Inter-band cascade laser and preparation method thereof
By adopting a hybrid waveguide structure in the inter-band cascade laser, the defects and low yields during epitaxial growth are solved, and higher quality device preparation and performance improvements are achieved.
Patent Information
- Application Number
- CN202411196122.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-22
AI Technical Summary
Existing interband cascade lasers are prone to defects during epitaxial growth, especially when the capping material is GaSb or InAs, the superlattice cladding is thicker and has high growth difficulty, resulting in a low yield.
Adopting a hybrid waveguide structure, including the first and second hybrid waveguides, consisting of an outer limiting layer and a superlattice restriction layer. The refractive index of the outer limiting layer is smaller than that of the superlattice restriction layer, reducing the thickness requirement of the superlattice material and reducing the The difficulty of epitaxial growth is achieved and the effective limit on the light field is achieved through the thinner hybrid waveguide structure.
It improves the yield and epitaxial growth quality of the device, reduces the occurrence of defects, simplifies the preparation process, and improves the performance of the device.
Smart Images

Figure CN119009678A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductors, and in particular to an interband cascade laser and a method for preparing the same. Background Art
[0002] Interband cascade laser (ICL) is an effective all-solid-state mid-infrared light source, which is widely used in communications, trace gas monitoring, electronic countermeasures and environmental monitoring.
[0003] At present, the epitaxial structure in the interband cascade laser includes a lower superlattice cladding, a lower waveguide layer, an active region, an upper waveguide layer, an upper superlattice cladding and a cap layer located on the substrate. The substrate material is GaSb, and the cap layer materials are GaSb and InAs. When the cap layer material is GaSb, the cap layer is etched to form a grating, and the active region, the upper waveguide layer, the upper superlattice cladding and the grating are etched to form a ridge waveguide structure. The superlattice cladding has a limiting effect on the light field. The lower superlattice cladding is thicker, and defects are more likely to occur during the epitaxial growth process. In addition, the epitaxial growth of superlattice materials is more difficult, resulting in difficult epitaxial growth. When the cap layer material is InAs, due to the lattice mismatch between InAs and the GaSb substrate, the InAs cap layer with a thickness that meets the requirements for preparing the grating cannot be grown on the top. Therefore, it is necessary to etch to the upper superlattice cladding to form a grating. Etching the superlattice cladding is prone to defects, resulting in a relatively low yield.
[0004] Therefore, how to solve the above technical problems should be the focus of technical personnel in this field. Summary of the invention
[0005] The purpose of the present application is to provide an interband cascade laser and a method for preparing the same, so as to reduce the difficulty of epitaxial growth and improve the yield of the device.
[0006] In order to solve the above technical problems, the present application provides an inter-band cascade laser, comprising:
[0007] substrate;
[0008] A first hybrid waveguide, a first waveguide layer, an active layer, a second waveguide layer, and a second hybrid waveguide are stacked in sequence from bottom to top on the upper surface of the substrate; wherein the first hybrid waveguide comprises a first outer confinement layer and a first superlattice confinement layer stacked from bottom to top, and the second hybrid waveguide comprises a second superlattice confinement layer and a second outer confinement layer stacked from bottom to top, the refractive index of the first outer confinement layer is smaller than that of the first superlattice confinement layer, and the refractive index of the second outer confinement layer is smaller than that of the second superlattice confinement layer; the second outer confinement layer is a grating structure, and at least the grating structure, the second superlattice confinement layer, the second waveguide layer, the active layer, and the first waveguide layer form a ridge waveguide structure;
[0009] a first electrode located on and in contact with the grating structure;
[0010] A second electrode is located on the lower surface of the substrate.
[0011] Optionally, when the substrate is a GaSb substrate, the first outer confinement layer and the second outer confinement layer include InAsSb layers, and the first superlattice confinement layer and the second superlattice confinement layer include InAs / AlSb superlattice layers.
[0012] Optionally, when the substrate is an InAs substrate, the first outer confinement layer and the second outer confinement layer include InAs layers, and the first superlattice confinement layer and the second superlattice confinement layer include InAs / AlSb superlattice layers.
[0013] Optionally, in the InAs / AlSb superlattice layer, the thickness of the InAs layer ranges from 22Å to 25Å, and the thickness of the AlSb layer ranges from 22Å to 25Å.
[0014] Optionally, the second outer confinement layer, the second superlattice confinement layer, the second waveguide layer, the active layer and the first waveguide layer form a ridge waveguide structure.
