Perovskite / silicon laminated solar cell and preparation method thereof
By combining perovskite solar cell modules in parallel and connecting them in series with the silicon base cell module, the problem of performance and stability improvement space of perovskite/silicon stacked solar cell is solved, and more efficient photoelectric conversion efficiency and good Resistivity.
Patent Information
- Application Number
- CN202410941796.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The device performance and stability of perovskite/silicon stacked solar cells still have room to improve, especially the complex preparation process of large-area modules and poor film formation uniformity, which has affected its commercial development.
By adjusting the top cell module from a single perovskite solar cell module to multiple perovskite solar sub-cells connected in parallel and connected in series with the silicon base cell module, the circuit series resistance of the top cell module is reduced and the photoelectric conversion efficiency is improved.
While not reducing the overall area of the top battery module, the output short-circuit current and the output open circuit voltage, the conversion efficiency of perovskite/silicon stacked solar cells is improved, and the product yield and resistivity are improved.
Smart Images

Figure CN119012736A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of solar cells, and in particular to a perovskite / silicon stacked solar cell and a preparation method thereof. Background Art
[0002] In recent years, perovskite / crystalline silicon tandem solar cells have become a research hotspot in the photovoltaic field because of their ultra-high efficiency and cost advantages that exceed the theoretical limit of single-junction Shockley-Queisser cells. After nearly ten years of development, the photoelectric conversion efficiency of perovskite / crystalline silicon tandem solar cells has increased from the initial 13.7% to the current 33.9%. However, the complex preparation process of large-area perovskite solar modules and poor film uniformity have seriously hindered the commercialization of perovskite solar cells. At this stage, more and more scientific researchers are committed to the development of efficient and stable large-area perovskite solar modules and the research of tandem cells, and the industrialization prospects of perovskite solar cells are promising.
[0003] In the production of solar cells, there are usually two ways to combine perovskite cells and crystalline silicon cells to prepare tandem cells. One is a parallel four-terminal tandem cell, and the other is a series two-terminal tandem cell. Among them, the two-terminal tandem cell is more suitable for industrialization because of its integrated structure and simple testing, but its many interfaces have a great impact on the photoelectric performance of the device. Therefore, the device performance and stability of perovskite / silicon tandem solar cells still have a lot of room for improvement. Summary of the invention
[0004] The present application provides a perovskite / silicon stacked solar cell and a preparation method thereof, which reduces the circuit series resistance of the top perovskite cell assembly and improves the conversion efficiency without reducing the overall area, output short-circuit current and output open-circuit voltage of the top cell assembly.
[0005] To solve the above technical problems, in the first aspect, an embodiment of the present application provides a perovskite / silicon stacked solar cell, comprising: a bottom cell assembly substrate and a bottom cell assembly, an insulating connection layer, a top cell assembly and a top cell assembly substrate sequentially stacked on the bottom cell assembly substrate; the top cell assembly is a perovskite thin film top cell assembly, and the top cell assembly includes a plurality of perovskite solar sub-cells connected in parallel; the bottom cell assembly is a silicon bottom cell assembly, and the bottom cell assembly and the top cell assembly are connected in series.
[0006] In some exemplary embodiments, the series connection mode of the bottom battery assembly and the top battery assembly is: the positive electrode of the top battery assembly is connected to the negative electrode of the bottom battery assembly; or, the negative electrode of the top battery assembly is connected to the positive electrode of the bottom battery assembly; the output current of the top battery assembly is the same as the output current of the bottom battery assembly.
[0007] In some exemplary embodiments, a perovskite solar subcell includes a substrate and a bottom conductive electrode layer, a hole transport layer, a perovskite light absorbing layer, an electron transport layer, and a top conductive electrode layer sequentially stacked on the substrate.
[0008] In some exemplary embodiments, the bottom cell assembly includes a plurality of silicon solar cell assemblies connected in parallel, and the silicon solar cell assembly includes two half-cells connected in series.
[0009] In some exemplary embodiments, a half-cell is formed by cutting a single crystalline silicon into two halves; the length and width of the half-cell are 182 mm and 91 mm, respectively.
[0010] In some exemplary embodiments, the architecture adopted by the silicon solar cell module is: one of the emitter and back passivation cell technology architecture, the oxide layer passivation contact cell technology architecture, the intrinsic thin film heterojunction cell technology architecture or the cross-finger back contact cell technology architecture.
[0011] In some exemplary embodiments, the area of a single perovskite solar cell in the top cell assembly is calculated by using solar cell parameters and a current matching formula; the solar cell parameters include: the area of a half-cell in the bottom cell assembly, the short-circuit current density of a single perovskite solar cell in the top cell assembly, and the short-circuit current density of a half-cell in the bottom cell assembly; the current matching formula is as follows:
[0012]
[0013] Among them, X1 is the area of a single perovskite solar sub-cell in the top cell assembly, A1 is the short-circuit current density of a single perovskite solar sub-cell in the top cell assembly, Y1 is the area of a half-cell in the bottom cell assembly, and B1 is the short-circuit current density of a half-cell in the bottom cell assembly.
