Jelly roll type electrode assembly, secondary battery, and method for manufacturing electrode assembly
By placing the exposed negative current collector in the central region of the jelly roll electrode assembly and adjusting the winding order of the positive and negative electrodes, the gap problem between the application start points of the positive and negative active materials was solved, increasing the capacity and reducing the resistance.
Patent Information
- Application Number
- CN202411037262.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2019-10-07
- Filing Date
- 2020-10-07
- Publication Date
- 2024-11-22
AI Technical Summary
In the prior art, the gap between the starting point of the positive electrode active material application and the starting point of the negative electrode active material application in the manufacturing process of the jelly roll type electrode assembly leads to capacity loss and safety issues, and the excessively long welding distance of the negative electrode terminal increases the resistance.
By placing the exposed portion of the negative current collector in the central area where winding begins and connecting the negative terminal piece to this location, while adjusting the winding sequence of the positive and negative terminals, the length of the positive terminal piece is increased and the length of the negative terminal piece is decreased to reduce resistance.
This allows for increased electrode assembly capacity without compromising safety, and reduced welding distance of the negative terminal piece, thereby lowering resistance.
Smart Images

Figure CN119009387A_ABST
Abstract
Description
[0001] Divisional application
[0002] This application is a divisional application of the Chinese patent application with application date of October 7, 2020, application number 202080063085.1, and invention name “Electrode assembly and manufacturing method thereof”.
[0003] CROSS-REFERENCE TO RELATED APPLICATIONS
[0004] This application claims the benefit of priority to Korean Patent Application No. 10-2019-0124206, filed on October 7, 2019, which is hereby incorporated by reference in its entirety. Technical Field
[0005] The present invention relates to an electrode assembly and a method for manufacturing the electrode assembly, and more specifically to: an electrode assembly in which the gap between the point where application of a positive electrode active material starts and the point where application of a negative electrode active material starts in the central region (in the starting end) of a jelly-roll type electrode assembly manufactured in a cylindrical shape can be reduced, thereby increasing the capacity (capable of providing a space capable of increasing the length of the distal end of the positive electrode); and a method for manufacturing the electrode assembly. Background Art
[0006] Batteries for storing electrical energy can be generally classified into primary batteries and secondary batteries. Primary batteries are disposable consumer batteries, but on the other hand, secondary batteries are rechargeable batteries manufactured by using materials that can repeatedly perform oxidation and reduction processes between electric current and substances. That is, when a reduction reaction is performed on the material by electric current, the power is recharged. And, when an oxidation reaction is performed on the material, the power is discharged. Such recharging and discharging can be performed repeatedly.
[0007] Among various types of secondary batteries, lithium secondary batteries are generally manufactured by mounting an electrode assembly in which a positive electrode (cathode), a separator, and a negative electrode (anode) are stacked to a housing. Recharging and discharging of lithium secondary batteries are performed while lithium ions are repeatedly intercalated and deintercalated from lithium metal oxide of the positive electrode into and from the negative electrode.
[0008] Moreover, as methods for manufacturing an electrode assembly, a jelly roll (winding) method, a stacking method, a stacking and folding method, and the like are well known. In the jelly roll (winding) method, a separator is stacked between a negative electrode and a positive electrode and then rolled up. In the stacking method, a negative electrode and a positive electrode are cut into a desired width and length, and then the negative electrode, the separator, and the positive electrode are repeatedly stacked. In the stacking and folding method, unit cells are placed side by side on a folding separator and then folded from one side.
[0009] In the electrode assembly, a jelly-roll type electrode assembly is manufactured by winding the cathode 4 , the separator 2 , and the anode 3 together around the winding core 1 .
[0010] In this article, as in Figure 1A As shown in FIG. 1 , separators 2a and 2b are first input to the winding core 1, and then the negative electrode 3 and the positive electrode 4 are sequentially input. That is, in the method for manufacturing a jelly roll type electrode assembly, the winding core 1 is rotated in a state where the start ends (ends where winding starts) of two sheets of separators 2a and 2b overlap each other and are fixed to the winding core 1. Then, the negative electrode 3 is input, and after a predetermined time has passed, the positive electrode 4 is input.
[0011] When the winding core 1 is rotated a predetermined number of times in a state in which the positive electrode 4 is input, the following structure is obtained, in which the starting ends of the separators 2a and 2b are located in the centralmost area of the completed cylindrical electrode assembly, the starting end of the negative electrode 3 is positioned outward from the starting ends of the separators 2a and 2b at the center, and the starting end of the positive electrode 4 is positioned outward from the starting end of the negative electrode 3.