[0015] Optionally, it also includes:
[0016] A passivation layer is at least located on the upper surface and side surfaces of the ridge waveguide structure, the passivation layer is provided with an electrode window, the electrode window is correspondingly located on the upper surface of the ridge waveguide structure, and the first electrode is in contact with the grating structure through the electrode window.
[0017] The present application also provides a method for preparing any of the above-mentioned inter-band cascade lasers, comprising:
[0018] A first outer confinement layer, a first superlattice confinement layer, a first waveguide layer, an active layer, a second waveguide layer, a second superlattice confinement layer and a second outer confinement layer to be processed are sequentially grown on the upper surface of the substrate; the refractive index of the first outer confinement layer is smaller than that of the first superlattice confinement layer, and the refractive index of the second outer confinement layer to be processed is smaller than that of the second superlattice confinement layer;
[0019] The second outer limiting layer to be processed is made into a grating structure;
[0020] At least the grating structure, the second superlattice confinement layer, the second waveguide layer, the active layer and the first waveguide layer are made into a ridge waveguide structure;
[0021] Fabricating a first electrode on the grating structure and in contact with the grating structure;
[0022] The substrate is thinned, and a second electrode is fabricated on a second surface of the substrate to obtain an interband cascade laser.
[0023] Optionally, manufacturing the second outer limiting layer to be processed into a grating structure comprises:
[0024] Coating a photoresist on the upper surface of the second outer restriction layer to be processed;
[0025] exposing and developing the photoresist to form a patterned photoresist;
[0026] The second outer limiting layer to be processed is etched using the patterned photoresist as a mask to form a grating structure.
[0027] Optionally, manufacturing at least the grating structure, the second superlattice confinement layer, the second waveguide layer, the active layer and the first waveguide layer into a ridge waveguide structure comprises:
[0028] growing a hard mask on the upper surface of the grating structure;
[0029] forming a patterned photoresist on the hard mask;
[0030] Using the patterned photoresist as a mask, etching the hard mask to form a patterned hard mask;
[0031] The grating structure, the second superlattice confinement layer, the second waveguide layer, the active layer and the first waveguide layer are etched using the patterned hard mask as a mask to form a ridge waveguide structure, wherein the etching stops at the lower surface of the first waveguide layer.
[0032] Optionally, before manufacturing a first electrode in contact with the grating structure on the grating structure, the method further comprises:
[0033] Depositing a passivation layer on the upper surface, the side surface and the area located on both sides of the ridge waveguide structure;
[0034] Etching the passivation layer to form an electrode window, wherein the electrode window is located correspondingly on the upper surface of the ridge waveguide structure;
[0035] Producing a first electrode on the grating structure and in contact with the grating structure comprises:
[0036] A first electrode is fabricated on the surface of the passivation layer, and the first electrode is in contact with the grating structure through an electrode window.
[0037] The present application provides an inter-band cascade laser, comprising: a substrate; a first hybrid waveguide, a first waveguide layer, an active layer, a second waveguide layer, and a second hybrid waveguide, which are located on the upper surface of the substrate and are stacked in sequence from bottom to top; wherein the first hybrid waveguide comprises a first outer confinement layer and a first superlattice confinement layer, which are stacked from bottom to top; the second hybrid waveguide comprises a second superlattice confinement layer and a second outer confinement layer, which are stacked from bottom to top; the refractive index of the first outer confinement layer is smaller than that of the first superlattice confinement layer; and the refractive index of the second outer confinement layer is smaller than that of the second superlattice confinement layer; the second outer confinement layer is a grating structure, and at least the grating structure, the second superlattice confinement layer, the second waveguide layer, the active layer, and the first waveguide layer form a ridge waveguide structure; a first electrode located on the grating structure and in contact with the grating structure; and a second electrode located on the lower surface of the substrate.
[0038] It can be seen that the cascade laser of the present application includes a first hybrid waveguide and a second hybrid waveguide, the first hybrid waveguide includes a first outer confinement layer and a first superlattice confinement layer, and the second hybrid waveguide includes a second outer confinement layer and a second superlattice confinement layer. Since the refractive index of the first outer confinement layer and the second outer confinement layer is smaller than that of the first superlattice confinement layer and the second superlattice confinement layer, the hybrid waveguide structure used in the present application has a stronger confinement effect on the light field than the superlattice cladding of the same thickness, so only thinner first hybrid waveguides and second hybrid waveguides are needed to achieve the confinement effect of the superlattice cladding on the light field in the prior art; and, the first outer confinement layer and the second outer confinement layer replace part of the superlattice material in the cladding of the prior art, so the thickness of the first superlattice confinement layer and the second superlattice confinement layer can be much thinner, which is conducive to epitaxial growth. Since the first outer confinement layer and the second outer confinement layer are both bulk materials, the difficulty of epitaxial growth is lower than that of superlattice materials, and therefore it is more conducive to epitaxial growth.