[0014] In some exemplary embodiments, the parallel resistance of the bottom battery assembly is calculated as:
[0015]
[0016] Where n is the number of half-cell batteries.
[0017] In the second aspect, the embodiment of the present application also provides a method for preparing a perovskite / silicon stacked solar cell, comprising the following steps: first, providing a bottom cell assembly substrate; then, arranging a bottom cell assembly on the bottom cell assembly substrate; the bottom cell assembly is a silicon bottom cell assembly; next, preparing a plurality of perovskite solar sub-cells; then, connecting the plurality of perovskite solar sub-cells in parallel to form a top cell assembly; the top cell assembly is a perovskite thin film top cell assembly; next, connecting the bottom cell assembly and the top cell assembly through an insulating connecting layer, and connecting the top cell assembly in series with the bottom cell assembly; finally, arranging a top cell assembly substrate on the top cell assembly.
[0018] In some exemplary embodiments, preparing a perovskite solar sub-cell includes the following steps: first, providing a substrate; then, sequentially forming a bottom conductive electrode layer, a hole transport layer, a perovskite light absorption layer and an electron transport layer on the substrate; finally, forming a top conductive electrode layer on the electron transport layer to obtain a perovskite solar sub-cell.
[0019] The technical solution provided by this application has at least the following advantages.
[0020] The present application provides a perovskite / silicon stacked solar cell and a preparation method thereof, wherein the solar cell comprises: a bottom cell assembly substrate, and a bottom cell assembly, an insulating connection layer, a top cell assembly and a top cell assembly substrate sequentially stacked on the bottom cell assembly substrate; the top cell assembly is a perovskite thin film top cell assembly, and the top cell assembly comprises a plurality of perovskite solar sub-cells connected in parallel; the bottom cell assembly is a silicon bottom cell assembly, and the bottom cell assembly and the top cell assembly are connected in series. The present application adjusts the top cell assembly from a single perovskite solar cell assembly to a parallel combination of multiple perovskite solar sub-cells, thereby reducing the circuit series resistance of the top cell assembly without reducing the overall area of the top cell assembly, the output short-circuit current and the output open-circuit voltage, thereby improving the conversion efficiency; the present application connects the positive / negative electrodes of the top cell assembly formed in parallel with the negative / positive electrodes of the bottom cell assembly to form a series connection mode, so that the output current of the top cell assembly (perovskite thin film top cell assembly) is the same as the output current of the bottom cell assembly (silicon bottom cell assembly), and then the perovskite thin film top cell assembly and the silicon bottom cell assembly are stacked and connected through an insulating connecting layer to form a perovskite / crystalline silicon stacked solar cell with high yield and low resistivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] One or more embodiments are exemplarily described by pictures in the corresponding drawings, and these exemplifications do not constitute limitations on the embodiments. Unless otherwise stated, the pictures in the drawings do not constitute proportional limitations.
[0022] Figure 1A schematic diagram of the structure of a perovskite / silicon tandem solar cell provided in one embodiment of the present application.
[0023] Figure 2 A schematic structural diagram of a bottom battery assembly provided in one embodiment of the present application.
[0024] Figure 3 A schematic diagram of the structure of a top battery assembly provided in one embodiment of the present application.
[0025] Figure 4 A schematic diagram of the structure of a perovskite solar cell provided in one embodiment of the present application.
[0026] Figure 5a A schematic diagram of a connection method between a bottom battery assembly and a top battery assembly provided in one embodiment of the present application.
[0027] Figure 5b A schematic diagram of another connection method for a bottom battery assembly and a top battery assembly provided in an embodiment of the present application.
[0028] Figure 6 A schematic diagram of a process for preparing a perovskite / silicon tandem solar cell provided in one embodiment of the present application. DETAILED DESCRIPTION
[0029] As can be seen from the background technology, in the research and development of solar cells, there is still much room for improvement in the device performance and stability of perovskite / silicon tandem solar cells.
[0030] As an important way to effectively utilize solar energy, the development of solar cells has received increasing attention. Among many photovoltaic devices, perovskite solar cells (PSCs) have developed particularly rapidly in recent years.
[0031] Perovskite (CH3NH3PbI3) solar cells belong to the third generation of solar cells. Their notable feature is that they use perovskite-type organic-inorganic hybrid halide semiconductor materials as light-absorbing layers. The notable feature of organic-inorganic hybrid halide perovskite materials is that they can obtain an adjustable band gap from 1.17eV to 3.1eV by changing their composition. Therefore, perovskite materials are very suitable for building tandem solar cells with photoelectric conversion efficiency exceeding the Shockley-Queisser limit. Silicon solar cells have a wide absorption spectrum, but less absorption of short-wave high-energy spectra, while perovskite solar cells have a narrow spectral range. By controlling the proportion of halogen elements in perovskite materials, their light absorption range can be further moved toward the short-wave direction. Therefore, the preparation of perovskite / silicon tandem solar cells can better realize the full utilization of sunlight, improve the utilization rate of photoexcited hot electrons, and improve the photoelectric conversion efficiency of solar cells.