[0012] Here, the positive electrode is manufactured to have a length smaller than that of the negative electrode, and therefore, the capacity of the manufactured electrode assembly is proportional to the length of the positive electrode 4, more specifically, proportional to the area of the surface of the positive electrode active material 4b of the positive electrode 4 applied to the positive electrode collector 4a. Therefore, in terms of capacity, it is advantageous to apply the positive electrode active material 4b to the surface of the positive electrode collector 4a as widely as possible. However, as shown in the disassembled state of the used electrode assembly Figure 1B As shown in , when heat is concentrated in the center of the electrode assembly, in the starting end of the positive electrode 4 , the separator 2 thermally contracts, and accordingly, a short circuit may occur due to contact between the positive electrode 4 and the negative electrode 3 .
[0013] Therefore, the positive electrode 4 is input later than the negative electrode 3 when winding, thereby preventing internal short circuit. Figure 1CAs shown in , the negative electrode 3 has a portion from the start end to a designated point not coated with the negative electrode active material 3b, and after a designated distance (gap) from the point where the application of the negative electrode active material 3b starts, the positive electrode 4 is input (that is, the electrode assembly is manufactured so that there is a designated gap between the point where the application of the negative electrode active material in the negative electrode starts and the point where the application of the positive electrode active material in the positive electrode starts). Here, the current collector exposure portion not coated with the negative electrode active material 3b in the negative electrode current collector 3a is formed in each of the start end (the end adjacent to the winding core) and the end (the end in the outermost region) of the negative electrode 3. The end current collector exposure portion of the negative electrode 3 has an area wider than that of the start end current collector exposure portion, and the end current collector exposure portion is bonded to the negative electrode terminal tab 3c so as to be connected to the outside. Moreover, the positive electrode 4 has a length smaller than that of the negative electrode 3, the current collector exposure portion not coated with the positive electrode active material 4b in the positive electrode current collector 4a is formed in a predetermined position between the two ends, and a structure in which the positive electrode terminal tab 4c is bonded to the current collector exposure portion is provided.
[0014] The electrode assembly in which the negative electrode 3 and the positive electrode 4 having the above-described structure are wound can ensure safety in proportion to the distance difference D between the positive electrode 4 and the negative electrode 3 .
[0015] That is, when the distance difference D is increased by shortening the positive electrode, the positive electrode does not contact the negative electrode even when the separator shrinks in the core, and therefore, safety with respect to fire is improved. However, the size of the positive electrode 4 is relatively reduced, thereby causing a capacity loss. Moreover, the positive electrode does not face the negative electrode active material coating portion (particularly the negative electrode 3) of the negative electrode 3 located in the region of the distance difference D at the winding center portion and coated with the negative electrode active material. Figure 1C Therefore, there is a problem that the negative electrode active material is wasted without generating electricity.
[0016] Moreover, for safety, the negative electrode tab 3c is bonded to the center of the can. However, since the negative electrode tab 3c is bonded to the end current collector exposed portion of the negative electrode 3 (since the negative electrode tab is placed in the outside of the electrode assembly), the negative electrode tab 3c must be long so as to be connected to the center of the can when the negative electrode tab 3c is welded to the battery can. Therefore, there is a problem that the internal resistance (direct current internal resistance (DCIR) and alternating current internal resistance (ACIR)) is unnecessarily increased. Summary of the invention
[0017] Technical issues
[0018] Therefore, the main object of the present invention is to provide an electrode assembly and a method for manufacturing the electrode assembly, in which the length of the positive electrode can be increased without deteriorating safety to maximize the capacity, and the welding distance of the negative electrode tab can be reduced to reduce the resistance.
[0019] Technical Solution
[0020] According to one aspect of the present invention, there is provided a jelly-roll type electrode assembly manufactured by winding a negative electrode, a separator, and a positive electrode together from ends thereof, the electrode assembly comprising: a negative electrode manufactured by applying a negative electrode active material to a surface of a negative electrode current collector, and having a negative electrode current collector exposed portion formed on one end of the negative electrode, the negative electrode current collector exposed portion not coated with the negative electrode active material to expose the surface of the negative electrode current collector, The negative electrode is wound together with a separator and a positive electrode so that the negative electrode current collector exposed portion is placed in a central region where the winding starts, and a negative electrode tab is coupled to the negative electrode current collector exposed portion.
[0021] According to another aspect of the present invention, there is provided a secondary battery in which the electrode assembly of the present invention is accommodated in a case.
[0022] According to still another aspect of the present invention, there is provided a method for manufacturing an electrode assembly, the electrode assembly being manufactured by winding a negative electrode, a separator, and a positive electrode around a winding core, the method comprising: a negative electrode rotating step (S1): inputting a negative electrode and allowing the negative electrode to rotate so that rotation around a winding core is performed from a starting end of the negative electrode; and a positive electrode input step (S2): inputting a positive electrode after the rotation of the negative electrode starts, and thereby allowing the positive electrode to rotate together with the negative electrode, wherein the negative electrode is manufactured by applying a negative electrode active material to the surface of a negative electrode current collector, wherein a negative current collector exposure portion is formed in the start end fixed to the winding core, the negative current collector exposure portion is not coated with the negative active material to expose the surface of the negative current collector, and a negative electrode tab is bonded to the negative current collector exposure portion.