[0039] In addition, the present application also provides a preparation method having the above advantages. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] In order to more clearly illustrate the embodiments of the present application or the technical solutions of the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0041] Figure 1 A schematic diagram of the local structure of an inter-band cascade laser provided in an embodiment of the present application;
[0042] Figure 2 A schematic diagram of the distribution of a passivation layer in an inter-band cascade laser provided in an embodiment of the present application;
[0043] Figure 3 A flow chart of a method for preparing an inter-band cascade laser provided in an embodiment of the present application;
[0044] Figures 4 to 8 A flow chart of a preparation process of an inter-band cascade laser provided in an embodiment of the present application;
[0045] Fig. 9 A test result diagram of a PIV test on a single-mode interband cascade laser manufactured in the present application;
[0046] Fig.10 A test result diagram of a spectrum test of the single-mode interband cascade laser manufactured in the present application;
[0047] In the figure, 1, substrate, 2, first outer confinement layer, 3, first superlattice confinement layer, 4, first waveguide layer, 5, active layer, 6, second waveguide layer, 7, second superlattice confinement layer, 8, grating structure, 9, ridge waveguide structure, 10, passivation layer, 11, electrode window, 12, second outer confinement layer to be processed, 13, first electrode, 14, second electrode. DETAILED DESCRIPTION
[0048] In order to enable those skilled in the art to better understand the present application, the present application is further described in detail below in conjunction with the accompanying drawings and specific implementation methods. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application.
[0049] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0050] As described in the background technology section, in the current interband cascade laser, when the cap material is GaSb, the problem is that the lower superlattice cladding is thicker, defects are more likely to occur during the epitaxial growth process, and growth is more difficult; when the cap material is InAs, the cap layer and the upper superlattice cladding need to be etched to form a grating, and etching the superlattice cladding is prone to defects, resulting in a relatively low yield.
[0051] In view of this, the present application provides an inter-band cascade laser, such as Figure 1 As shown, including:
[0052] Substrate 1;
[0053] A first hybrid waveguide, a first waveguide layer 4, an active layer 5, a second waveguide layer 6, and a second hybrid waveguide are stacked in sequence from bottom to top on the upper surface of the substrate 1; wherein the first hybrid waveguide comprises a first outer confinement layer 2 and a first superlattice confinement layer 3 stacked from bottom to top, and the second hybrid waveguide comprises a second superlattice confinement layer 7 and a second outer confinement layer stacked from bottom to top, the refractive index of the first outer confinement layer 2 is smaller than that of the first superlattice confinement layer 3, and the refractive index of the second outer confinement layer is smaller than that of the second superlattice confinement layer 7; the second outer confinement layer is a grating structure 8, and at least the grating structure 8, the second superlattice confinement layer 7, the second waveguide layer 6, the active layer 5, and the first waveguide layer 4 form a ridge waveguide structure 9;
[0054] A first electrode 13 located on the grating structure 8 and in contact with the grating structure 8;
[0055] A second electrode 14 is located on the lower surface of the substrate 1 .
[0056] The inter-band cascade laser in this embodiment may be a single-mode inter-band cascade laser.
[0057] It should be noted that the interband cascade laser may further include a buffer layer between the substrate 1 and the first hybrid waveguide. The buffer layer can reduce or eliminate the lattice mismatch between the substrate 1 and the first outer confinement layer 2, can effectively alleviate the stress and dislocation caused by the lattice mismatch, and improve the growth quality of the epitaxial structure.
[0058] The substrate 1 may be a GaSb substrate or an InAs substrate 1 .
[0059] The active layer 5, the first waveguide layer 4 and the second waveguide layer 6 refer to the related art and will not be described in detail here.
