Porous spherical silica, catalyst carrier, cosmetic, analytical column, abrasive, resin composition, and method for producing porous spherical silica
Through the process of gelation and spray-drying in liquid, combined with high temperature firing, porous spherical silica is prepared with high hardness and durability, which solves the problems of easy disintegration and pore blockage of porous silica. It is suitable for Catalysts, analytical columns and cosmetics fields.
Patent Information
- Application Number
- CN202480002104.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-06
- Filing Date
- 2024-02-29
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-02-29
AI Technical Summary
Porous silica is prone to disintegration during long-term use, has poor durability, and the porous structure is prone to clogging or deforming the particle shape during the firing process, resulting in poor handling in applications such as catalyst support, analytical column fillers and cosmetic additives. .
By gelling the vapor-phase silica dispersion in the liquid and spray-drying it, then firing it at high temperature, independently spherical porous spherical silica with low alkali metal content, high particle hardness and few fragmented particles were prepared. , avoid particle aggregation and crushing processes, and maintain the integrity of the porous structure.
It improves the pore capacity and hardness of porous spherical silica, extends its service life, enhances the durability of catalysts and analysis columns, improves the touch of cosmetics and the handling of industrial products.
Smart Images

Figure BDA0005075293960000201
Abstract
Description
Technical Field
[0001] The present invention relates to novel porous spherical silica, a catalyst carrier, a cosmetic, an analytical column, an abrasive, a resin composition and a method for producing the porous spherical silica. Background Art
[0002] Various studies have been conducted on porous silica, and porous silica with various physical properties has been proposed. Porous silica can be manufactured, for example, by the following methods: adding an inorganic acid to an alkali metal silicate aqueous solution for neutralization, and separating / recovering the generated particles (Patent Document 1); a method for spray drying a fumed silica dispersion (Patent Document 2); a method for gelling a fumed silica dispersion in a liquid (Patent Document 3). The porous silica manufactured by the above method is characterized by pore volume and pore size, and is expected to be used as a carrier for a catalyst and a filler for an analytical column. In addition, when used as an abrasive for industrial products, the resin will penetrate into the pores and is therefore easily fixed to the resin of the polishing pad. When a spherical product is used in the above-mentioned application, it has the advantages of being easy to adjust the particle size and improving the filling rate. In addition, the porous spherical silica has a smooth touch due to its shape, so it can also be used as a cosmetic additive.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: International Publication No. 2004 / 101139 Pamphlet
[0006] Patent Document 2: International Publication No. 2019 / 131873 Pamphlet
[0007] Patent Document 3: International Publication No. 2022 / 154014 Pamphlet
[0008] Non-patent literature
[0009] Non-patent document 1: "Sintering of fine ceramics", Journal of the Society of Powder Engineering, Vol. 25, No. 12, (1988), p. 805-811 Summary of the invention
[0010] Problem that the invention aims to solve
[0011] However, since porous silica has the easy disintegration from its porous structure, there is a problem in durability in the use of the filler of the analytical column used in the carrier of the catalyst used for a long time and the fluid. In addition, in the use of the abrasive of industrial products, there is a problem that the particle shape is deformed, the particles are destroyed and the handling property is deteriorated in the process of mixing to the resin. Usually, as a method to improve the hardness of inorganic materials, the method of calcination is adopted (non-patent document 1), and for the porous silica recorded in patent document 1 using sodium silicate as raw material, the melting point is lowered because it contains sodium from the raw material, resulting in pore blockage when calcined at high temperature, and the porous structure cannot be maintained.
[0012] For the porous silica described in the patent document 2 obtained by spray drying the fumed silica dispersion, it is impossible to obtain the silica with low compression strength and high hardness after firing. For the porous silica described in the patent document 3 obtained by gelling the fumed silica dispersion in liquid, particles will gather due to firing, and a crushing process is required, and fragmented micropowder will be produced in the process, and the circularity of the whole particle is reduced. When the porous spherical silica is used for the purpose of the filler of the analysis column, the mixing of the above-mentioned micropowder will become the main cause of column clogging, and in addition, when the porous spherical silica is used as a cosmetic additive, the tactile property deteriorates.
[0013] Therefore, an object of the present invention is to provide porous spherical silica having a reduced alkali metal content, high particle hardness, and a reduced number of fragmentary particles, and a method for producing the same.
[0014] Solutions for solving problems
[0015] The inventors of the present invention have repeatedly conducted in-depth research to solve the above-mentioned problems. As a result, it was found that in the manufacturing process of porous spherical silica, a fumed silica dispersion is gelled in a liquid to obtain a gel, which is spray-dried and then calcined, so that an independent spherical porous spherical silica with a reduced alkali metal content, high particle hardness, and a reduced number of fragmented particles can be manufactured, thereby completing the following present invention.
[0016] [1] A porous spherical silica, characterized in that: the volume-based cumulative 50% particle size (D50) measured by a Coulter counter method is in the range of 2 μm or more and 200 μm or less,
[0017] Similarly, the ratio (D10 / D90) of the cumulative 10% particle size (D10) to the cumulative 90% particle size (D90) is 0.3 or more.
[0018] The pore volume based on the BJH method is 0.5 ml / g or more and 8 ml / g or less,
[0019] The mode value of the pore radius based on the BJH method is 5 nm or more and 50 nm or less.
[0020] The specific surface area based on the BET method is 50 m 2 / g and above 400m 2 / g or less,
[0021] The arithmetic mean value of the "test force at which the sample was confirmed to be broken" for 10 particles was obtained by the method specified in JIS Z8844 with the loading speed set to 0.4462 mN / s, and was 1.0×10 1 mN or more and 2.0×10 1 Below mN,
[0022] Among the 200 particles observed in the SEM image, less than 20 particles had a circularity of 0.7 or less.
[0023] The alkali metal content is 50 ppm or less.