[0023] In order to achieve the above-mentioned purpose, the present invention provides a method for manufacturing a jelly-roll type electrode assembly, which is manufactured by winding a negative electrode, a separator and a positive electrode around a winding core, the method comprising: a negative electrode rotation step (S1): inputting a negative electrode and allowing the negative electrode to rotate so that the rotation around the winding core is performed from the starting end of the negative electrode; and a positive electrode input step (S2): inputting a positive electrode after the rotation of the negative electrode starts, and thereby allowing the positive electrode to rotate together with the negative electrode, wherein the negative electrode is manufactured by applying a negative electrode active material to the surface of a negative electrode collector, wherein a negative electrode collector exposure portion is formed in the starting end fixed to the winding core, the negative electrode collector exposure portion is not coated with a negative electrode active material to expose the surface of the negative electrode collector, and a negative electrode terminal tab is bonded to the negative electrode collector exposure portion.
[0024] The negative electrode current collector exposed portion is formed in an end of the negative electrode on the side opposite to the start end, wherein in the negative electrode rotating step ( S1 ), the rotation starts from a negative electrode current collector exposed portion having a larger area among the negative electrode current collector exposed portions.
[0025] Moreover, in order to achieve the above-mentioned object, the present invention also provides an electrode assembly. The electrode assembly according to the present invention is a jelly roll type electrode assembly, which is manufactured by winding a negative electrode, a separator and a positive electrode together from the end thereof, and the electrode assembly includes a negative electrode, which is manufactured by applying a negative electrode active material to the surface of a negative electrode collector, and the negative electrode has a negative electrode collector exposure portion formed on one end of the negative electrode, the negative electrode collector exposure portion is not coated with a negative electrode active material to expose the surface of the negative electrode collector, wherein the negative electrode is wound together with the separator and the positive electrode so that the negative electrode collector exposure portion is placed in the central area where the winding starts, and the negative electrode tab is connected to the negative electrode collector exposure portion.
[0026] The negative electrode current collector exposed portion is formed in each of both ends of the negative electrode, and a negative electrode current collector exposed portion having a larger area among the negative electrode current collector exposed portions is disposed in a central region.
[0027] Also, a negative electrode tab is coupled to a negative electrode collector exposed portion having a larger area among the negative electrode collector exposed portions, and the negative electrode collector exposed portion is electrically connected to a negative terminal (the negative terminal is mounted to a can or case accommodating the electrode assembly therein) through the negative electrode tab.
[0028] The negative electrode tab is coupled to the negative electrode current collector exposed portion while protruding in a width direction of the negative electrode.
[0029] Here, the positive electrode is shorter than the negative electrode, so that when winding of the negative electrode, the separator, and the positive electrode starts, winding of the positive electrode starts later than winding of the negative electrode, wherein winding of the positive electrode is completed earlier than winding of the negative electrode.
[0030] The winding is performed so that both ends of the positive electrode are respectively spaced apart from the negative electrode current collector exposed portions formed on both ends of the negative electrode by a specified distance. Here, the distance may be changed according to the specifications of the electrode assembly to be manufactured.
[0031] The positive electrode is manufactured by applying a positive electrode active material to a surface of a positive electrode collector, and has a positive electrode collector exposure portion formed therein, the positive electrode collector exposure portion not coated with the positive electrode active material to expose the surface of the positive electrode collector.
[0032] Also, the positive electrode current collector exposed portion is disposed between two regions of the positive electrode current collector coated with the positive electrode active material.
[0033] It is desirable that the positive electrode current collector exposed portion has an area smaller than that of the negative electrode current collector exposed portion having a larger area among the negative electrode current collector exposed portions and larger than that of the negative electrode current collector exposed portion having a smaller area among the negative electrode current collector exposed portions.
[0034] The positive electrode current collector exposed portion is disposed closer to a negative electrode current collector exposed portion having a larger area among the negative electrode current collector exposed portions than to a negative electrode current collector exposed portion having a smaller area.
[0035] The electrode assembly having the above structure is housed in a case to manufacture a secondary battery.
[0036] Beneficial effects
[0037] In the electrode assembly of the present invention having the above structure, the negative electrode tab is placed in the center of the electrode assembly, so when the negative electrode tab is welded to the can, the length of the negative electrode tab can be reduced. Accordingly, unnecessary resistance increase can be reduced.