[0032] Perovskite / crystalline silicon stacked cells are a structure that stacks perovskite solar cells and crystalline silicon solar cells, which achieves an improvement in conversion efficiency through complementary advantages and synergistic effects. This application aims at the main technical challenges of the current connection method of perovskite / crystalline silicon stacked cells, and provides a perovskite / silicon stacked solar cell and a preparation method thereof. The solar cell includes: a bottom cell assembly substrate and a bottom cell assembly, an insulating connection layer, a top cell assembly, and a top cell assembly substrate sequentially stacked on the bottom cell assembly substrate; the top cell assembly is a perovskite thin film top cell assembly, and the top cell assembly includes a plurality of perovskite solar sub-cells connected in parallel; the bottom cell assembly is a silicon bottom cell assembly, and the bottom cell assembly is connected in series with the top cell assembly. This application proposes a new type of perovskite / crystalline silicon stacked module connection method, and adjusts the top cell assembly from a single perovskite solar cell assembly to a parallel combination of multiple perovskite solar sub-cells, while not reducing the overall area of the top cell assembly, the output short-circuit current, and the output open-circuit voltage, while reducing the circuit series resistance of the top cell assembly and improving the conversion efficiency.
[0033] The following will describe the various embodiments of the present application in detail with reference to the accompanying drawings. However, it will be appreciated by those skilled in the art that in the various embodiments of the present application, many technical details are provided in order to enable the reader to better understand the present application. However, even without these technical details and various changes and modifications based on the following embodiments, the technical solution claimed in the present application can be implemented.
[0034] refer to Figure 1The embodiment of the present application provides a perovskite / silicon stacked solar cell, including: a bottom cell assembly substrate 110 and a bottom cell assembly 120, an insulating connection layer 130, a top cell assembly 140 and a top cell assembly substrate 150 sequentially stacked on the bottom cell assembly substrate 110; the top cell assembly 140 is a perovskite thin film top cell assembly, and the top cell assembly 140 includes a plurality of perovskite solar sub-cells connected in parallel; the bottom cell assembly 120 is a silicon bottom cell assembly, and the bottom cell assembly 120 and the top cell assembly 140 are connected in series.
[0035] This application aims to address the main technical challenges of the current stacked battery connection method and proposes a new perovskite / crystalline silicon stacked module connection solution and implementation method. Figure 1 As shown, the perovskite / silicon tandem solar cell provided in the embodiment of the present application has a bottom cell assembly substrate 110 located at the bottom layer, on which a bottom cell assembly 120, an insulating connection layer 130, a top cell assembly 140 (perovskite thin film top cell assembly) and a top cell assembly substrate 150 (perovskite thin film top cell assembly transparent substrate) are sequentially stacked, and the top cell assembly 140 is adjusted from a single perovskite solar cell assembly to a plurality of perovskite solar sub-cells connected in parallel to form a perovskite / crystalline silicon tandem solar cell with high yield and low resistivity. With such a configuration, the present application can reduce the circuit series resistance of the top cell assembly without reducing the overall area of the top cell assembly, the output short-circuit current and the output open-circuit voltage, thereby improving the conversion efficiency.
[0036] In some embodiments, the bottom cell assembly substrate 110 is a general FTO (Fluorine-doped Tin Oxide) or ITO (Indium Tin Oxide) substrate.
[0037] like Figure 2 As shown, in some embodiments, the bottom cell assembly 120 of the present application adopts a commercial half-cell silicon solar cell assembly. The architecture adopted by the silicon solar cell assembly is one of the following: Passivated Emitter Rear Cell (PERC), Tunnel Oxide Passivated Contact (TOPCon), Heterojunction with Intrinsic Thin-film (HJT), or Interdigitated Back Contact (IBC).
[0038] In the production of solar cells, there are two common types of crystalline silicon bottom cells: full-cell cells and half-cell cells. A full-cell cell means that the entire cell is made of a single crystalline silicon, which has a relatively simple manufacturing process, low price, and large temperature rise losses. A half-cell cell means that a single crystalline silicon is cut into two halves and connected to form a cell. In order to ensure that the overall output voltage and current are consistent with those of conventional components, the half-cell battery component generally adopts a series-parallel structure design in the panel design, which is equivalent to two small components connected in parallel. Based on the advantages of high half-cell packaging efficiency, small current mismatch and low component operating temperature, the bottom battery component 120 of the present application adopts a half-cell battery series-parallel structure.
[0039] See also Figure 2 In some embodiments, the bottom battery assembly 120 includes a plurality of silicon solar cell assemblies 1201 connected in parallel, and the silicon solar cell assembly 1201 includes two half-cell batteries 1201a connected in series.
[0040] In some embodiments, a half-cell battery 1201a is formed by cutting a single piece of crystalline silicon into two halves; specifically, compared to a traditional single-piece silicon battery, a half-cell battery 1201a refers to cutting a single piece of crystalline silicon into two halves that are connected separately into battery cells. In order to ensure that the overall output voltage and current are consistent with those of conventional components, the half-cell battery component generally adopts a series-parallel structure design in terms of panel design, which is equivalent to connecting two half-cell batteries 1201a in parallel.