[0024] [2] A catalyst carrier comprising the porous spherical silica described in [1].
[0025] [3] A cosmetic comprising the porous spherical silica described in [1].
[0026] [4] An analytical column comprising the porous spherical silica described in [1].
[0027] [5] An abrasive comprising the porous spherical silica described in [1].
[0028] [6] A resin composition comprising the porous spherical silica described in [1].
[0029] [7] A method for producing porous spherical silica, comprising the following steps:
[0030] A step of preparing a W / O emulsion comprising an aqueous phase in which fumed silica is dispersed and an organic phase having a water-insoluble solvent as a main component;
[0031] The step of heating the emulsion to gel the aqueous phase to obtain a gel dispersion;
[0032] The step of recovering the generated gel from the liquid and spray drying it; and
[0033] A step of calcining the obtained porous spherical silica at a temperature of 900 to 1500° C. for 10 to 25 hours.
[0034] [8] The method for producing porous spherical silica according to [7], characterized in that the spraying method of spray drying is a two-fluid nozzle method.
[0035] Effects of the Invention
[0036] The porous spherical silica of the present invention has a high pore volume and has high hardness as shown by the height of "test force when sample destruction is confirmed", so even if it is used for a long time or used in a fluid, the disintegration of particles or the clogging of holes will not occur, and the porous structure can be maintained. Therefore, the porous spherical silica of the present invention can improve the durability required by the carrier of the catalyst, the adsorbent material of carbon dioxide, etc., and the filler of the analytical column. Furthermore, when used as an abrasive for industrial products, the particle strength that can withstand mixing with resin is reached, and the handling property in the manufacturing process is improved.
[0037] Furthermore, as shown by the high D10 / D90, the width of the particle size distribution is narrow, so when used as a filler for an analytical column, clogging due to the entry of fine powder into the gaps between particles is less likely to occur.
[0038] Furthermore, if 20 or less particles have a circularity of 0.7 or less out of 200 particles observed in the SEM image, the number of fragmented particles decreases and the particles become independent spherical. Therefore, when used as a cosmetic additive, a smooth touch can be imparted.
[0039] In addition, when the alkali metal content is 50 ppm or less, the purity is high, and it is extremely useful as a polishing agent for materials such as semiconductors that are not suitable for containing alkali metals.
[0040] The manufacturing method of the present invention suppresses the aggregation of particles by spray drying the base material and then calcining it, so that the manufacturing method can be carried out by a process that does not include a crushing process. Thus, when the crushing process is implemented, the possible generation of fragmented particles can be suppressed, and the porous spherical silica having the above-mentioned characteristics can be manufactured without generating fine powder and reducing the overall roundness of the particles.
[0041] In addition, the production method of the present invention performs sintering under specific conditions, thereby increasing the bonding strength between primary particles, thereby obtaining porous spherical silica with high particle hardness. DETAILED DESCRIPTION
[0042] The embodiments described below are examples of the present invention, and the present invention is not limited to these embodiments.
[0043] <Porous spherical silica>
[0044] For the porous spherical silica of the present invention, the volume-based cumulative 50% particle size (D50) in the particle size distribution measured by the Coulter counter method is in the range of 2 μm or more and 200 μm or less, and the ratio (D10 / D90) of the cumulative 10% particle size (D10) to the cumulative 90% particle size (D90) obtained is 0.3 or more. If the porous spherical silica is in the above range, the column is not easily clogged when used as a filler for an analytical column, and filling becomes easy. D50 is preferably 2 μm or more and 100 μm or less, particularly preferably 5 μm or more and 50 μm or less, and further preferably 5 μm or more and 20 μm or less. In addition, D10 / D90 is preferably 0.4 or more, and more preferably 0.5 or more. It should be noted that D10 / D90 will not exceed 1.0, and is generally 0.6 or less.
[0045] For the porous spherical silica of the present invention, the pore volume measured by the following BJH method is 0.5ml / g or more and 8ml / g or less. It is difficult to obtain a porous spherical silica with a pore volume as large as more than 8ml / g. If it is less than 6ml / g, it is easier to manufacture, if it is less than 4ml / , it is further easy to manufacture, and if it is less than 2.5ml / g, it is particularly easy to manufacture. In particular, in the case of using the porous spherical silica of the present invention as a carrier of a catalyst, an adsorbent material of carbon dioxide, etc., in order to have a high loading or adsorption capacity, the pore volume is preferably more than 0.6ml / g, more preferably more than 0.7ml / g, and more preferably more than 1.0ml / g.
[0046] The mode value of the pore radius based on the BJH method is 5 nm or more, preferably 10 nm or more, and more preferably 15 nm or more. The upper limit is 50 nm or less, and preferably 30 nm or less.
[0047] It should be noted that the pore volume and pore radius based on the BJH method are obtained by drying the sample of the measurement object at a temperature of 200°C for more than 3 hours under a vacuum of less than 1 kPa, and then obtaining an adsorption isotherm on the adsorption side of only nitrogen at liquid nitrogen temperature, and analyzing it using the BJH method (Barrett, EP; Joyner, LG; Halenda, PP, J. Am. Chem. Soc. 73, 373 (1951)). The "mode value of the pore radius based on the BJH method" refers to the value of the pore radius when the pore distribution curve (volume distribution curve) obtained by the above-mentioned BJH method, which is plotted with the differential of the cumulative pore volume based on the logarithm of the pore radius as the vertical axis and the pore radius as the horizontal axis, takes the maximum value.
[0048] The porous spherical silica of the present invention has a specific surface area of 50 m 2 / g and above 400m 2 / g or less. The specific surface area is preferably 100m 2 / g or more, particularly preferably 120m 2 / g and above and 350m 2 / g or less. The higher the specific surface area of the fumed silica used as the raw material, the higher the specific surface area of the porous spherical silica. In addition, the higher the specific surface area of the fumed silica, the easier it is to gel and to form into a spherical shape. However, the specific surface area of fumed silica is usually around 400m 2 / g or less, so it is difficult to obtain a specific surface area exceeding 400m 2 / g of porous spherical silica. It should be noted that the specific surface area is a value obtained based on a nitrogen adsorption BET multipoint method.