[0038] In particular, according to the present invention, the negative electrode current collector exposed portion located in the starting end (the end placed in the center of the winding) has a larger area than the negative electrode current collector exposed portion located in the ending end (the end placed in the outside of the electrode assembly), and therefore, compared with the structure of the related art, the gap between the point where the application of the negative electrode active material in the starting end and the point where the application of the positive electrode active material in the starting end starts can be reduced (that is, compared with the structure of the related art, the length of the positive electrode can be increased). Therefore, the capacity of the electrode assembly can be increased. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1A is a view showing a state in which two sheets of separators are first fixed to a winding core, and then a negative electrode and a positive electrode are sequentially input.
[0040] Figure 1B 1 and 2 are views showing a state where a used electrode assembly J / R is disassembled and unfolded (upper figure) and a state where the disassembled negative electrode and positive electrode are compared (lower figure).
[0041] Figure 1C is a view comparing a negative electrode and a positive electrode input in a method for manufacturing a jelly-roll type electrode assembly of the related art.
[0042] Figure 2 is a flow chart of the steps applied in a method for manufacturing an electrode assembly according to the present invention.
[0043] Figure 3 : is a view showing a state where a positive electrode and a negative electrode input in an electrode assembly according to the present invention are compared (lower figure) and a state where a negative electrode and a positive electrode are located in the electrode assembly (upper figure) ( Figure 3 It is shown that a certain space is set inside while the negative electrode, separator, and positive electrode are rotated, but the components are intentionally shown as separated from each other because it is difficult to identify the components when their lines appear to be attached together in the drawing. That is, during rotation, the negative electrode, separator, and positive electrode are wound in a tightly packed cylindrical shape while actually being attached to each other).
[0044] Figure 4 are views showing a state in which a negative electrode tab and a positive electrode tab are located in an electrode assembly of the related art (left diagram) and a state in which a negative electrode tab and a positive electrode tab are located in an electrode assembly according to the present invention (right diagram).
[0045] Figure 5 is a view showing a graph for comparing experimental results of an electrode assembly according to the present invention (Example) and an electrode assembly of the related art (Comparative Examples 1 and 2). DETAILED DESCRIPTION
[0046] Hereinafter, the present invention will be described in detail with reference to the accompanying drawings so that those skilled in the art to which the present invention belongs can easily implement the present invention. However, the present invention can be embodied in several different forms and is not limited to the embodiments set forth herein.
[0047] Parts that are not related to the description will be omitted in order to clearly describe the present invention, and the same reference numerals are attached to the same or similar elements throughout the specification.
[0048] Furthermore, the terms or words used in this specification and the claims should not be restrictively interpreted as ordinary meanings or dictionary-based meanings, but should be interpreted as meanings and concepts consistent with the scope of the present invention based on the principle that the inventor can appropriately define the concepts of the terms to best describe and interpret his or her invention.
[0049] The present invention relates to an electrode assembly and a method for manufacturing the electrode assembly, in which capacity can be increased while reducing internal resistance. Hereinafter, embodiments according to the present invention will be described in more detail with reference to the accompanying drawings.
[0050] First embodiment
[0051] As a first embodiment, the present invention provides a method for manufacturing a jelly-roll type electrode assembly manufactured by winding a negative electrode 30 , a separator 20 ( 20 a and 20 b ), and a positive electrode 40 around a winding core.
[0052] Figure 2 is a flow chart of the steps applied in the method for manufacturing an electrode assembly according to the present invention. Figure 3 : is a view showing a state where a positive electrode and a negative electrode are compared in an electrode assembly according to the present invention (lower figure) and a state where a negative electrode and a positive electrode are located in the electrode assembly (upper figure). For reference, Figure 3 It is shown that a certain space is provided inside while the negative electrode 30, the separator 20, and the positive electrode 40 rotate, but the components are intentionally shown as being separated from each other because it is difficult to identify the components when their lines appear to be attached together in the drawing. That is, during rotation, the negative electrode 30, the separator 20, and the positive electrode 40 are wound in a tightly packed cylindrical shape while actually being attached to each other.
[0053] refer to Figure 2 and Figure 3 , the present invention is manufactured so that the two sheets of separators 20a and 20b are first fixed to the winding core as in the related art, and then, the negative electrode 30 is first input and the positive electrode 40 is input later (see Figure 1A In the negative electrode 30 input in the present invention, the negative electrode terminal tab 30c is bonded to the negative electrode current collector exposed portion, and the negative electrode current collector exposed portion bonded with the negative electrode terminal tab 30c is located at the beginning end of the negative electrode 30 (as the end portion placed adjacent to the winding core). Figure 3 ) in the left end of the electrode assembly so that the negative electrode tab 30c is located in the central area of the electrode assembly.
