous, and rod-shaped inorganic materials of this size can enhance the mechanical strength of the battery coating and improve its durability.
[0044] Exemplarily, the diameter of the inorganic material is 20 nm, 30 nm, 40 nm, 5 nm, 60 nm, 70 nm, 90 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, 600 nm, 700nm, 800 nm, 900 nm, etc.; the length of the inorganic material is 1 μm, 5 μm, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, etc.
[0045] In a specific embodiment, at least one of linear, fibrous, and rod-shaped inorganic materials is used, and the linear, fibrous, and rod-shaped inorganic materials are compounded with organic fibers to form a mesh coating. When the diaphragm / base film shrinks under high temperature, compared with a coating of mainly granular inorganic materials, the mesh coating is more inclined to form a complete mesh structure rather than coating fragments, which can effectively prevent short circuits between the positive and negative electrodes.
[0046] In some embodiments, the specific surface area of the inorganic material is 0.5 m 2 / g~1000m 2 / g.
[0047] Exemplarily, the specific surface area of the inorganic material is 10 m 2 / g, 20 m 2 / g, 50 m 2 / g, 80 m 2 / g、100m 2 / g, 150 m 2 / g, 200 m 2 / g, 250 m 2 / g, 300 m 2 / g, 350 m 2 / g, 400 m 2 / g, 450 m 2 / g, 500 m 2 / g、600m 2 / g, 700 m 2 / g, 800 m 2 / g, 900 m 2 / g, etc.
[0048] In some embodiments, the high molecular polymer includes one or more of polystyrene, polymethyl methacrylate, polyethylene, and polypropylene.
[0049] Among them, adding the above polymer materials to the battery coating can increase the interfacial adhesion between the battery coating and the electrode, thereby improving the hardness of the soft-pack battery. In addition, the above polymer materials have a certain melting point range and can also play a role of thermal closure in the battery coating.
[0050] In some embodiments, the specific surface area of the high molecular polymer material is 0.5 m 2 / g~1000m 2 / g; And / or, the polymer material is in granular form, and its particle size is 0.2 μm to 2 μm; And / or, the polymer material is at least one of linear, fibrous, and rod-shaped, with a diameter of 10nm to 1000nm and a length of 1μm to 100μm. The linear, fibrous, and rod-shaped polymer material of this size can enhance the mechanical strength of the battery coating and improve its durability.
[0051] Exemplarily, the particle size of the granular polymer material is 0.5μm, 0.7μm, 1μm, 1.2μm, 1.5μm, 1.7μm, 1.9μm, etc.; the diameter of the linear, fibrous, and rod-shaped polymer materials is 20 nm, 30 nm, 40nm, 5 nm, 60 nm, 70 nm, 90 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm, etc.; the length of the inorganic material is 1μm, 5μm, 10μm, 20μm, 30μm, 40μm, 50μm, 60μm, 70μm, 80μm, 90μm, etc.
[0052] In a specific embodiment, at least one of linear, fibrous, and rod-shaped materials is used, and the linear, fibrous, and rod-shaped inorganic materials are compounded with organic fibers to form a mesh coating. When the separator / base film shrinks under high temperature, the mesh coating is more inclined to form a complete mesh structure rather than coating fragments, compared with linear, fibrous, and rod-shaped coatings which are mainly granular, thereby effectively preventing short circuits between the positive and negative electrodes.
[0053] In order to take into account both the cost and the lithium ion permeability of the battery coating, in some embodiments, the mass ratio of the inorganic material, the high molecular polymer material and the organic fiber is 0~100:0~100:1~10; wherein the masses of the inorganic material and the high molecular polymer material are not 0 at the same time.
[0054] In a specific embodiment, the mass ratio of the inorganic material, the high molecular polymer material and the organic fiber is 100:1~10:1~10.
[0055] In a specific embodiment, the mass ratio of the inorganic material, the high molecular polymer material and the organic fiber is 100:1~5:1~10.
[0056] In a specific embodiment, the mass ratio of the inorganic material to the organic fiber is 100:1-10.
[0057] In a specific embodiment, the mass ratio of the high molecular polymer material to the organic fiber is 100:1-10.
[0058] In some embodiments, the battery coating is disposed on at least one surface of the positive electrode, and / or, disposed on at least one surface of the negative electrode, and / or, disposed on at least one surface of the separator.
[0059] In some embodiments, the battery coating has a thickness of 0.5 μm to 5 μm.
[0060] Exemplarily, the thickness of the battery coating can be tested with reference to the national standard GB / T 36363-2018.
[0061] The battery coating of the present invention can be applied to any element of the battery, including the positive electrode sheet, the negative electrode sheet and the diaphragm. When the battery coating is arranged on the surface of the diaphragm, the thermal stability of the diaphragm can be improved, and the safety performance of the battery can be improved.