[0049] For the porous spherical silica of the present invention, the arithmetic mean value of the "test force when the sample is confirmed to be broken" (hereinafter referred to as "test force at break") for 10 particles obtained by the method specified in JIS Z8844:2019 with the loading speed set to 0.4462 mN / sec is 1.0×10 1 ~2.0×10 1 If the test force at failure exceeds 2.0×10 1 mN, it is difficult to obtain porous spherical silica with a pore volume of 0.5 ml / g or more. 1 ~1.8×10 1 If the test force at the time of destruction is within the above range, the particle hardness is high and porous spherical silica having the target durability is obtained.
[0050] The alkali metal content of the porous spherical silica of the present invention is 50 ppm or less (mass basis), and is particularly preferably 40 ppm or less, and more preferably 30 ppm or less.
[0051] For the porous spherical silica of the present invention, its shape is spherical. Here, spherical means that the average circularity obtained by image analysis using a scanning electron microscope (SEM) is 0.8 or more. "Average circularity obtained by image analysis" refers to the sum of the circularity obtained by image analysis of SEM images by observing more than 2000 porous spherical silicas at a magnification of 1000 times using SEM. Here, "circularity" is the value obtained by the following formula (1).
[0052] C=4πS / L 2 (1)
[0053] In the above formula (1), C represents circularity, S represents the area (projected area) occupied by the porous spherical silica in the image, and L represents the length (perimeter) of the outer periphery of the porous spherical silica in the image. The average circularity is particularly preferably 0.85 or more.
[0054] For the porous spherical silica of the present invention, among 200 particles observed in the SEM image, the number of fragmentary particles is 20 or less. Here, fragmentary particles refer to particles having a circularity of 0.7 or less calculated according to the above definition. The number of fragmentary particles is preferably 15 or less, and more preferably 10 or less.
[0055] In addition, the porous spherical silica of the present invention can be either hydrophilic or hydrophobic. The porous spherical silica of the present invention manufactured by the manufacturing method described later is hydrophilic. The hydrophobic porous spherical silica can be obtained by appropriately applying the method of silica surface treatment after obtaining the hydrophilic porous spherical silica by the manufacturing method. It should be noted that "hydrophilic" here means that it can be dispersed in water without an organic solvent.
[0056] The porous spherical silica of the present invention has the above-mentioned properties and can be used as a carrier of catalysts or fragrances, an adsorbent of carbon dioxide, etc., a filler for analytical columns, a cosmetic additive, a polishing agent for industrial products, etc., and an additive for various resin compositions.
[0057] <Method for producing porous spherical silica>
[0058] The method for manufacturing the porous spherical silica of the present invention is not particularly limited, and the above-mentioned high pore volume and the mode particle size of the pore radius can be easily achieved by using a fumed silica dispersion as a raw material. Usually, fumed silica has a structure formed by the aggregation of particulate silica (primary particles). Therefore, a fumed silica dispersion is used as the raw material of porous spherical silica, and the fumed silica in the dispersed liquid is gelled to form a network, thereby suppressing the pore volume reduction caused by drying shrinkage, and a porous spherical silica with a high pore volume can be obtained.
[0059] More specifically, the following method can be cited: preparing a W / O emulsion including an aqueous phase in which fumed silica is dispersed and an organic phase having a non-water-soluble solvent as a main component (W / O emulsion preparation step), then heating the emulsion to gel the aqueous phase to obtain a porous spherical silica dispersion (gelation step), then recovering the generated porous spherical silica from the liquid (gel recovery step), spray drying (drying step), and calcining (calcination step) to produce porous spherical silica. Each step is described in detail below.
[0060] (W / O emulsion preparation process)
[0061] As a method for preparing a W / O emulsion comprising an aqueous phase in which fumed silica is dispersed and an organic phase having a non-water-soluble solvent as a main component, the following method is particularly preferred: first, a dispersion liquid in which fumed silica is dispersed in an aqueous phase is prepared (dispersion liquid preparation step), and the dispersion liquid and an organic solvent are used to prepare an emulsion according to a conventional method (emulsification step). These are further described below.
[0062] (Dispersion liquid preparation process)
[0063] The dispersion preparation step is a step of dispersing fumed silica in water to prepare a dispersion.
[0064] The fumed silica used can be dispersed in water and can be gelled by heating, adjusting pH, etc. This property is achieved by having a large number of silanol groups on the surface of the silica. Therefore, most fumed silica that has not been so-called surface treated can be used. In addition, from the perspective of easy gelation, it is preferred to use a fumed silica with a specific surface area of 100 m 2 / g or more, especially 200m 2 More preferably, it is 250 m 2 / g or more. The larger the specific surface area, the faster the gelation rate, and the easier it is to gel the droplets (W phase) in which the fumed silica is dispersed. From the perspective of easy availability, it is preferred to use 400m 2 The upper limit is 10000 g. It should be noted that the specific surface area is a value obtained by a nitrogen adsorption BET multipoint method.
[0065] In addition, the larger the specific surface area of the fumed silica used as a raw material, the larger the specific surface area of the porous spherical silica obtained by the method described herein. Therefore, according to the specific surface area of the target porous spherical silica, the fumed silica used as a raw material is appropriately selected, and the specific surface area of the porous spherical silica can be arbitrarily controlled without changing the manufacturing conditions. It should be noted that the fumed silica used in the present invention can also be used by mixing different specific surface areas.
[0066] The above-mentioned fumed silica is commercially available, and for example, various hydrophilic grades of Reolosil from Tokuyama Co., Ltd., various hydrophilic grades of AEROSIL from Nippon AEROSIL Co., Ltd., and various hydrophilic grades of dry silica HDK from Asahi Kasei Wacker Silicone Co., Ltd. can be used.