[0054] That is, in the manufacturing method of the present invention, two sheets of separators 20a and 20b are first fixed to the winding core and wound around the winding core in the same manner as in the related art. Then, the negative electrode 30 is input between the separators 20a and 20b or is input while contacting one of the separators 20a and 20b. A negative electrode rotating step (S1) is performed in which the negative electrode 30 is rotated around the winding core together with the separators 20a and 20b.
[0055] Then, the rotation of the negative electrode 30 starts, and after a short time difference, the positive electrode 40 is input. Here, the short time difference is sufficient to be able to rotate at the beginning ( Figure 3 The left end of the positive electrode 40 ( Figure 3 The time difference between the distance difference D between the left end and the right end can be expressed as Figure 3 The formation shown in FIG.
[0056] A positive electrode input step (S2) is performed in which, after the rotation of the negative electrode 30 is started, the positive electrode 40 is input to rotate together with the negative electrode 30. Then, when the winding core rotates a predetermined number of rotations, the winding of the positive electrode 40, the negative electrode 30, and the separator 20 that have been input is completed.
[0057] Moreover, the negative electrode 30 according to the present invention is manufactured by applying a negative electrode active material 30b to the surface of a negative electrode collector 30a, and a negative electrode collector exposure portion 31a is formed in the starting end fixed to the winding core, which is not coated with a negative electrode active material to expose the surface of the negative electrode collector 30a.
[0058] As in Figure 3 As shown in FIG. 1 , the negative current collector exposed portion 31a is formed in the end and the beginning of the negative electrode 30. The negative current collector exposed portion 31a formed in the beginning has a larger area than the negative current collector exposed portion 31b formed in the end and is bonded to the negative electrode tab 30c.
[0059] That is, in the manufacturing method according to this embodiment, the rotation starts from the negative current collector exposed portion 31a having a larger area among the negative current collector exposed portions 31a and 31b. In the negative electrode rotating step (S1), the rotation starts from the negative current collector exposed portion 31a having a larger area.
[0060] The present invention having the above structure can reduce the negative electrode active material coating portion wasted in the area of the distance difference D between the positive electrode and the negative electrode at the winding center portion. That is, instead of applying the negative electrode active material to the area where the reaction does not proceed ( Figure 1C In the gap region), a negative electrode current collector exposed portion is formed in the region. Moreover, the negative electrode active material is additionally applied to the region of the negative electrode current collector exposed portion formed in the winding end of the negative electrode in the related art. Therefore, relative to the application length ( Figure 3 β), the length of the portion of the end of the positive electrode to which the positive electrode active material is applied can be increased by β. By extending the reaction length β, more electricity can be generated. Accordingly, compared with the related art, the battery capacity can be further increased.
[0061] Here, because the safety of the battery regarding the positive and negative short circuit is determined by the positive and negative distance difference D, the distance difference between the positive and negative electrodes is maintained at D to maintain safety, and in the first embodiment of the present invention, the length of the positive electrode can be further extended to t+β.
[0062] Second embodiment
[0063] In addition, as a second embodiment, the present invention provides an electrode assembly that can be manufactured by the above-mentioned manufacturing method.
[0064] The electrode assembly according to the present invention is a jelly roll type electrode assembly in which the negative electrode 30, the separator 20, the positive electrode 40 are stacked, wound from the center, and then manufactured in a cylindrical shape. Unlike the related art, the negative electrode tab 30c is placed in or around the center of the cylindrical electrode assembly.
[0065] In an embodiment, the negative electrode 30 is manufactured by applying a negative electrode active material 30b to the surface of a negative electrode collector 30a, and negative electrode collector exposure portions 31a and 31b are formed at both ends (i.e., a starting end near the winding core and an end opposite to the starting end), and the negative electrode collector exposure portions 31a and 31b are not coated with the negative electrode active material 30b to expose the surface of the negative electrode collector 30a.
[0066] Here, the negative electrode current collector exposed portion 31a formed in the starting end has an area larger than that of the negative electrode current collector exposed portion 31b formed in the ending end, and the negative electrode terminal tab 30c may be coupled to the negative electrode current collector exposed portion 31a formed in the starting end. The negative electrode terminal tab 30c is coupled to the negative electrode current collector exposed portion 31a formed in the starting end of the negative electrode 30, and the negative electrode terminal tab 30c is coupled to the negative electrode current collector exposed portion 31a while protruding in the width direction of the negative electrode 30. Moreover, the negative electrode terminal tab 30c is electrically connected to the negative terminal (the negative terminal is mounted to the can or case in which the electrode assembly is accommodated).
[0067] Here, the positive electrode 40 is shorter than the negative electrode 30, so that during the manufacturing process, the winding of the positive electrode 40 wound with the separator 20 therebetween starts later than the winding of the negative electrode 30 and is completed earlier than the winding of the negative electrode 30. Also, the winding is performed so that both ends of the positive electrode 40 are spaced apart from the negative current collector exposed portions 31a and 31b formed on both ends of the negative electrode 30 by a specified distance, respectively.