[0062] In a specific embodiment, the battery coating is coated on one or more surfaces of the positive electrode, the negative electrode or the separator by dipping, spraying, spin coating or roller coating; In a second aspect, the present invention provides a battery comprising the coating of the battery of the first aspect.
[0063] As for the composition and material of the positive electrode, negative electrode and separator of the battery, the present invention does not make any special limitation. Exemplarily, the above-mentioned negative electrode sheet includes a current collector and a negative electrode active material layer located on at least one surface of the current collector, the negative electrode active material layer includes a negative electrode active material, a conductive agent and a binder, the negative electrode active material includes one or more of graphite, hard carbon, soft carbon, silicon-based negative electrode, titanium-based material, nitride, tinide, and metallic lithium. The negative electrode current collector can be a conventional negative electrode current collector in the art, for example, including copper foil, etc. The mass fraction of the negative electrode active material in the negative electrode active layer is 92%-98%, the mass fraction of the binder is 0.5%-3%, and the mass fraction of the conductive agent is 0.5%-2.5%. The positive electrode sheet comprises a current collector and a positive electrode active material layer located on at least one surface of the current collector, the positive electrode active material layer comprises a positive electrode active material, a conductive agent and a binder, the positive electrode active material comprises at least one of lithium cobalt oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium manganese phosphate, lithium iron phosphate and lithium manganese iron phosphate; the material of the current collector is not specifically limited in the present invention, for example, it can be selected from any one or more of copper foil, titanium foil, tin foil, chromium foil and composite foils of the above metals; the conductive agent can be selected from natural graphite , artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, carbon nanotubes, metal powder, and graphene; the binder can be selected from at least one of carboxymethyl cellulose, styrene-butadiene rubber, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamide-imide, polyvinyl alcohol, and sodium polyacrylate; the dispersant can be selected from at least one of sodium carboxymethyl cellulose, triethylhexyl phosphoric acid, and sodium dodecyl sulfate.
[0064] The battery of the present invention can be manufactured according to conventional methods in the art, such as stacking the positive electrode sheet, the separator, and the negative electrode sheet in sequence, assembling the battery cell through a winding process or a stacking process, and then packaging and baking, injecting the electrolyte, and then hot pressing and other processes to obtain the battery.
[0065] Exemplarily, the battery may further include a diaphragm. The present invention does not particularly limit the material of the diaphragm, and any known porous structure diaphragm with electrochemical stability and chemical stability may be selected, for example, it may be at least one of glass fiber, non-woven fabric, polyethylene, polypropylene or polyvinylidene fluoride. The diaphragm may be single-layer or multi-layer.
[0066] The present invention does not specifically limit the above-mentioned electrolyte, for example, an electrolyte including an organic solvent and an electrolyte salt is selected. Among them, the organic solvent is used as a medium for transmitting ions in the electrochemical reaction, and can be an organic solvent for battery electrolyte known in the art, such as: one or more of fluorinated carbonates, fluorinated carboxylates, non-fluorinated carbonates, fluorinated carbonates, non-fluorinated carboxylates, fluorinated carboxylates, fluorinated carboxylates, fluorinated ethers, non-fluorinated ethers, and tetrahydrofuran; the electrolyte salt is used as a source of ions, and can be an electrolyte salt for battery electrolyte known in the art, such as: one or more of lithium hexafluorophosphate, bistrifluoromethylsulfonyl imide, and bis(fluorosulfonyl)imide lithium.
[0067] In a third aspect, the present invention provides a battery pack comprising the battery described in the second aspect.
[0068] In a fourth aspect, the present invention provides an electrical device, comprising the battery described in the second aspect or the battery pack described in the third aspect.
[0069] It should be noted that the above-mentioned electrical equipment can be any conventional equipment that requires electricity, for example, including but not limited to computers, electric cars, air conditioners, refrigerators, washing machines, microwave ovens, printers, fax machines, etc.
[0070] The technical scheme of the present invention is further illustrated below in conjunction with specific examples. All parts, percentages and ratios described in the following examples are based on weight, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further treatment, and the instruments used in the examples are commercially available.
[0071] Example 1 This example provides a battery coating and a battery including the battery coating. The battery coating includes: aluminum oxide particles with a surface modification of 0.1wt% -OH, with a particle size of 1 μm and a specific surface area of 10 m 2 / g; cellulose fibers with 0.4 wt%-SO3H surface modification, with a diameter of 10nm and a length of 10μm; polymethyl methacrylate particles with 0.5wt%-COOH surface modification, with a particle size of 0.5μm and a specific surface area of 90m 2 / g; the mass ratio of alumina particles: polymethyl methacrylate particles: cellulose fibers is 100:10:3, the thickness of the battery coating is 2μm, and the surface density is 3g / m 2 .