[0041] In some embodiments, the length and width of the half-cell battery 1201a are 182 mm and 91 mm, respectively.
[0042] In some embodiments, the insulating connecting layer 130 between the bottom battery assembly 120 and the top battery assembly 140 is a transparent insulating connecting layer, and the material of the insulating connecting layer 130 is polyoxymethylene, polyethylene, polyvinyl methyl ether, polyvinyl ethyl ether, ethylene propylene copolymer, polyvinyl alcohol, polyvinyl carbazole, polyvinyl acetate, polyvinyl fluoride, polytetrafluoroethylene, polyvinylidene fluoride, vinylidene fluoride and hexafluoropropylene copolymer, polyvinyl chloride, polyvinylidene chloride, polypropylene, polyacrylic acid, polymethyl methacrylate, polyethyl acrylate, poly (α-cyanobutyl acrylate ), polyacrylamide, polyacrylonitrile, polyisobutylene rubber, polychloroprene, polycis-1,4-isoprene, gutta-percha, styrene-butadiene rubber, polycaprolactam, polydecylene formamide, polyhexamethylene adipamide, polyhexamethylene sebacamide, polynonylene urea, polyisophenylene diamine, polyethylene terephthalate, polycarbonate, polyethylene oxide, poly-2,6-dimethyl-p-phenylene ether, polyphenylene sulfide, poly[bis(methylamino)phosphazene], poly[bis(trifluoroethoxy)phosphazene], polydimethylsiloxane, celluloid cellulose or polydiphenyl ether sulfone.
[0043] Figure 3 The top cell assembly 140 is a perovskite thin film top cell assembly, and the top cell assembly 140 includes a plurality of perovskite solar sub-cells 1401 connected in parallel. Figure 3 In the embodiment of the present application, the top battery assembly 140 includes two parallel-connected perovskite solar sub-cells 1401 as an example for illustration. It is understandable that the top battery assembly 140 may also include 3, 4, 5 or other numbers of parallel-connected perovskite solar sub-cells 1401. In a specific embodiment, the number of perovskite solar sub-cells 1401 may be adjusted according to actual conditions.
[0044] Figure 4 The schematic diagram of the structure of the perovskite solar cell provided in one embodiment of the present application is shown. The perovskite solar cell includes a substrate 241 and a bottom conductive electrode layer 242 (transparent electrode), a hole transport layer 243, a perovskite light absorption layer 244, an electron transport layer 245 and a top conductive electrode layer 246 (transparent electrode) stacked on the substrate 241 in sequence. It should be noted that, Figure 4 As shown, the bottom conductive electrode layer 242 and the top conductive electrode layer 246 are both transparent conductive electrode layers.
[0045] Specifically, the materials of the bottom conductive electrode layer 242 and the top conductive electrode layer 246 include ITO, FTO, silver nanowires, carbon nanotubes, ultrathin metals and graphene, etc.; the hole transport layer 243 can be prepared by spin coating, blade coating, slit coating, spray coating, solution gel method, magnetron sputtering, thermal evaporation, electron beam evaporation, reactive plasma deposition and atomic layer deposition, etc. The materials of the hole transport layer 243 include nickel oxide, poly (3,4-ethylenedioxythiophene): poly (styrene sulfonic acid) (PEDOT:PSS) and poly [bis (4-phenyl) (2,4,6-trimethylphenyl) amine] (PTAA) and other polymer semiconductors and 2- (9H-carbazole-9-yl) ethyl) phosphonic acid (2PACz), 2- (3,6-dimethoxy-9 [H-carbazole-9-yl)ethyl]phosphonic acid (MeO-2PACz), 4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid (Me-4PACz) and [4-(7H-dibenzocarbazole-7-yl)butyl]phosphonic acid (4PADCB) and other single-molecule self-assembled layer small molecules; the perovskite light absorption layer 244 is an organic-inorganic hybrid metal halide perovskite material based on formamidine (FA) cations, methylamine (MA) cations, cesium (Cs) cations, lead (Pb) cations, iodine (I) anions, bromine (Br) anions and chloride (Cl) anions, or an inorganic metal halide perovskite material based on cesium (Cs) cations, lead (Pb) cations, iodine (I) anions, bromine (Br) anions and chloride (Cl) anions.
[0046] Furthermore, the bandgap of the perovskite light absorption layer 244 is greater than or equal to 1.55 eV. The preparation method of the perovskite light absorption layer 244 includes a doctor blade coating method, a slit coating method, a spraying method, an inkjet printing method, a screen printing method, a soft cover deposition method, a vapor deposition method, etc. The electron transport layer 245 is prepared by a doctor blade coating method, a slit coating method, a spraying method, a thermal evaporation method, a magnetron sputtering method, a reactive plasma deposition method, and an atomic layer deposition method. The materials of the electron transport layer 245 include fullerene (C60), [6,6]-benzene-C61-butyric acid isomethyl ester (PCBM), [6,6]-phenyl-C71-butyric acid isomethyl ester (PC71BM), tin oxide (SnOx), 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline (BCP), titanium oxide (TiO2), zinc oxide (ZnO) and Zn(O,S), etc.