[0060] The refractive index of the first outer confinement layer 2 is smaller than that of the first superlattice confinement layer 3, and the refractive index of the second outer confinement layer is smaller than that of the second superlattice confinement layer 7. Since the first hybrid waveguide and the second hybrid waveguide structure have a stronger limiting effect on the light field than the superlattice cladding of the same thickness, when achieving the same light field limiting effect as in the prior art, the thickness of the first hybrid waveguide and the second hybrid waveguide is thinner, and the thickness of the first superlattice confinement layer 3 and the second superlattice confinement layer 7 can be much thinner than that of the superlattice in the cladding of the original technology. Since the thickness of the first superlattice confinement layer 3 and the second superlattice confinement layer 7 is thinner, the growth is relatively easier and has fewer defects. Since the first outer confinement layer 2 and the second outer confinement layer are both bulk materials, they are more conducive to epitaxial growth, and have fewer growth defects than the pure superlattice cladding of the original technology.
[0061] It should be pointed out that in this embodiment, the materials of the first outer confinement layer 2 , the first superlattice confinement layer 3 , the second outer confinement layer and the second superlattice confinement layer 7 are not limited and can be determined according to the material of the substrate 1 .
[0062] As an implementation method, when the substrate 1 is a GaSb substrate, the first outer confinement layer 2 and the second outer confinement layer include InAsSb layers, the first superlattice confinement layer 3 and the second superlattice confinement layer 7 include InAs / AlSb superlattice layers, and the first waveguide layer 4 and the second waveguide layer 6 can be GaSb layers.
[0063] In the InAs / AlSb superlattice layer, the thickness of the InAs layer can range from 22Å to 25Å, such as 22Å, 23Å, 24Å, 25Å, etc., and the thickness of the AlSb layer can range from 22Å to 25Å, such as 22Å, 23Å, 24Å, 25Å, etc.
[0064] The InAs / AlSb superlattice layer is an alternately stacked InAs layer and AlSb layer. One InAs layer and one AlSb layer constitute one period. In this embodiment, the number of periods in the InAs / AlSb superlattice layer is not limited and is determined according to the required thickness of the InAs / AlSb superlattice layer.
[0065] When the first outer limiting layer 2 and the second outer limiting layer are InAsSb layers, the composition of As and Sb is not limited in this embodiment and can be set at will. In order to make the lattice constant of the first outer limiting layer 2 and the second outer limiting layer material match the lattice constant of GaSb, the composition of As in the InAsSb layer is 0.91 and the composition of Sb is 0.09, that is, the first outer limiting layer 2 and the second outer limiting layer are InAs 0.91 Sb 0.09 layer.
[0066] As another possible implementation mode, when the substrate 1 is an InAs substrate, the first outer confinement layer 2 and the second outer confinement layer include InAs layers, the first superlattice confinement layer 3 and the second superlattice confinement layer 7 include InAs / AlSb superlattice layers, and the first waveguide layer 4 and the second waveguide layer 6 can be InAs layers.
[0067] In the InAs / AlSb superlattice layer, the thickness of the InAs layer can range from 22Å to 25Å, such as 22Å, 23Å, 24Å, 25Å, etc., and the thickness of the AlSb layer can range from 22Å to 25Å, such as 22Å, 23Å, 24Å, 25Å, etc.
[0068] The InAs / AlSb superlattice layer is an alternately stacked InAs layer and AlSb layer. One InAs layer and one AlSb layer constitute one period. In this embodiment, the number of periods in the InAs / AlSb superlattice layer is not limited and is determined according to the required thickness of the InAs / AlSb superlattice layer.
[0069] In the prior art, the capping material is GaSb, but in the present application, when substrate 1 is a GaSb substrate, the second outer confinement layer is an InAsSb layer, and when substrate 1 is an InAs substrate, the second outer confinement layer is an InAs layer. The InAsSb layer and the InAs layer are convenient for n-type doping and are more likely to form n-type contact, that is, they are easy to form ohmic contact with metal.
[0070] When etching to form the ridge waveguide structure 9, the etching needs to exceed the active layer 5. In this embodiment, the ridge waveguide structure 9 is not limited and can be set at will. The longitudinal section of the ridge waveguide structure 9 can be a structure of equal width or a trapezoidal structure with narrow upper part and wide lower part.
[0071] As an implementation method, the second outer confinement layer, the second superlattice confinement layer 7, the second waveguide layer 6, the active layer 5 and the first waveguide layer 4 form a ridge waveguide structure 9. That is, the ridge waveguide structure 9 extends downward from the grating structure 8 to the first waveguide layer 4, as shown in FIG. Figure 1 As shown, at this time, the side wall area of the ridge waveguide structure 9 is small, which can reduce the leakage of the ridge waveguide side wall, thereby improving the performance of the cascade laser.