[0067] Furthermore, since fumed silica is generally high-purity and contains almost no impurities such as alkali metals, the alkali metal content of the produced porous spherical silica can also be reduced to an extremely low level.
[0068] As a solvent for this step, water is essential, but other solvents may be included within the range that does not hinder emulsion formation and subsequent gelation. In addition, when a latent base is used to promote gelation described later, the fumed silica may be dissolved in water before dispersing it.
[0069] As a method for dispersing fumed silica in a solvent, it is preferred to prepare a dispersion in which fumed silica is pre-dispersed in a solvent, and to perform microdispersion using a crusher or the like. Specific examples of crushers that can be used for microdispersion include ball mills, bead mills, vibration mills, pin mills, atomizers, colloid mills, homogenizers, high-pressure homogenizers, and ultrasonic homogenizers. As the degree of dispersion after microdispersion, when the particle size distribution of the dispersion is measured by a laser diffraction scattering method, it is preferred that the D90 value reaches 0.5 μm or less.
[0070] The silica concentration in the fumed silica dispersion is preferably in the range of 10% to 30% by mass. In addition, it is more preferably 15% by mass or more, and particularly preferably 20% by mass or more. The higher the silica concentration in the fumed silica dispersion, the faster the gelation rate. However, when the concentration is too high, the fluidity is lost, and it is difficult to prepare a fumed silica dispersion.
[0071] It should be noted that heating will accelerate the gelation of the fumed silica dispersion. When the gelation of the fumed silica dispersion is carried out in the above-mentioned dispersion preparation process, it is difficult for the W phase to form a sphere in the subsequent emulsification process. In extreme cases, the formation of the emulsion itself becomes difficult. Therefore, in the dispersion preparation process, the liquid temperature of the fumed silica dispersion is preferably maintained below room temperature (20°C). In cases where the specific surface area or concentration of the fumed silica is high and gelation is easy to proceed, cooling to a temperature below room temperature (preferably below 15°C, more preferably below 12°C) is also effective.
[0072] (Emulsification process)
[0073] The W / O emulsion preparation step is a step of dispersing the fumed silica dispersion obtained in the dispersion preparation step in a non-water-soluble solvent to form a W / O emulsion. By forming such a W / O emulsion, the fumed silica dispersion as a dispersoid becomes spherical due to surface tension, etc., and therefore, the fumed silica dispersion dispersed in the non-water-soluble solvent in the spherical shape is gelled to obtain a spherical gel.
[0074] As the non-water-soluble solvent used in this manufacture method, any solvent having a hydrophobicity that can form an emulsion with the fumed silica dispersion can be used. As such a solvent, for example, organic solvents such as hydrocarbons and halogenated hydrocarbons can be used. More specifically, non-water-soluble solvents such as hexane, heptane, octane, nonane, decane, liquid paraffin, methylene chloride, chloroform, carbon tetrachloride, and dichloropropane can be cited. Among them, hexane, heptane, and decane with appropriate viscosity can be used appropriately. It should be noted that, as required, a variety of solvents can also be mixed and used. In addition, as long as it can form an emulsion with the fumed silica dispersion, hydrophilic solvents such as lower alcohols (used as a mixed solvent) can also be used in combination.
[0075] The amount of the water-insoluble solvent used is not particularly limited as long as it is within a range that allows the formation of a W / O emulsion. Generally, the water-insoluble solvent is used in an amount of about 1 to 10 parts by volume based on 1 part by volume of the fumed silica dispersion.
[0076] In the present manufacturing method, when forming the above-mentioned W / O emulsion, it is preferred to add a surfactant. As the surfactant used, known surfactants that can be used for the formation of W / O emulsions can be used without restriction, and anionic surfactants, cationic surfactants and nonionic surfactants can all be used. Among them, from the viewpoint of easy formation of W / O emulsions and not easy mixing of alkali metals, nonionic surfactants are preferred. In particular, surfactants having an HLB value of 3 or more and 5 or less, which represents the hydrophilicity and hydrophobicity of the surfactant, can be used. It should be noted that the "HLB value" here refers to the HLB value obtained by the Griffith method. Specific examples of surfactants that can be suitably used include: sorbitan monooleate, sorbitan monostearate, sorbitan monostearate, and the like.
[0077] The amount of the surfactant used is the same as the general amount used when forming a W / O emulsion. Specifically, it can be preferably used in the range of 0.05 g or more and 10 g or less relative to 100 ml of the fumed silica dispersion.
[0078] When forming a W / O emulsion, as a method for dispersing the fumed silica dispersion in a non-water-soluble solvent, a known method for forming a W / O emulsion can be used. From the viewpoint of ease of industrial manufacturing, it is preferred to form an emulsion by mechanical emulsification. Specifically, a method using a mixer, a homogenizer, etc. can be exemplified. A homogenizer can be used appropriately. Through this emulsification process, an emulsion with a narrow particle size distribution of droplets of the aqueous phase can be obtained, and therefore, the particle size distribution of the spherical porous silica finally obtained is also narrow. In the case where particles of 1 μm or more and less than 100 μm are preferably obtained, and particles of 8 μm or more and less than 90 μm are more preferably obtained, the rotation speed of the homogenizer is preferably 1,000 rpm or more and 15,000 rpm or less, more preferably 2,000 rpm or more and 12,000 rpm or less, and further preferably 4,000 rpm or more and 9,000 rpm or less. The stirring time is preferably 30 seconds or more and 1 hour or less, and more preferably 1 minute or more and 30 minutes or less.