[0068] That is, as in Figure 3 As shown in FIG. 1 , due to the presence of the negative electrode current collector exposed portion 31 a located in the beginning of the negative electrode 30, the positive electrode 40 has a gap α with respect to the beginning of the positive electrode 40. Moreover, when the length of the positive electrode of the related art is t (see FIG. 1 ), the positive electrode 40 has a gap α with respect to the beginning of the positive electrode 40. Figure 1C), the positive electrode is extended by β corresponding to the extended length of the negative electrode active material, and thus can have a length of t+β.
[0069] In the present invention, the negative electrode current collector exposed portion 31a having a larger area is located in the beginning of the negative electrode 30, and therefore, the negative electrode active material retained in an amount corresponding to the length of the negative electrode current collector exposed portion 31a can be applied to the end of the negative electrode. Accordingly, the end of the positive electrode 40 can be extended, and the length of the positive electrode can be maximized. In this case, the gap α between the negative electrode active material and the positive electrode active material in the beginning of the present invention can be smaller than the gap of the structure of the related art. The gap α between the negative electrode active material and the positive electrode active material represents a waste area, and therefore, in the present invention, waste can be reduced compared to the related art.
[0070] As in Figure 1C and Figure 3 As shown in FIG. 1 , for safety (ie, to prevent short circuit), a gap D is created between the start end of the negative electrode 30 and the start end of the positive electrode 40 at a predetermined distance (regardless of the area of the negative electrode current collector exposed portion). Figure 1C In the structure of the related art, the negative electrode active material is applied to the area closer to the beginning of the negative electrode. Figure 3 In the structure of the embodiment, the negative electrode active material is applied from a region relatively far from the start end of the negative electrode.
[0071] Therefore, in a state where the gap D between the start end of the negative electrode 30 and the start end of the positive electrode 40 is fixed for safety, the negative electrode active material is placed closer to Figure 1C Therefore, the gap between the point where the application of the negative electrode active material starts and the point where the application of the positive electrode active material starts becomes larger than Figure 3 That is, the area with the gap is an area where only the negative electrode active material is applied, and is a waste area that is not involved in the charge and discharge of the electrode assembly. However, in this embodiment, the distance of the waste area is reduced to α, and according to the reduced size α, the length of the negative electrode active material applied to the end of the negative electrode 30 is increased by β. Therefore, the capacity can be increased (that is, Figure 1C The gap may be the sum of α and β). Therefore, in a state where the length of the negative electrode 30 is not changed, the region where the negative electrode active material is applied is relatively further extended in the end of the negative electrode 30. Therefore, the length of the positive electrode 40 can be extended by the length by which the application of the negative electrode active material is extended, as long as it is shorter than the negative electrode 30. Accordingly, the capacity of the electrode assembly can be increased.
[0072] Here, the size of α can be determined according to the manufacturing process. For example, a winding core having a sufficiently small size is used (condition 1), the applied thickness of the electrode active material has a uniformity exceeding a specified level (condition 2), and the coating start point difference is adjusted on both surfaces of the electrode (condition 3). Under the above conditions, the size of α can have a value of 0.9 mm to 1.1 mm, which is smaller than the size of the structure of the related art.
[0073] When the size of α is reduced to 0.9 mm to 1.1 mm as described above, the capacity of the battery can be increased by 3.2% to 3.4%, and the energy density per unit volume can be increased by 2% to 2.2%.
[0074] Also, the positive electrode 40 is manufactured by applying a positive electrode active material 40b to the surface of a positive electrode collector 40a, similarly to the negative electrode 30, and is formed with a positive electrode collector exposure portion 41 which is not coated with the positive electrode active material 40b to expose the surface of the positive electrode collector 40a. A positive electrode tab 40c is bonded to the positive electrode collector exposure portion 41, and the positive electrode tab 40c is bonded while protruding in a direction opposite to the negative electrode tab 30c.
[0075] Unlike the negative electrode current collector exposed portions 31a and 31b, the positive electrode current collector exposed portion 41 is placed between two areas of the positive electrode current collector 40a that are coated with the positive electrode active material 40b and separated from each other. The area and position of the positive electrode current collector exposed portion 41 are not limited to a specific range, but it is desirable that the positive electrode current collector exposed portion 41 has an area smaller than the area of the negative electrode current collector exposed portion 31a with a larger area among the negative electrode current collector exposed portions 31a and 31b and an area larger than the area of the negative electrode current collector exposed portion 31b with a smaller area among the negative electrode current collector exposed portions 31a and 31b. In addition, the positive electrode current collector exposed portion 41 is placed closer to the negative electrode current collector exposed portion 31a with a larger area among the negative electrode current collector exposed portions 31a and 31b than to the negative electrode current collector exposed portion 31b with a smaller area.