[0072] As another possible implementation mode, the second outer confinement layer, the second superlattice confinement layer 7, the second waveguide layer 6, the active layer 5, the first waveguide layer 4, and the first superlattice confinement layer 3 form a ridge waveguide structure 9. That is, the ridge waveguide structure 9 extends downward from the grating structure 8 to the first superlattice confinement layer 3. Since the thickness of the first waveguide layer 4 is relatively thin, it is relatively difficult to stop etching on the first waveguide layer 4, and the etching can be stopped at the first superlattice confinement layer 3 to reduce the difficulty of etching to form the ridge waveguide structure 9.
[0073] The cascade laser of this embodiment includes a first hybrid waveguide and a second hybrid waveguide. The first hybrid waveguide includes a first outer confinement layer 2 and a first superlattice confinement layer 3, and the second hybrid waveguide includes a second outer confinement layer and a second superlattice confinement layer 7. Since the refractive index of the first outer confinement layer 2 and the second outer confinement layer is smaller than that of the first superlattice confinement layer 3 and the second superlattice confinement layer 7, the hybrid waveguide structure used in this application has a stronger confinement effect on the light field than the superlattice cladding of the same thickness, so only thinner first hybrid waveguides and second hybrid waveguides are needed to achieve the confinement effect of the superlattice cladding on the light field in the prior art; and, the first outer confinement layer 2 and the second outer confinement layer replace part of the superlattice material in the cladding of the prior art, so the thickness of the first superlattice confinement layer 3 and the second superlattice confinement layer 7 can be much thinner, which is conducive to epitaxial growth. Since the first outer confinement layer and the second outer confinement layer are both bulk materials, the difficulty of epitaxial growth is lower than that of superlattice materials, so it is more conducive to epitaxial growth.
[0074] On the basis of the above embodiments, in one embodiment of the present application, the inter-band cascade laser may further include:
[0075] A passivation layer 10 is at least located on the upper surface and side surfaces of the ridge waveguide structure 9 , and the passivation layer 10 is provided with an electrode window 11 . The electrode window 11 is correspondingly located on the upper surface of the ridge waveguide structure 9 , and the first electrode 13 is in contact with the grating structure 8 through the electrode window 11 .
[0076] The purpose of providing the electrode window 11 is to make the first electrode 13 contact the grating structure 8 to achieve ohmic contact. The width of the electrode window 11 is smaller than the width of the upper surface of the ridge waveguide structure 9.
[0077] The side of the ridge waveguide structure 9 , namely the side wall of the ridge waveguide, can be protected by covering the ridge waveguide structure 9 with a passivation layer 10 to prevent the side wall of the ridge waveguide structure 9 from leaking electricity and causing a short circuit.
[0078] The material of the passivation layer 10 can be SiN or SiO 2 .
[0079] It should be noted that the passivation layer 10 may be located only on the upper surface and side surfaces of the ridge waveguide structure 9, or may be located on the upper surface and side surfaces of the ridge waveguide structure 9 and the areas on both sides of the ridge waveguide structure 9. When the ridge waveguide structure 9 extends downward from the grating structure 8 to the first waveguide layer 4, the areas on both sides of the ridge waveguide structure 9 are the areas of the first superlattice confinement layer 3 that are not covered by the ridge waveguide structure 9, such as Figure 2 As shown; when the ridge waveguide structure 9 extends downward from the grating structure 8 to the first superlattice confinement layer 3, the areas on both sides of the ridge waveguide structure 9 are the areas of the first outer confinement layer 2 not covered by the ridge waveguide structure 9.
[0080] This application also provides a method for preparing an inter-band cascade laser, please refer to Figure 3 ,include:
[0081] Step S101: growing a first outer confinement layer, a first superlattice confinement layer, a first waveguide layer, an active layer, a second waveguide layer, a second superlattice confinement layer and a second outer confinement layer to be processed in sequence on the upper surface of the substrate; the refractive index of the first outer confinement layer is smaller than that of the first superlattice confinement layer, and the refractive index of the second outer confinement layer to be processed is smaller than that of the second superlattice confinement layer.
[0082] The first outer confinement layer, the first superlattice confinement layer, the first waveguide layer, the active layer, the second waveguide layer, the second superlattice confinement layer and the second outer confinement layer to be processed are epitaxial structure layers. The first outer confinement layer, the first superlattice confinement layer, the first waveguide layer, the second waveguide layer, the second superlattice confinement layer and the second outer confinement layer to be processed are symmetrically arranged in an upper and lower structure with the active layer as the center.
[0083] The material of the epitaxial structure varies depending on the material of the substrate.