[0072] The battery comprises a positive electrode sheet, a negative electrode sheet and a separator, wherein the separator comprises a separator substrate and the battery coating coated on a side of the separator substrate close to the negative electrode, and the separator substrate is a PE separator.
[0073] The preparation method of the battery comprises: mixing artificial graphite (99.5%), conductive carbon black SP (99.6%), adhesive SBR (99.9%), and dispersant CMC (99.5%) in a mass ratio of 95:1:2:2, slurrying with water as solvent, coating on a 9µm thick copper foil, and the coating surface density is 170g / m 2 The ZY400-A45 battery pole piece automatic rolling equipment is used to roll the pole piece into a thickness of 105µm (the compaction density is 1.6g / cm 3 ), and then cut it into 40mm (width) × 400mm (length) negative electrode sheets for standby use using a P50-HLP-20 laser cutting machine; Lithium manganese iron phosphate, carbon nanotubes, adhesive PVDF, and dispersant PVP were mixed in a mass ratio of 100:2:4:0.2, slurried with NMP as solvent, and coated on a 12µm thick aluminum foil with a coating surface density of 360g / m 2 The ZY400-A45 battery pole piece automatic rolling equipment is used to roll the pole piece into a thickness of 170µm (the compaction density is 2.2g / cm 3 ), and then cut it into 40mm (width) × 400mm (length) negative electrode sheets for standby use using a P50-HLP-20 laser cutting machine; The positive electrode, separator and negative electrode sheets are stacked in sequence to form a "sandwich" structure to form a battery cell that can be encapsulated, and finally the battery cell is assembled in a battery shell.
[0074] Example 2 This example provides a battery coating and a battery comprising the battery coating. The battery coating comprises: boehmite particles with a surface modification of 0.1 wt % -OH, with a particle size of 1 μm and a specific surface area of 10 m 2 / g; para-aramid fibers with a surface modification of 0.4 wt% -NH2, with a diameter of 10 nm and a length of 10 μm; polyethylene particles with a surface modification of 0.5 wt% -COOH, with a particle size of 0.5 μm and a specific surface area of 90 m 2 / g; the mass ratio of boehmite particles, polyethylene particles, and para-aramid fibers is 100:5:4, the thickness of the battery coating is 3μm, and the surface density is 3.5g / m 2 .
[0075] The battery comprises a positive electrode sheet, a negative electrode sheet and a separator, wherein the separator comprises a separator substrate and a battery coating coated on a side of the separator substrate close to the positive electrode. The preparation method of the battery is as described in Example 1.
[0076] Example 3 This example provides a battery coating and a battery including the battery coating, wherein the battery coating includes: an inorganic material modified by a first group, an organic fiber modified by a second group, and a silicon carbide fiber with a surface modification of 1 wt% -OH, a diameter of 50 nm, a length of 20 μm, and a specific surface area of 100 m 2 / g; cellulose fibers with 0.4 wt%-COOLi surface modification, with a particle size of 10nm and a length of 10 μm; the mass ratio of silicon carbide fiber to cellulose fiber is 100:3, the thickness of the battery coating is 2μm, and the surface density is 2.2g / m 2 .
[0077] The battery comprises a positive electrode sheet, a negative electrode sheet and a separator, and one side of the positive electrode sheet comprises the battery coating. The preparation method of the battery is as described in Example 1.
[0078] Example 4 This example provides a battery coating and a battery including the battery coating, wherein the battery coating includes: a para-aramid fiber with a surface modification of 0.4 wt% -NH2, a diameter of 10 nm and a length of 10 μm; a polymethyl methacrylate particle with a surface modification of 0.5 wt% -COOH, a particle size of 0.5 μm and a specific surface area of 90 m 2 / g; the mass ratio of polymethyl methacrylate particles: para-aramid fiber is 100:4, the thickness of the battery coating is 3μm, and the surface density is 3.5g / m 2 .
[0079] The battery comprises a positive electrode sheet, a negative electrode sheet and a separator, wherein the separator comprises a separator substrate and a battery coating coated on a side of the separator substrate close to the positive electrode. The preparation method of the battery is as described in Example 1.
[0080] Comparative Example 1 This example provides a battery coating and a battery comprising the battery coating. The battery coating comprises: aluminum oxide particles with a surface modification of 0.1wt% -OH, with a particle size of 1 μm and a specific surface area of 10 m 2 / g; polymethyl methacrylate particles with 0.5 wt% -COOH modified on the surface, with a particle size of 0.5 μm and a specific surface area of 90 m 2 / g; the mass ratio of aluminum oxide particles to polymethyl methacrylate particles is 100:10, the binder is polyacrylic acid, the mass ratio of aluminum oxide particles to the binder is 100:3, and the thickness of the battery coating is 2 μm.