[0079] (Gelation process)
[0080] The gelation process is a process of gelling the fumed silica dispersion in a state where the droplets of the fumed silica dispersion are dispersed in a non-water-soluble solvent after the W / O emulsion preparation process. The gelation can be performed by a known method. For example, the gelation can be easily performed by heating to a high temperature; or by adjusting the pH of the fumed silica dispersion to a weak acid or even alkaline state. From the viewpoint of being able to mainly control the reaction, the above method is preferred. It should be noted that the pH of the fumed silica dispersion prepared by the above method and without pH adjustment is generally in the range of 3.0 to 4.5.
[0081] When heating is performed, the boiling point of each solvent used should not be exceeded, and the lower limit of the gelation temperature is preferably 50° C., more preferably 60° C. The upper limit is preferably 100° C. or lower, more preferably 90° C. or lower.
[0082] The above-mentioned pH adjustment can be easily performed by the following methods: a method in which a substance such as urea which decomposes thermally when heated and exhibits alkalinity (referred to as a "latent base") is mixed in advance into the fumed silica dispersion, and the pH is raised by heating during gelation; a method in which a base is added to the emulsion while stirring with a mixer or the like and maintaining the W / O emulsion in a formed state.
[0083] Specific examples of the base include ammonia, tetraalkylammonium hydroxides such as tetramethylammonium hydroxide (TMAH), amines such as trimethylamine, alkali metal hydroxides such as sodium hydroxide, alkali metal carbonates such as sodium carbonate and sodium bicarbonate, and alkali metal silicates. It should be noted that the intensity of the stirring may be strong enough to cause mixing of the W / O emulsion and the base.
[0084] Among the above-mentioned methods for pH adjustment, the method using thermal decomposition of a latent base such as urea or the method using ammonia, tetraalkylammonium hydroxides or amines as a base is preferred from the viewpoint of not mixing metal elements. When ammonia is used for pH adjustment, ammonia can be blown in the form of gas or added in the form of ammonia water. From the viewpoint of being able to adjust the pH without unevenness as a whole when heating, pH adjustment using urea is particularly preferred.
[0085] When adjusting the pH to promote gelation, it is particularly preferred to adjust the amount added so that the pH value of the fumed silica dispersion is raised to about 4.5 to 8.0. The same is true for the case of using a latent base. If the specific amount added is shown, for example, when urea is used, it is preferably 1% by mass or more, and particularly preferably 2% by mass or more, relative to the fumed silica dispersion. The upper limit is preferably 7% by mass or less, and more preferably 5% by mass or less.
[0086] When performing the heating and pH adjustment, stirring is preferably performed to prevent the gel from agglomerating. A known method is generally used for stirring, and a mixer equipped with a stirring blade can be used as a specific example.
[0087] In addition, after gelation, the dispersoid changes from a liquid to a solid state, so the system becomes a dispersion (suspension) in which a solid (gel) is dispersed in a hydrophobic solvent, and is no longer a W / O emulsion.
[0088] (Gel recovery process)
[0089] In the present manufacturing method, the gel produced as described above is recovered from the liquid. As a method for recovering the gel, conventional solid-liquid separation methods such as filtration and centrifugation can be used, but W-O phase separation can also be performed before the recovery. W-O phase separation refers to the separation of the aforementioned gel dispersion into two layers, namely, the O phase and the W phase, and this operation is also generally referred to as demulsification. Here, the gel obtained by the aforementioned gelation step is present on the W phase side after separation. By separating it from the O phase, it is easy to perform solid-liquid separation and recover the gel by filtration or the like.
[0090] As the above-mentioned WO phase separation method, a known method can be appropriately selected as a demulsification method and implemented, but it is preferably carried out in the following manner: a certain amount of a water-soluble organic solvent usually used in demulsification is added to the gel dispersion liquid and heated to separate into an O phase and a W phase. After this step, the upper layer is usually an O phase (a layer mainly containing an organic solvent), and the lower layer is a W phase (a water layer containing an aqueous organic solvent and a gel).
[0091] Examples of the water-soluble organic solvent include acetone, methanol, ethanol, isopropyl alcohol, etc. Among them, isopropyl alcohol can be particularly preferably used.
[0092] The amount of the water-soluble organic solvent added is preferably adjusted according to the type and amount of the surfactant having an HLB of 3 or more and 5 or less used when forming the emulsion. For example, when sorbitan monooleate is used as the surfactant, the water-soluble organic solvent is added in an amount of about 1 / 6 to 1 / 2 times (water-soluble organic solvent / water-insoluble organic solvent) by mass relative to the mass of the water-insoluble organic solvent, and the emulsion is broken suitably after stirring as needed and then left to stand.
[0093] During the WO phase separation, the surfactant migrates to the O phase side (extracts), and therefore, by removing the O phase, porous spherical silica free of impurities generated by the surfactant can be obtained.
[0094] The heating temperature range is 50°C or higher, preferably about 50 to 80°C, and more preferably about 60 to 70°C.
[0095] As described above, after adding the water-soluble organic solvent to the gel dispersion, it is preferably stirred to prevent the gels from agglomerating with each other. The stirring is usually carried out by a known method. For example, a mixer with stirring blades can be used. The degree of mixing is not particularly limited as long as the liquid surface is rotated by stirring. For example, stirring using a mixer is 0.1 to 3.0 kW / m 3 , preferably 0.5~1.5kW / m 3 The stirring time is appropriately 0.5 to 24 hours, preferably about 0.5 to 1 hour.
[0096] After the WO phase separation, the W phase including the gel is recovered. Specifically, the O phase (upper layer) can be separated and removed by decantation or the like.
[0097] (Drying process)
[0098] The gel contained in the recovered W phase is preferably recovered from the W phase. As a recovery method, a known method can be used, and specific examples include suction filtration and centrifugal separation. In this case, the solvent is preferably removed in a manner such that the recovered gel is in the form of a filter cake.