[0084] When the substrate is a GaSb substrate, the first outer confinement layer and the second outer confinement layer to be processed may be InAsSb layers, the first superlattice confinement layer and the second superlattice confinement layer may be InAs / AlSb superlattice layers, and the first waveguide layer and the second waveguide layer may be GaSb layers.
[0085] When the substrate is an InAs substrate, the first outer confinement layer and the second outer confinement layer to be processed may be InAs layers, the first superlattice confinement layer and the second superlattice confinement layer may be InAs / AlSb superlattice layers, and the first waveguide layer and the second waveguide layer may be InAs layers.
[0086] As an implementation method, before growing the first outer restriction layer on the substrate, a buffer layer may be grown on the upper surface of the substrate. Accordingly, the first outer restriction layer is grown on the upper surface of the buffer layer.
[0087] The buffer layer can reduce or eliminate the lattice mismatch between the substrate and the first outer confinement layer, can effectively alleviate the stress and dislocation caused by the lattice mismatch, and improve the growth quality of the epitaxial structure.
[0088] Step S102: manufacturing the second outer limiting layer to be processed into a grating structure.
[0089] In this embodiment, there is no limitation on the method of manufacturing the grating structure, which can be selected at will.
[0090] As an implementation method, forming the second outer limiting layer to be processed into a grating structure includes:
[0091] Step S1021a: coating photoresist on the upper surface of the second outer restriction layer to be processed.
[0092] The photoresist is uniformly coated on the entire upper surface of the second outer restriction layer to be processed.
[0093] Step S1022a: exposing and developing the photoresist to form a patterned photoresist.
[0094] Step S1023a: using the patterned photoresist as a mask to etch the second outer restriction layer to be processed to form a grating structure.
[0095] The second outer limiting layer to be processed may be etched in a dry etching manner to form the second outer limiting layer, and the second outer limiting layer is a grating structure.
[0096] As another possible implementation method, forming the second outer limiting layer to be processed into a grating structure comprises:
[0097] Step S1021b: coating photoresist on the upper surface of the second outer restriction layer to be processed.
[0098] Step S1022b: exposing and developing the photoresist to form a patterned photoresist.
[0099] Step S1023b: using the patterned photoresist as a mask to etch the second outer limiting layer to be processed to form a grating structure.
[0100] The difference between this embodiment and the previous embodiment is that the second outer limiting layer to be processed is treated by corrosion, and the corrosion liquid can be a weak acid solution, such as tartaric acid, citric acid, etc.
[0101] Step S103: at least the grating structure, the second superlattice confinement layer, the second waveguide layer, the active layer and the first waveguide layer are made into a ridge waveguide structure.
[0102] As an implementation method, when the ridge waveguide structure extends downward from the grating structure to the first waveguide layer, at least the grating structure, the second superlattice confinement layer, the second waveguide layer, the active layer and the first waveguide layer are made into the ridge waveguide structure, comprising:
[0103] Step S1031: growing a hard mask on the upper surface of the grating structure.
[0104] The hard mask may be grown by chemical vapor deposition, and the material of the hard mask may be silicon nitride, silicon dioxide, or the like.
[0105] Step S1032: making a patterned photoresist on the hard mask.
[0106] The manufacturing process of the patterned photoresist may include coating the photoresist on a hard mask, and then exposing and developing the photoresist to form the patterned photoresist.
[0107] Step S1033: etching the hard mask using the patterned photoresist as a mask to form a patterned hard mask.
[0108] Step S1034: using the patterned hard mask as a mask to etch the grating structure, the second superlattice confinement layer, the second waveguide layer, the active layer and the first waveguide layer to form a ridge waveguide structure, wherein the etching stops at the bottom surface of the first waveguide layer.
[0109] The ridge waveguide structure consists of a second outer confinement layer (ie, a grating structure), a second superlattice confinement layer, a second waveguide layer, an active layer and a first waveguide layer.
[0110] As another possible implementation method, when the ridge waveguide structure extends downward from the grating structure to the first superlattice confinement layer, the processing process is similar to the above implementation method, the difference is that when etching is performed using the patterned hard mask as a mask, the etching cuts off the lower surface of the first superlattice confinement layer.
[0111] Step S104: manufacturing a first electrode on the grating structure and in contact with the grating structure.
[0112] Step S105: thinning the substrate and manufacturing a second electrode on the second surface of the substrate to obtain an interband cascade laser.
[0113] When thinning the substrate, thinning is performed from the second surface of the substrate. The thinning method may be chemical mechanical polishing, and the thickness of the substrate may be thinned to about 150 microns.