[0047] Furthermore, the top conductive electrode layer 246 preparation process includes magnetron sputtering, reactive plasma deposition, electron beam evaporation and thermal evaporation, and the materials used include transparent conductive oxides such as ITO, ICO, IWO, IZO and AZO, and metals such as copper, silver, aluminum, and gold. The negative electrode is connected to the electron transport layer 245 in the perovskite solar cell, the electron transport layer 245 is connected to the perovskite light absorption layer 244, the perovskite light absorption layer 244 is connected to the hole transport layer 243, and the hole transport layer 243 is connected to the positive electrode of the perovskite solar cell.
[0048] This application forms a perovskite thin-film top cell assembly by connecting two perovskite solar sub-cells in parallel. Figure 4 In the perovskite thin film top cell assembly, the bottom conductive electrode layer 242 (bottom transparent electrode) is first scribed by the first P1 scribe line, and then the hole transport layer 243, the perovskite light absorption layer 244 and the electron transport layer 245 are scribed by the second P2 scribe line. After the top conductive electrode layer 246 (top transparent electrode) is prepared, the top conductive electrode layer 246, the electron transport layer 245, the perovskite light absorption layer 244 and the hole transport layer 243 are scribed by the third P3 scribe line.
[0049] In some embodiments, the area of a single perovskite solar cell 1401 in the top cell assembly 140 is calculated by using solar cell parameters and a current matching formula; the solar cell parameters include: the area of a half-cell in the bottom cell assembly 120, the short-circuit current density of a single perovskite solar cell 1401 in the top cell assembly 140, and the short-circuit current density of a half-cell 1201a in the bottom cell assembly 120; the current matching formula is as follows:
[0050]
[0051] Among them, X1 is the area of a single perovskite solar sub-cell in the top cell assembly, A1 is the short-circuit current density of a single perovskite solar sub-cell in the top cell assembly, Y1 is the area of a half-cell in the bottom cell assembly, and B1 is the short-circuit current density of a half-cell in the bottom cell assembly.
[0052] In some embodiments, the parallel resistance of the bottom battery assembly 120 is calculated as:
[0053]
[0054] Where n is the number of half-cell batteries.
[0055] In some embodiments, the series connection mode of the bottom battery assembly 120 and the top battery assembly 140 is: the positive electrode of the top battery assembly 140 is connected to the negative electrode of the bottom battery assembly 120; or, the negative electrode of the top battery assembly 140 is connected to the positive electrode of the bottom battery assembly 120; the output current of the top battery assembly 140 is the same as the output current of the bottom battery assembly 120.
[0056] See also Figure 5a and Figure 5b , which are two connection methods of the bottom cell assembly and the perovskite thin film top cell assembly of the perovskite / silicon tandem solar cell assembly provided in the embodiments of the present application. The perovskite thin film top cell assembly includes two perovskite solar sub-cells connected in parallel. After the crystalline silicon bottom cell assembly and the perovskite thin film top cell assembly are completed respectively, the positive / negative electrode of the crystalline silicon bottom cell assembly is connected to the negative / positive electrode of the wide bandgap perovskite thin film top cell assembly. The bottom cell assembly substrate is used as the back cover of the tandem cell assembly, and the top cell assembly substrate is used as the front cover of the tandem cell assembly. A transparent insulating connection layer is used between the crystalline silicon bottom cell assembly and the perovskite thin film top cell assembly to encapsulate and form a perovskite / silicon tandem solar cell assembly.
[0057] The perovskite / silicon tandem solar cell assembly provided in the embodiment of the present application reduces the circuit series resistance of the top perovskite cell assembly and improves the conversion efficiency by adjusting the number of perovskite solar sub-cells connected in parallel in the top cell assembly without reducing the overall area of the top cell assembly, the output short-circuit current, and the output open-circuit voltage. The output current of the top cell assembly 140 is the same as the output current of the bottom cell assembly 120, the positive / negative electrode of the top cell assembly 140 is connected to the negative / positive electrode of the bottom cell assembly 120, and the top cell assembly 140 and the bottom cell assembly 120 are stacked and connected together through an insulating connection layer 130 to form a perovskite / crystalline silicon tandem solar cell module device.
[0058] See also Figure 6 , an embodiment of the present application also provides a method for preparing a perovskite / silicon tandem solar cell, comprising the following steps.
[0059] Step S1, providing a bottom battery assembly substrate.
[0060] Step S2, arranging a bottom cell assembly on a bottom cell assembly substrate; the bottom cell assembly is a silicon bottom cell assembly.
[0061] Step S3, preparing a plurality of perovskite solar cells.
[0062] Step S4, connecting a plurality of perovskite solar sub-cells in parallel to form a top cell assembly; the top cell assembly is a perovskite thin film top cell assembly.