[0099] The recovered gel is dried by spray drying. As in the manufacturing method of the present invention, when the gel is manufactured by a wet process, when the gel is taken out from the liquid and dried, the capillary force of the solvent will be generated between the particles of the gel. As a result, due to the aggregation of particles, especially in static drying, the dry powder will also aggregate. And by using spray drying for drying, the droplet diameter of the solvent during drying can be made close to the particle size of the porous spherical silica particles. Ideally, if the droplet diameter of the solvent is equal to the particle size of the porous spherical silica particles, a state is formed in which the porous spherical silica particles are contained in the droplets of the solvent during drying. In the above state, the porous spherical silica particles are not adjacent during drying, so it is possible to dry in a state where the capillary force caused by the solvent is not generated between the particles, and it is easy to obtain particles without aggregation. The spray drying method is not particularly limited, and known methods such as rotary atomization method and nozzle method can be used, preferably in a manner that the particle size of the target porous spherical silica particles is equal to the droplet diameter of the sprayed solvent. Generally, the nozzle method tends to produce finer droplet diameters than the rotary atomization method. The two-fluid nozzle method is particularly preferred from the viewpoint that the droplet diameter can be made finer and aggregation is less likely to occur during drying.
[0100] From the viewpoint of not easily generating aggregation, the gel during spray drying is preferably dispersed in a water-soluble organic solvent. Specific examples of water-soluble organic solvents include acetone, methanol, ethanol, isopropanol, etc. By using a solvent with a lower boiling point, the drying efficiency can be improved.
[0101] Water or a non-water-soluble solvent may also be mixed into the water-soluble organic solvent. In order to suppress aggregation during drying, the concentration of the water-soluble organic solvent in the solvent is preferably 60% by mass or more, more preferably 65% by mass or more, and particularly preferably 70% by mass or more. If the concentration of the water-soluble organic solvent is within the above range, aggregation caused by poor drying during spray drying is unlikely to occur. It should be noted that the drying shrinkage inside the pores can be adjusted according to the concentration of the water-soluble solvent during drying. Therefore, by adjusting the concentration of the aforementioned water-soluble organic solvent, appropriate drying shrinkage can be produced and the pore volume can be controlled. Specifically, by increasing the proportion of water contained in the solvent and reducing the concentration of the water-soluble organic solvent, drying shrinkage is likely to occur and the pore volume becomes smaller. On the contrary, by reducing the proportion of water contained in the solvent and increasing the concentration of the water-soluble organic solvent, drying shrinkage is suppressed and the pore volume becomes higher.
[0102] In order to suppress the aggregation of particles in the liquid, it is preferred to stir the water-soluble organic solvent (slurry) dispersed with the gel. The stirring method can use a generally known method, and if a specific example is given, there is a stirring rod, a mixer with a stirring blade, etc. The degree of mixing is as long as the particles do not settle in the liquid and the particles are not destroyed. The slurry can be put into the spray dryer while stirring, or it can be put into the spray dryer after stirring for a certain period of time. From the viewpoint of preventing the sedimentation of particles, it is more preferred to put it into the spray dryer while stirring.
[0103] The inlet temperature during spray drying is preferably adjusted to above the boiling point of the solvent of the slurry and the porous spherical silica forms a dry powder rather than a slurry or a filter cake at the outlet of the spray dryer. It should be noted that the above-mentioned "above the boiling point" refers to the boiling point of the solvent under the pressure during drying. It is more preferred to adjust the inlet temperature to a value of about 20 to 50°C higher than the boiling point of the solvent of the slurry, and it is preferably adjusted to a temperature difference between the inlet temperature and the outlet temperature in the range of 10 to 70°C. Usually, the spray dryer only sets a heating device at the input port (inlet), and the outlet temperature does not exceed the inlet temperature. The temperature difference between the inlet temperature and the outlet temperature is more preferably in the range of 20 to 70°C, and particularly preferably in the range of 20 to 60°C. If the inlet temperature and the outlet temperature are within the above range, the drying state during spray drying is good, and porous spherical silica without aggregation is obtained.
[0104] The circulating air volume during spray drying can be adjusted in such a way that the temperature in the drying chamber is stable, and is preferably adjusted according to the scale of the spray dryer. When a cyclone separator is used to collect the dried porous spherical silica, the circulating air volume will affect the collection efficiency under the cyclone separator. The larger the circulating air volume, the higher the collection efficiency under the cyclone separator.
[0105] The concentration of the gel contained in the slurry can be adjusted to a degree that the slurry in which the gel is dispersed has fluidity and does not clog when the liquid is sent to the spray dryer. Specifically, the solid content concentration of silica after drying (converted by mass) is preferably 60% by mass or less, more preferably 50% by mass or less, and further preferably 40% by mass or less. There is no particular lower limit to the concentration of the gel, but the lower the concentration, the lower the drying treatment efficiency, so it is preferably not extremely low, and more preferably 5% by mass or more.
[0106] The liquid feeding speed of the slurry during spray drying can be adjusted to a stable spray and the inlet temperature and outlet temperature reach the above values, and is preferably adjusted according to the scale of the spray dryer. The liquid feeding speed of the slurry affects the temperature difference between the inlet temperature and the outlet temperature. When the liquid feeding speed becomes faster, the temperature difference between the inlet temperature and the outlet temperature becomes larger.
[0107] As a collection method for dry porous spherical silica, generally known methods can be used. Specifically, one collection method, two collection methods, etc. can be cited. In addition, the collector can use a general collector, specifically a cyclone separator, a bag filter, etc. From the viewpoint of removing coarse particles, it is preferably collected by using a two-collection method using a cyclone separator.
[0108] (Firing process)
[0109] The porous spherical silica of the present invention is further calcined after drying. By calcining, the test force at destruction can be increased. The calcining conditions only need to be adjusted so that the test force at destruction reaches the target value. The longer the calcining time and the higher the calcining temperature, the higher the test force at destruction. The calcining temperature is 900 to 1500°C. Preferably it is below 1400°C, more preferably below 1300°C. The calcining time is 10 to 25 hours. Preferably it is 12 to 23 hours, more preferably 12 to 20 hours. If the calcining temperature and the calcining time are within the above ranges, a porous spherical silica having a test force at destruction within the target range can be obtained, and the particles dried without aggregation by spray drying will not aggregate again and the pores will not be clogged.