[0076] Also, the electrode assembly having the above structure is housed in a case to manufacture a secondary battery.
[0077] In the electrode assembly of the present invention having the above structure, the negative electrode tab 30c is placed in the center of the electrode assembly, so when the negative electrode tab 30c is welded to the can, the length of the negative electrode tab 30c can be reduced. Accordingly, unnecessary resistance increase can be reduced.
[0078] As shown in the state where the negative electrode terminal tab 3c and the positive electrode terminal tab 4c are located in the electrode assembly of the related art (left figure) and the state where the negative electrode terminal tab 30c and the positive electrode terminal tab 40c are located in the electrode assembly according to the present invention (right figure) Figure 4As shown in , in the structure of the present invention, the negative electrode tab 30c is positioned close to the center of the electrode assembly. Therefore, welding can be performed directly on the bottom surface of the can to reduce the length, and accordingly, the increase in resistance can be reduced.
[0079] In particular, according to the present invention, the negative electrode current collector exposed portion 31a located in the starting end (the end placed in the winding center) has a larger area than the negative electrode current collector exposed portion 31b located in the end (the end placed in the outside of the electrode assembly), and thus, compared with the structure of the related art, the waste between the positive electrode 40 and the negative electrode 30 in the starting end can be reduced (that is, compared with the structure of the related art, the length of the positive electrode can be increased). Therefore, the capacity of the electrode assembly can be increased.
[0080] experiment
[0081] Figure 5 is a view showing a graph for comparing experimental results of an electrode assembly according to the present invention (Example) and an electrode assembly of the related art (Comparative Examples 1 and 2).
[0082] This embodiment is as in Figure 3 The electrode assembly of the structure shown in FIG. 1 is an electrode assembly in which the negative electrode current collector exposed portion 31a having a larger area is located in the center of the electrode assembly, and the negative electrode terminal tab 30c is placed close to the center. Figure 1B The electrode assembly of the structure of the related art shown in FIG. 1, in which the negative electrode tab is placed outside the electrode assembly. Comparative Example 2 is an electrode assembly having the same structure of the related art as Comparative Example 1, but the gap between the positive electrode and the negative electrode is further extended (a structure in which the gap is increased by 5 mm compared to Comparative Example 1. That is, Figure 1B The structure in which the length of the positive electrode is further reduced) (Comparative Example 2 corresponds to Figure 1C , and Comparative Example 2 has a structure in which the positive-negative electrode gap D is extended to the extent of preventing short circuit). Moreover, in this experiment, the length of the positive electrode inside the electrode assembly of Comparative Example 1 is the same as the length of the positive electrode inside the electrode assembly of Example. Due to the increase in the gap between the positive and negative electrodes, the length of the positive electrode in Comparative Example 2 is reduced.
[0083] Each electrode assembly was manufactured into a jelly roll type and then inserted into a cylindrical can. Subsequently, an electrolyte was injected therein. Experiments were performed using a cylindrical secondary battery manufactured by the above conventional method.
[0084] The experimental conditions were that each secondary battery was placed in a closed chamber and heated at a rate of 5°C / min. And, when reaching 130°C, the temperature was maintained.
[0085] As in Figure 5 As shown in, in the secondary battery of Comparative Example 1, the temperature reaches 130°C at about 22 to 23 minutes and is maintained for 10 minutes. Fire occurs, and the cell voltage becomes 0 V. Moreover, in the secondary battery of Comparative Example 2 and the secondary battery according to the example of the present invention, it can be found that the temperature reaches 130°C and no fire occurs in one hour or more.
[0086] That is, comparing Comparative Example 1 and Comparative Example 2, it can be found that when the gap between the negative electrode and the positive electrode increases in the related art, the safety with respect to fire increases. However, in the structure of Comparative Example 2, as the gap increases, the length of the positive electrode becomes shorter. Accordingly, the total capacity decreases. However, in the structure of the example of the present invention, it can be found that the gap increases without reducing the length of the present invention (without reducing the capacity) to obtain improved safety with respect to fire.
[0087] In addition, the following Table 1 shows relative values of energy density and DCIR of Comparative Example 1 and Example when the energy density of Comparative Example 2 is B and the DCIR is C.
[0088] [Form 1]
[0089] Comparative Example 1 Comparative Example 2 Example Energy density (Wh / L) B+7 B B+7 DCIR (mohm) C C C-5
[0090] As shown in Table 1, the energy density of Example is equal to that of Comparative Example 1, and the value of DCIR of Example is measured to be smaller than that of Comparative Example 1 and Comparative Example 2.