[0063] Step S5, connecting the bottom battery assembly and the top battery assembly through an insulating connection layer, and connecting the top battery assembly and the bottom battery assembly in series.
[0064] Step S6: Dispose a top battery assembly substrate on the top battery assembly.
[0065] In some embodiments, preparing a perovskite solar sub-cell includes the following steps: first, providing a substrate; then, sequentially forming a bottom conductive electrode layer, a hole transport layer, a perovskite light absorption layer, and an electron transport layer on the substrate; finally, forming a top conductive electrode layer on the electron transport layer to obtain a perovskite solar sub-cell.
[0066] In order to further understand the present application, the present application is described below in conjunction with specific embodiments, but the embodiments are only for further elaboration of the features and advantages of the present application, rather than for limitation of the claims of the present application.
[0067] It should be noted that before preparing the perovskite / silicon tandem solar cell, a commercial crystalline silicon half-cell solar cell module is first prepared. In this embodiment, a commercial crystalline silicon half-cell solar cell module is used as the bottom cell module of the tandem perovskite / silicon cell module. The module size of the commercial crystalline silicon half-cell solar cell module used in this embodiment is 2278mm (length) × 1134mm (width) × 30mm (thickness). The commercial crystalline silicon half-cell solar cell module used in this embodiment contains 144 crystalline silicon half-cell cells, and the length and width of the crystalline silicon half-cell cell are 182mm×91mm respectively. The short-circuit current of the commercial crystalline silicon half-cell solar cell module used in this embodiment is 14.05 A at one sun intensity, and the short-circuit current density of a single half-cell silicon cell in the module is 42.41mAcm -2 .
[0068] An embodiment of the present application provides a method for preparing a perovskite / silicon tandem solar cell, comprising the following steps.
[0069] Step 1: Remove dust, organic stains, etc. on the surface of a glass substrate with a thickness of 2 mm to 4 mm, a length of 2278 mm, and a width of 1134 mm by cleaning with a detergent, ultrapure water, hot air drying, and ultraviolet ozone cleaning.
[0070] Step 2: Use magnetron sputtering to deposit ITO (In2O3:Sn) bottom conductive electrode layer on a glass substrate. The substrate temperature is heated to 250°C, the argon flow rate is 20sccm, the hydrogen flow rate is 2.5sccm, the sputtering power is 750W, the sputtering pressure is 0.5Pa, and the thickness is 200nm.
[0071] Step 3: After depositing the ITO bottom conductive electrode layer, the ITO layer is divided into ITO strips by using the first laser scribing line P1 in the direction parallel to the long side of the glass substrate. The length and width of each ITO strip are 2278 mm and 5 mm respectively, and the ITO strips are not electrically connected to each other. The scribing width of P1 is 30 μm, and the laser used for P1 laser scribing is generated by a 1064 nm nanosecond laser.
[0072] Step 4: Clean the ITO glass substrate after the laser scribing P1 according to the cleaning method described in step 1.
[0073] Step 5, forming a hole transport layer: After the ITO glass is cleaned in step 4, a 2PACz solution (0.2 mg / mL to 3 mg / mL ethanol solution) is coated on the ITO substrate by slit coating. The slit coating die is 200 μm away from the substrate, and the coating speed is 30 mm / s. After the 2PACz solution film is coated, the substrate is heated at 100°C for 10 minutes and then naturally cooled to room temperature.
[0074] Step 6. The composition of the perovskite solution is FAPbI3+35mol%MACl, the concentration of FAPbI3 is 1.0M, and the solvent is DMF:NMP=6:1 (vt%).
[0075] Step 7: Apply the perovskite solution on the 2PACz-covered ITO substrate by slit coating. The slit coating die head is 250 μm away from the substrate, and the coating speed is 50 mm / s. After the perovskite solution film is coated, the substrate covered with the perovskite film is placed in a vacuum flash evaporation device for 30 seconds to complete the pre-crystallization process. The pressure of the vacuum flash evaporation device can be reduced to 3 Pa within 10 seconds. After the perovskite pre-crystallization is completed, the substrate is heated at 170°C for 15 minutes to form a perovskite light-absorbing layer, and then naturally cooled to room temperature.
[0076] Step 8: Forming an electron transport layer: Vacuum thermal evaporation is used to deposit 5nm~50nm thick C60 on the perovskite light absorption layer at a temperature of 500°C. Then, an atomic layer deposition (ALD) method is used to prepare a 5nm~30nm thick SnO x Tetrakis(dimethylamino)tin (TDMASn) is the ALD tin source, and ultrapure water is the ALD oxygen source.
[0077] Step 9: At 40 μm to the right of laser scribing P1, a second laser scribing P2 is used in a direction parallel to P1 to separate the hole transport layer / perovskite light absorption layer / electron transport layer of the perovskite thin film sample prepared with the SnOx layer. The scribing width of P2 is 50 μm, and the laser used for P2 laser scribing is generated by a 355 nm or 532 nm picosecond laser.