[0110] As the firing method, a known method can be used, and generally, a method in which dry porous spherical silica is placed in a crucible, a quartz pot or the like and heated in an electric furnace is mentioned.
[0111] The atmosphere during firing is not particularly limited, and the firing can be performed in an inert gas such as argon or nitrogen or in an air atmosphere.
[0112] The heating rate during sintering can be within the temperature rise range of a heating device such as an electric furnace. The slower the heating rate, the lower the sintering treatment efficiency, so it is preferably not extremely low. When using a general electric furnace, it is suitable to heat at 2 to 10°C / min.
[0113] The particle size of the porous spherical silica obtained in the above-mentioned manufacturing method is basically consistent with the droplet (W phase) diameter of the fumed silica dispersion in the W / O emulsion prepared in the emulsification process. Therefore, it is necessary to set the dispersion conditions to reach the target diameter range. There are many known methods for controlling the droplet diameter in the W / O emulsion, which can be appropriately selected and applied. As a method for adjusting the particle size of the droplets, known methods can be used, specifically: a method for adjusting the amount of surfactant added; a method for adjusting the shear force applied during emulsification according to the rotation speed, flow rate, etc. When adjusting the amount of surfactant added, if the amount of surfactant used is large, the droplets tend to become fine, and if the amount used is small, the droplets tend to become larger. In addition, when adjusting the shear force, the greater the shear force applied, the easier it is for the droplets to become fine, and the smaller the shear force, the easier it is for the droplets to become larger.
[0114] In addition, the pore volume can be controlled by drying shrinkage. The control method of drying shrinkage can use a known method, specifically, it can be cited as: a method of adjusting the concentration of the water-soluble solvent before drying. The pore volume can also be controlled by the firing conditions, and the direction is that the higher the firing temperature and the longer the firing time, the smaller the pore volume. In addition, by using fumed silica as a raw material as the manufacturing method of the present invention, since fumed silica has an aggregated structure, the mode value of the aforementioned high pore radius is reached. The specific surface area can be adjusted by appropriately selecting the specific surface area of the fumed silica used as a raw material, and it can also be adjusted by the gelation time. It should be noted that the direction is that the shorter the gelation time, the higher the specific surface area. The specific surface area can also be adjusted by firing conditions. Generally speaking, the direction is that the higher the firing temperature and the longer the firing time, the lower the specific surface area.
[0115] As long as the fumed silica that does not substantially contain alkali metals as described above is used as a raw material, other raw materials also use raw materials that do not substantially contain alkali metals, and those skilled in the art pay full attention to and avoid contamination (impurity mixing) during production, the alkali metal content can be easily reduced. In addition, when the goal is to reduce the alkali metal content, the filter cake can also be washed with water, an organic solvent, etc. after solid-liquid separation and before drying.
[0116] By suppressing the aggregation of particles generated during the manufacturing process as in the manufacturing method of the present invention and not implementing the crushing process, the number of fragmented particles can be reduced. In addition, it is necessary to be careful not to apply excessive load to the particles during the entire manufacturing process to prevent the particles from being damaged.
[0117] Example
[0118] Hereinafter, examples are shown for specifically explaining the present invention, but the present invention is not limited to these examples.
[0119] <Evaluation Method>
[0120] The produced porous spherical silica was evaluated with respect to the following items.
[0121] (Measurement of particle size distribution and volume-based cumulative particle size using a Coulter counter)
[0122] 0.1 g of porous spherical silica was added to 40 ml of ion exchange water and dispersed for 30 minutes using an ultrasonic cleaner (BRANSON IC1510J-DTH manufactured by BRANSON). The particle size distribution of the dispersion was measured using Multisizer III manufactured by Beckman Coulter Co., Ltd. A hole with a pore size of 100 μm was used in the measurement. Based on the obtained particle size distribution, the cumulative 50% particle size, the cumulative 10% particle size, and the cumulative 90% particle size based on volume were evaluated.
[0123] (Determination of BJH pore volume, pore radius (mode value) and BET specific surface area)
[0124] The BJH pore volume, pore radius (mode value) and BET specific surface area were measured according to the above definitions using BLESORP-mini (manufactured by BEL JAPAN Co., Ltd.).
[0125] (Test force when the sample is confirmed to be broken)
[0126] The test force at which the sample is confirmed to be broken is measured according to the above definition using a micro compression tester (MCT-W510-J manufactured by Shimadzu Corporation). The loading speed during the measurement is set to 0.4462 mN / sec, and the loading holding time is set to 10 sec. A 200 μm diameter indenter is used in the measurement.
[0127] (Alkali metal content)
[0128] 10 ml of nitric acid and 10 ml of hydrofluoric acid were added to 1 g of porous spherical silica and dissolved. The solution was heated at 180°C for 4 hours to evaporate to dryness. After cooling to room temperature, 2 ml of nitric acid and 18 ml of ultrapure water were added and the volume was fixed to 20 ml to obtain a test sample. The alkali metal content of the obtained test sample was measured using an inductively coupled plasma emission spectrometer (Thermo Scientific, ICAP650DUO).
[0129] (Average circularity)
[0130] An image of 2000 or more porous spherical silica observed at 1000 times magnification using SEM (S-5500 manufactured by Hitachi High Technologies, accelerating voltage 3.0 kV, secondary electron detection) was analyzed to calculate the average circularity according to the above definition.
[0131] (Number of fragmented particles (Number of particles with a circularity of 0.7 or less))
[0132] For more than 200 porous silica particles, SEM images observed at a magnification of 800 times using SEM (S-5500 manufactured by Hitachi High Technologies, accelerating voltage 3.0 kV, secondary electron detection) were analyzed, the circularity of each particle was calculated according to the above definition, and the number of particles with a circularity of less than 0.7 was counted.