[0091] Therefore, according to Figure 5 According to Table 1, the electrode assembly of the example of the present invention has the same length as the electrode assembly of Comparative Example 1, and therefore, the same energy density can be achieved. Moreover, the example of the present invention can have the safety about fire equal to Comparative Example 2 (Comparative Example 2 has the advantage of increasing the gap between the negative electrode and the positive electrode and thereby improving the safety about fire, but has the disadvantage of reducing energy density). Moreover, the negative electrode tab is moved to the center, and therefore, its length is reduced. Accordingly, there can be a side effect of reducing internal resistance.
[0092] Although the present invention has been described through specific embodiments and drawings, the present invention is not limited thereto, and various changes and modifications may be made by those skilled in the art within the technical idea of the present invention and the equivalent scope of the appended claims.
[0093] [Explanation of Reference Numerals]
[0094] 20: Separator
[0095] 30: Negative electrode
[0096] 40: Positive electrode
Claims
1. A jelly-roll type electrode assembly manufactured by winding a negative electrode, a separator, and a positive electrode together from ends thereof, the electrode assembly comprising: a negative electrode manufactured by applying a negative electrode active material to a surface of a negative electrode current collector, and having a negative electrode current collector exposed portion formed on one end of the negative electrode, the negative electrode current collector exposed portion not coated with the negative electrode active material to expose the surface of the negative electrode current collector, The negative electrode is wound together with a separator and a positive electrode so that the negative electrode current collector exposed portion is placed in a central region where the winding starts, and a negative electrode tab is coupled to the negative electrode current collector exposed portion.
2. The electrode assembly according to claim 1, wherein: The negative electrode current collector exposure portion is formed in each of both ends of the negative electrode, and A negative electrode current collector exposed portion having a larger area among the negative electrode current collector exposed portions is disposed in the central region.
3. The electrode assembly according to claim 2, wherein: The negative electrode tab is coupled to the negative electrode current collector exposed portion having a larger area among the negative electrode current collector exposed portions, and The negative current collector exposed portion is electrically connected to a negative terminal through the negative electrode tab.
4. The electrode assembly according to claim 3, wherein: The negative electrode tab is coupled to the negative electrode current collector exposed portion while protruding in a width direction of the negative electrode.
5. The electrode assembly according to claim 4, wherein: the positive electrode is shorter than the negative electrode so that when the winding of the negative electrode, the separator, and the positive electrode starts, the winding of the positive electrode starts later than the winding of the negative electrode, The winding of the positive electrode is completed earlier than the winding of the negative electrode.
6. The electrode assembly according to claim 5, wherein: The winding is performed such that both ends of the positive electrode are spaced apart from the negative electrode current collector exposed portions formed on both ends of the negative electrode by designated distances, respectively.
7. The electrode assembly according to claim 2, wherein: The positive electrode is manufactured by applying a positive electrode active material to a surface of a positive electrode collector, and the positive electrode has a positive electrode collector exposed portion formed in the positive electrode, the positive electrode collector exposed portion not coated with the positive electrode active material to expose the surface of the positive electrode collector, and The positive electrode current collector exposed portion is disposed between two regions of the positive electrode current collector coated with the positive electrode active material.
8. The electrode assembly according to claim 7, wherein: The positive electrode current collector exposed portion has an area smaller than the larger area of the negative electrode current collector exposed portion among the negative electrode current collector exposed portions and larger than the smaller area of the negative electrode current collector exposed portion among the negative electrode current collector exposed portions.
9. The electrode assembly according to claim 7, wherein: The positive electrode current collector exposed portion is disposed closer to the negative electrode current collector exposed portion having a larger area among the negative electrode current collector exposed portions than to the negative electrode current collector exposed portion having a smaller area. 10 . A secondary battery in which the electrode assembly according to claim 1 is accommodated in a case.
11. A method for manufacturing an electrode assembly, the electrode assembly being manufactured by winding a negative electrode, a separator, and a positive electrode around a winding core, the method comprising: a negative electrode rotating step (S1): inputting a negative electrode and allowing the negative electrode to rotate so that rotation around a winding core is performed from a starting end of the negative electrode; and a positive electrode input step (S2): inputting a positive electrode after the rotation of the negative electrode starts, and thereby allowing the positive electrode to rotate together with the negative electrode, wherein the negative electrode is manufactured by applying a negative electrode active material to the surface of a negative electrode current collector, wherein a negative current collector exposure portion is formed in the start end fixed to the winding core, the negative current collector exposure portion is not coated with the negative active material to expose the surface of the negative current collector, and a negative electrode tab is bonded to the negative current collector exposure portion.
12. The method according to claim 11, wherein: The negative electrode current collector exposed portion is formed in an end of the negative electrode on a side opposite to the starting end, Wherein, in the negative electrode rotating step (S1), the rotation starts from a negative electrode current collector exposed portion having a larger area among the negative electrode current collector exposed portions.