[0078] Step 10: Prepare an ITO top transparent conductive electrode on the perovskite film sample with P2 marking by magnetron sputtering. Heat the substrate to 250°C, with an argon flow rate of 20 sccm, a hydrogen flow rate of 2.5 sccm, a sputtering power of 750 W, a sputtering pressure of 0.5 Pa, and a thickness of 100 nm.
[0079] Step 11, at 40 μm to the right of laser scribe line P2, use a third laser scribe line P3 in a direction parallel to P2 to scribe the hole transport layer / perovskite light absorption layer / electron transport layer / ITO layer of the perovskite thin film sample prepared with the transparent conductive electrode on the top of ITO to form a perovskite thin film top battery assembly. The scribe line width of P3 is 40 μm. The laser used for P3 laser scribe line is generated by a 355nm or 532nm picosecond laser.
[0080] Step 12, repeat step 1 to step 11 to prepare the remaining two top perovskite solar sub-cell modules. Connect the positive electrodes of sub-module 1, sub-module 2 and sub-module 3 to form the top perovskite solar cell group. Connect the negative electrodes of sub-module 1, sub-module 2 and sub-module 3 to form the negative electrode of the top cell module (top perovskite solar cell module).
[0081] Step 13: Cover the two prepared perovskite thin-film top cell modules on the commercial crystalline silicon half-cell solar cell module prepared in advance in the embodiment of the present application. Under one sunlight intensity, measure: (1) the output short-circuit current of a perovskite thin-film top cell module and the short-circuit current density of a single sub-cell in the module; (2) the output short-circuit current of the commercial crystalline silicon half-cell solar cell module and the short-circuit current density of a single half-cell silicon cell in the module when the incident light is filtered by the perovskite thin-film top cell module and irradiated on the commercial crystalline silicon half-cell solar cell module.
[0082] Step 14: Under one solar intensity, the output short-circuit current of the perovskite thin-film top cell assembly prepared according to steps 1 to 12 is 2.90 A, and the short-circuit current density of a single sub-cell in the assembly is 25.46 mA cm -2 .
[0083] Step 15: Under one sunlight intensity, after filtering by the perovskite thin-film top cell assembly prepared according to steps 1 to 12, the output short-circuit current of the commercial crystalline silicon half-cell solar cell assembly is 5.60A, and the short-circuit current density of a single half-cell silicon cell in the assembly is 16.90mAcm -2 .
[0084] Step 16: In this embodiment, the area of the laminated battery assembly is M=2.58m 2The area of a single subcell in the perovskite thin-film top cell assembly is X1=113.90cm 2 The area of a single half-cell silicon cell in a crystalline silicon half-cell solar cell module is Y1=165.62 cm 2 The short-circuit current density of a single sub-cell of the perovskite thin-film top cell module is A1=25.46 mAcm -2 And the short-circuit current density of a single half-cell silicon cell in a crystalline silicon half-cell solar cell module is B1=16.90 mAcm -2 According to the current matching calculation formula that the perovskite thin-film top cell module and the crystalline silicon half-cell solar cell module must meet: X1*A1=2 * (Y1*B1), the area of a single sub-cell in the perovskite thin-film top cell module must be adjusted to X1=219.87cm 2 , that is, the width of each ITO strip is adjusted to 9.65mm.
[0085] Step 17: Prepare a perovskite thin-film top cell assembly according to the method steps described in steps 1 to 12, except that the width of each ITO strip described in step 3 is adjusted from 5 mm to 9.65 mm.
[0086] Step 18, connect and cover the two perovskite thin film top cell modules prepared according to step 17 on the commercial crystalline silicon half-cell solar cell module prepared in advance in this application. The perovskite solar sub-cells are connected in parallel to form a top cell module, the negative electrode / positive electrode of the perovskite thin film top cell module is connected to the positive electrode / negative electrode of the crystalline silicon half-cell bottom cell module, and the perovskite thin film top cell module and the crystalline silicon half-cell bottom cell module are connected together through a transparent insulating connection layer to form a new type of perovskite / silicon laminated solar cell module.
[0087] Based on the above technical scheme, the present application provides a perovskite / silicon stacked solar cell and a preparation method thereof, a bottom cell assembly substrate, and a bottom cell assembly, an insulating connection layer, a top cell assembly and a top cell assembly substrate sequentially stacked on the bottom cell assembly substrate; the top cell assembly is a perovskite thin film top cell assembly, and the top cell assembly includes a plurality of perovskite solar sub-cells connected in parallel; the bottom cell assembly is a silicon bottom cell assembly, and the bottom cell assembly and the top cell assembly are connected in series. The present application adjusts the top cell assembly from a single perovskite solar cell assembly to a parallel combination of multiple perovskite solar sub-cells, thereby reducing the circuit series resistance of the top cell assembly without reducing the overall area of the top cell assembly, the output short-circuit current and the output open-circuit voltage, thereby improving the conversion efficiency; the present application connects the positive / negative electrodes of the top cell assembly formed in parallel with the negative / positive electrodes of the bottom cell assembly to form a series connection mode, so that the output current of the top cell assembly (perovskite thin film top cell assembly) is the same as the output current of the bottom cell assembly (silicon bottom cell assembly), and then the perovskite thin film top cell assembly and the silicon bottom cell assembly are stacked and connected through an insulating connecting layer to form a perovskite / crystalline silicon stacked solar cell with high yield and low resistivity.