[0114] The present application also provides another method for preparing an inter-band cascade laser, comprising:
[0115] Step S201: growing a first outer confinement layer, a first superlattice confinement layer, a first waveguide layer, an active layer, a second waveguide layer, a second superlattice confinement layer and a second outer confinement layer to be processed in sequence on the upper surface of the substrate; the refractive index of the first outer confinement layer is smaller than that of the first superlattice confinement layer, and the refractive index of the second outer confinement layer to be processed is smaller than that of the second superlattice confinement layer.
[0116] like Figure 4 As shown, the first outer confinement layer 2, the first superlattice confinement layer 3, the first waveguide layer 4, the active layer 5, the second waveguide layer 6, the second superlattice confinement layer 7 and the second outer confinement layer to be processed 12 are stacked in sequence on the upper surface of the substrate 1.
[0117] Step S202: manufacturing the second outer limiting layer to be processed into a grating structure.
[0118] like Figure 5 As shown, the second outer limiting layer 12 to be processed is etched to form a second outer limiting layer, and the second outer limiting layer is a grating structure 8.
[0119] Step S203: making the grating structure, the second superlattice confinement layer, the second waveguide layer, the active layer and the first waveguide layer into a ridge waveguide structure.
[0120] like Figure 1 As shown, the ridge waveguide structure 9 is composed of a second outer confinement layer (ie, the grating structure 8 ), a second superlattice confinement layer 7 , a second waveguide layer 6 , an active layer 5 and a first waveguide layer 4 .
[0121] Step S204: depositing a passivation layer on the upper surface and side surfaces of the ridge waveguide structure and the area where the first superlattice confinement layer is not covered by the ridge waveguide structure.
[0122] like Figure 6 As shown, the passivation covers the entire surface of the structure after the previous step.
[0123] Step S205: etching the passivation layer to form an electrode window, wherein the electrode window is located correspondingly on the upper surface of the ridge waveguide structure.
[0124] The passivation layer 10 is subjected to photolithography and etching to form an electrode window 11. Figure 2 shown.
[0125] Step S206: manufacturing a first electrode on the surface of the passivation layer, wherein the first electrode contacts the grating structure through an electrode window.
[0126] like Figure 7 As shown, the first electrode 13 can be deposited by evaporation and forms an ohmic contact with the grating through the electrode window 11.
[0127] Step S207: thinning the substrate and manufacturing a second electrode on the second surface of the substrate to obtain an interband cascade laser.
[0128] like Figure 8 As shown, the second electrode 14 is located on the second surface of the substrate 1 .
[0129] The single-mode interband cascade laser prepared in this application was subjected to PIV test and spectrum test. The PIV test results are as follows: Fig. 9 As shown, the horizontal axis is current, the vertical axis on the left is power, and the vertical axis on the right is voltage. Fig. 9 It can be seen that at different temperatures, the power of the single-mode interband cascade laser is about 6mW, and the laser begins to emit light when the current is applied to about 0.03A. The spectrum test results are as follows Fig.10As shown, the horizontal axis is the wavelength and the vertical axis is the relative intensity. Fig.10 It can be seen that at the same temperature, as the current changes, the emission wavelength of the single-mode interband cascade laser will change, and the current can be determined according to the required wavelength.
[0130] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.
[0131] The above is a detailed introduction to the interband cascade laser and its preparation method provided by the present application. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the scheme and its core idea of the present application. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present application, several improvements and modifications can be made to the present application, and these improvements and modifications also fall within the scope of protection of the present application.
Claims
1. An interband cascade laser, characterized in that: include: Substrate (1); A first hybrid waveguide, a first waveguide layer (4), an active layer (5), a second waveguide layer (6), and a second hybrid waveguide are stacked in sequence from bottom to top on the upper surface of the substrate (1); wherein the first hybrid waveguide comprises a first outer confinement layer (2) and a first superlattice confinement layer (3) stacked in sequence from bottom to top, and the second hybrid waveguide comprises a second superlattice confinement layer (7) and a second outer confinement layer stacked in sequence from bottom to top, the refractive index of the first outer confinement layer (2) is smaller than that of the first superlattice confinement layer (3), and the refractive index of the second outer confinement layer is smaller than that of the second superlattice confinement layer (7); the second outer confinement layer is a grating structure (8), and at least the grating structure (8), the second superlattice confinement layer (7), the second waveguide layer (6), the active layer (5), and the first waveguide layer (4) form a ridge waveguide structure (9); A first electrode (13) located on the grating structure (8) and in contact with the grating structure (8); A second electrode (14) is located on the lower surface of the substrate (1).