[0081] The battery comprises a positive electrode sheet, a negative electrode sheet and a separator, wherein the separator comprises a separator substrate and a battery coating coated on a side of the separator substrate close to the negative electrode. The preparation method of the battery is as described in Example 1.
[0082] Test Case Test 1: Transition metal ion content test in the negative electrode After the battery was cycled 500 times at 45° C., the battery was disassembled, and the negative electrode was cleaned with a salt-free electrolyte solvent. After drying, the negative electrode was subjected to an ICP (inductively coupled plasma spectrometer) test; the test results are shown in Table 1.
[0083] Test 2: Battery capacity retention test The battery was cycled 1000 times at 25°C and 1C rate. The ratio of the capacity after the cycle to the initial capacity is the capacity retention rate. The test results are shown in Table 1.
[0084] Table 1:
[0085] It can be seen from Table 1 that, compared with the comparative example, the battery of the embodiment has a lower content of transition metal ions in the negative electrode and a better cycle performance.
[0086] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A battery coating, characterized in that: It comprises a base material modified by a first group and a bonding material modified by a second group, wherein the base material is an inorganic material and / or a high molecular polymer material, and the bonding material comprises organic fiber; the first group and the second group are used for adsorbing transition metal ions.
2. The battery coating according to claim 1, characterized in that: The transition metal ion is at least one of nickel ion, cobalt ion and manganese ion.
3. The battery coating according to claim 1 or 2, characterized in that: The first group and the second group are each independently one or more of -OH, -CN, -NO2, -NH2, -COOH, -COOLi, -H2PO4, -LiHPO4, -LiHPO4, -SO3H, -SO3Li.
4. The battery coating according to claim 3, characterized in that: The first group accounts for 0.1wt%-1wt% of the mass of the matrix material; the second group accounts for 0.1wt%-1wt% of the mass of the bonding material.
5. The battery coating according to claim 1, characterized in that: The material of the organic fiber is one or more of cellulose, chitin, polyimide, polyacrylonitrile, poly(p-phenylene benzobisoxazole), para-aramid, and meta-aramid; And / or, the inorganic material is one or more of alumina, boehmite, boron nitride, silicon carbide, silicon nitride, zinc oxide, titanium dioxide, silicon dioxide, and zirconium dioxide.
6. The battery coating according to claim 5, characterized in that: The organic fiber has a diameter of 2nm~100nm and a length of 1μm~100μm; And / or, the inorganic material is in granular form, and its particle size is 0.2 μm to 2 μm; And / or, the organic material is in at least one of a linear, fibrous, and rod-like shape, with a diameter of 10 nm to 1000 nm and a length of 1 μm to 100 μm; And / or, the specific surface area of the inorganic material is 0.5 m 2 / g~1000 m 2 / g.
7. The battery coating according to claim 1, characterized in that: The high molecular polymer includes one or more of polystyrene, polymethyl methacrylate, polyethylene and polypropylene.
8. The battery coating according to claim 7, characterized in that: The specific surface area of the high molecular polymer material is 0.5 m 2 / g~1000 m 2 / g; And / or, the polymer material is in granular form, and its particle size is 0.2 μm to 2 μm; And / or, the high molecular polymer material is in at least one of a linear, fibrous, and rod-like shape, with a diameter of 10 nm to 1000 nm and a length of 1 μm to 100 μm.
9. The battery coating according to any one of claims 4 to 8, characterized in that: The mass ratio of the inorganic material, the high molecular polymer material and the organic fiber is 0-100:0-100:1-10; wherein the masses of the inorganic material and the high molecular polymer material are not 0 at the same time.
10. The battery coating according to claim 1, characterized in that: The battery coating is disposed on at least one surface of the positive electrode, and / or, on at least one surface of the negative electrode, and / or, on at least one surface of the separator.
11. The battery coating according to claim 10, characterized in that: The thickness of the battery coating is 0.5 μm to 5 μm.
12. A battery, characterized in that: The battery coating comprises the battery coating described in any one of claims 1-11.
13. A battery pack, characterized in that: Comprising the battery of claim 12.
14. Electrical equipment, characterized in that: Includes the battery according to claim 12 or the battery pack according to claim 13.
Citation Information
Patent Citations
Diaphragm slurry, battery diaphragm, preparation method and lithium battery
CN115579583A
Diaphragm and battery
CN116365162A
Separator for Lithium Secondary Battery Containing Coating Layers of Different type
KR1020160097537A
Cited By
Diaphragm and preparation method thereof, battery and electric device