[0088] Those skilled in the art can understand that the above-mentioned embodiments are specific examples for implementing the present application, and in practical applications, various changes can be made to them in form and detail without departing from the spirit and scope of the present application. Any person skilled in the art can make their own changes and modifications without departing from the spirit and scope of the present application, so the scope of protection of the present application shall be based on the scope defined in the claims.
Claims
1. A perovskite / silicon tandem solar cell, characterized in that: include: A bottom battery assembly substrate, and a bottom battery assembly, an insulating connection layer, a top battery assembly, and a top battery assembly substrate sequentially stacked on the bottom battery assembly substrate; The top cell assembly is a perovskite thin film top cell assembly, and the top cell assembly includes a plurality of perovskite solar sub-cells connected in parallel; The bottom cell assembly is a silicon bottom cell assembly, and the bottom cell assembly is connected in series with the top cell assembly.
2. The perovskite / silicon tandem solar cell according to claim 1, characterized in that: The bottom battery assembly and the top battery assembly are connected in series in the following modes: the positive electrode of the top battery assembly is connected to the negative electrode of the bottom battery assembly; or the negative electrode of the top battery assembly is connected to the positive electrode of the bottom battery assembly; The output current of the top cell assembly is the same as the output current of the bottom cell assembly.
3. The perovskite / silicon tandem solar cell according to claim 1, characterized in that: The perovskite solar cell comprises a substrate and a bottom conductive electrode layer, a hole transport layer, a perovskite light absorption layer, an electron transport layer and a top conductive electrode layer sequentially stacked on the substrate.
4. The perovskite / silicon tandem solar cell according to claim 1, characterized in that: The bottom cell assembly comprises a plurality of silicon solar cell assemblies connected in parallel, and the silicon solar cell assembly comprises two half-cell cells connected in series.
5. The perovskite / silicon tandem solar cell according to claim 4, characterized in that: The half-cell battery is formed by cutting a single crystalline silicon into two half-cells equally; The length and width of the half-cell battery are 182 mm and 91 mm respectively.
6. The perovskite / silicon tandem solar cell according to claim 4, characterized in that: The architecture adopted by the silicon solar cell module is one of: an emitter and back passivation cell technology architecture, an oxide layer passivation contact cell technology architecture, an intrinsic thin film heterojunction cell technology architecture or an interdigitated back contact cell technology architecture.
7. The perovskite / silicon tandem solar cell according to claim 4, characterized in that: The area of a single perovskite solar cell in the top cell assembly is calculated using solar cell parameters and a current matching formula; The solar cell parameters include: the area of a half-cell in the bottom cell assembly, the short-circuit current density of a single perovskite solar subcell in the top cell assembly, and the short-circuit current density of a half-cell in the bottom cell assembly; The current matching formula is as follows: , Among them, X1 is the area of a single perovskite solar sub-cell in the top cell assembly, A1 is the short-circuit current density of a single perovskite solar sub-cell in the top cell assembly, Y1 is the area of a half-cell in the bottom cell assembly, and B1 is the short-circuit current density of a half-cell in the bottom cell assembly.
8. The perovskite / silicon tandem solar cell according to claim 4, characterized in that: The calculation formula of the parallel resistance of the bottom battery assembly is: , Where n is the number of half-cell batteries.
9. A method for preparing a perovskite / silicon tandem solar cell, characterized in that: The following steps are involved: Providing a bottom cell assembly substrate; A bottom cell assembly is arranged on the bottom cell assembly substrate; the bottom cell assembly is a silicon bottom cell assembly; Prepare multiple perovskite solar subcells; Connecting multiple perovskite solar sub-cells in parallel to form a top cell assembly; the top cell assembly is a perovskite thin film top cell assembly; Connecting the bottom battery assembly and the top battery assembly through an insulating connection layer, and connecting the top battery assembly and the bottom battery assembly in series; A top cell assembly substrate is disposed on the top cell assembly.
10. The method for preparing a perovskite / silicon tandem solar cell according to claim 9, characterized in that: The preparation of a perovskite solar cell comprises the following steps: providing a substrate; forming a bottom conductive electrode layer, a hole transport layer, a perovskite light absorption layer and an electron transport layer in sequence on the substrate; A top conductive electrode layer is formed on the electron transport layer to obtain a perovskite solar cell.
Citation Information
Patent Citations
Perovskite crystalline silicon laminated solar cell and preparation method thereof
CN117979725A
Crystalline silicon two-end laminated solar cell and preparation method thereof
CN118173635A
Perovskite / silicon laminated solar cell module and preparation method thereof
CN118175861A
Voltage matching tandem solar module
JP2024058455A