2. The interband cascade laser according to claim 1, characterized in that When the substrate (1) is a GaSb substrate, the first outer confinement layer (2) and the second outer confinement layer include InAsSb layers, and the first superlattice confinement layer (3) and the second superlattice confinement layer (7) include InAs / AlSb superlattice layers.
3. The interband cascade laser according to claim 1, characterized in that When the substrate (1) is an InAs substrate, the first outer confinement layer (2) and the second outer confinement layer include InAs layers, and the first superlattice confinement layer (3) and the second superlattice confinement layer (7) include InAs / AlSb superlattice layers.
4. The interband cascade laser according to claim 3, characterized in that In the InAs / AlSb superlattice layer, the thickness of the InAs layer ranges from 22Å to 25Å, and the thickness of the AlSb layer ranges from 22Å to 25Å.
5. The interband cascade laser according to claim 1, characterized in that The second outer confinement layer, the second superlattice confinement layer (7), the second waveguide layer (6), the active layer (5) and the first waveguide layer (4) form a ridge waveguide structure (9).
6. The interband cascade laser according to any one of claims 1 to 5, characterized in that Also includes: A passivation layer (10) is at least located on the upper surface and side surfaces of the ridge waveguide structure (9), the passivation layer (10) is provided with an electrode window (11), the electrode window (11) is correspondingly located on the upper surface of the ridge waveguide structure (9), and the first electrode (13) is in contact with the grating structure (8) through the electrode window (11).
7. A method for preparing an interband cascade laser according to any one of claims 1 to 6, characterized in that: include: A first outer confinement layer (2), a first superlattice confinement layer (3), a first waveguide layer (4), an active layer (5), a second waveguide layer (6), a second superlattice confinement layer (7) and a second outer confinement layer (12) to be processed are sequentially grown on the upper surface of the substrate (1); the refractive index of the first outer confinement layer (2) is smaller than that of the first superlattice confinement layer (3), and the refractive index of the second outer confinement layer (12) to be processed is smaller than that of the second superlattice confinement layer (7); The second outer limiting layer (12) to be processed is made into a grating structure (8); At least the grating structure (8), the second superlattice confinement layer (7), the second waveguide layer (6), the active layer (5) and the first waveguide layer (4) are made into a ridge waveguide structure (9); Fabricating a first electrode (13) on the grating structure (8) and in contact with the grating structure (8); The substrate (1) is thinned, and a second electrode (14) is fabricated on the second surface of the substrate (1) to obtain an interband cascade laser.
8. The method for preparing an interband cascade laser according to claim 7, characterized in that: The step of manufacturing the second outer limiting layer (12) to be processed into a grating structure (8) comprises: Coating a photoresist on the upper surface of the second outer limiting layer (12) to be processed; exposing and developing the photoresist to form a patterned photoresist; The second outer limiting layer (12) to be processed is etched using the patterned photoresist as a mask to form a grating structure (8).
9. The method for preparing an interband cascade laser according to claim 7, characterized in that: At least the grating structure (8), the second superlattice confinement layer (7), the second waveguide layer (6), the active layer (5) and the first waveguide layer (4) are made into a ridge waveguide structure (9), comprising: Growing a hard mask on the upper surface of the grating structure (8); forming a patterned photoresist on the hard mask; Using the patterned photoresist as a mask, etching the hard mask to form a patterned hard mask; The grating structure (8), the second superlattice confinement layer (7), the second waveguide layer (6), the active layer (5) and the first waveguide layer (4) are etched using the patterned hard mask as a mask to form a ridge waveguide structure (9), wherein the etching stops at the lower surface of the first waveguide layer (4).
10. The method for preparing an interband cascade laser according to any one of claims 7 to 9, characterized in that: Before manufacturing a first electrode (13) on the grating structure (8) and in contact with the grating structure (8), the method further comprises: Depositing a passivation layer (10) on the upper surface, the side surface and the regions located on both sides of the ridge waveguide structure (9); Etching the passivation layer (10) to form an electrode window (11), wherein the electrode window (11) is located correspondingly on the upper surface of the ridge waveguide structure (9); Producing a first electrode (13) on the grating structure (8) and in contact with the grating structure (8) comprises: A first electrode (13) is fabricated on the surface of the passivation layer (10), wherein the first electrode (13) is in contact with the grating structure (8) through an electrode window (11).