[0133] <Example 1>
[0134] (Dispersion liquid preparation process)
[0135] In 200 ml of ion exchange water in which 6.65 g of urea was dissolved, 66 g of Reolosil QS-30 (manufactured by Tokuyama Co., Ltd.) was added while stirring with a homogenizer (manufactured by IKA, T25BS1) to pre-disperse the fumed silica, and then finely dispersed using an ultrasonic homogenizer (manufactured by BRANSON, Sonifier SFX250) to obtain a fumed silica dispersion. The particle size distribution of the dispersed liquid was measured by laser diffraction scattering method, and the D90 value was 0.19 μm. It should be noted that the dispersion preparation process was carried out in a cooler cooled to 10°C.
[0136] (W / O emulsion preparation process)
[0137] 65.5 g of the fumed silica dispersion prepared in the above method was separated, 0.75 g of sorbitan monooleate (Rheodol SP-010V manufactured by Kao Corporation) was dispersed in 129 g of decane, and the mixture was stirred at 8600 rpm for 3 minutes using a homogenizer to obtain a W / O emulsion.
[0138] (Gelation process)
[0139] The obtained W / O emulsion was kept in a water bath at 80° C. for 3 hours while being stirred at 200 rpm using four paddles having a blade diameter of 60 mm, a blade width of 20 mm and an inclination angle of 45 degrees to achieve gelation.
[0140] (Gel recovery process)
[0141] 77 g of isopropyl alcohol and 52 g of water were added, and the mixture was stirred with a stirring blade while being kept at 70° C. for 30 minutes. The mixture was then left to stand to separate into two layers, with the O phase as the upper layer and the W phase as the lower layer.
[0142] Next, the O phase and the W phase were separated by decantation, and the W phase was recovered.
[0143] The W phase was filtered to remove the gel from the W phase.
[0144] (Drying process)
[0145] The obtained gel cake was dispersed in 60 g of isopropanol and placed in a spray dryer (Mini Spray Dryer B-290 manufactured by BUCHI) while stirring with a stirring rod. At this time, the solid content concentration of silica in the slurry after drying was 10% by mass. The inlet temperature of the spray dryer was set to 120°C and the outlet temperature was set to 85°C. The liquid delivery rate was set to 15 ml / min and the circulating air volume was set to 35 m 3 / Hour.
[0146] (Firing process)
[0147] The obtained dry powder was put into a crucible, heated at a heating rate of 5°C / min in an electric furnace (manufactured by ADVANTEC, FUS722PB), and calcined at 1000°C for 20 hours. The calcination atmosphere was not adjusted but was set in an air atmosphere.
[0148] The physical properties of the porous spherical silica thus obtained are shown in Table 1. (The same is true for the following Examples and Comparative Examples. The physical properties of the porous spherical silica obtained are shown in Table 1.)
[0149] <Example 2>
[0150] In Example 1, porous spherical silica was obtained in the same manner as in Example 1 except that the calcination conditions were changed to 900°C for 17 hours. The outlet temperature during spray drying was 85°C.
[0151] <Example 3>
[0152] In Example 1, porous spherical silica was obtained in the same manner as in Example 1 except that the rotation speed of the homogenizer in the W / O emulsion preparation step was changed to 3000 rpm. The outlet temperature during spray drying was 85°C.
[0153] <Example 4>
[0154] In Example 1, porous spherical silica was obtained in the same manner as in Example 1 except that the rotation speed of the homogenizer in the W / O emulsion preparation step was changed to 10000 rpm. The outlet temperature during spray drying was 85°C.
[0155] <Example 5>
[0156] In Example 1, porous spherical silica was obtained in the same manner as in Example 1 except that the calcination conditions were changed to 1200° C. for 15 hours. The outlet temperature during spray drying was 85° C.
[0157] <Example 6>
[0158] In Example 1, porous spherical silica was obtained in the same manner as in Example 1 except that the rotation speed of the homogenizer in the W / O emulsion preparation step was changed to 6000 rpm and the calcination conditions were changed to 1200° C. for 10 hours. The outlet temperature during spray drying was 85° C.
[0159] <Comparative Example 1>
[0160] 10 g / 100 mL of sulfuric acid was added to a sodium silicate aqueous solution having a molar ratio of 9 g / 100 mL and SiO2 / Na2O of 3.1 so as to reach a pH of 2.9, and 500 mL of silica sol was prepared. 66.5 g of the silica sol was taken out, and the fumed silica dispersion in Example 1 was replaced with the silica sol. Except for this, the W / O emulsion preparation step, gelation step, and gel recovery step were carried out in the same manner as in Example 1 to obtain a gel. The obtained gel was dried using a vacuum dryer and calcined at 1000°C for 20 hours to obtain porous spherical silica.
[0161] <Comparative Example 2>
[0162] The fumed silica dispersion prepared in the same manner as in the dispersion preparation step of Example 1 was spray-dried and then calcined at 1000° C. for 20 hours to obtain porous spherical silica.
[0163] <Comparative Example 3>
[0164] In Example 1, the speed of the homogenizer in the W / O emulsion preparation step was changed to 5500 rpm, and the gelation step and the gel recovery step were performed to obtain a gel. The obtained gel was dried using a vacuum dryer and calcined at 1000° C. for 20 hours. After calcination, it was crushed using a jet mill to obtain porous spherical silica.
[0165] <Comparative Example 4>
[0166] In Example 1, porous spherical silica was obtained in the same manner as in Example 1 except that the calcination step was not performed.
[0167] <Comparative Example 5>
[0168] Porous spherical silica was obtained in the same manner as in Example 6 except that the calcination was performed at 800° C. for 10 hours.
[0169] [Table 1]
[0170] (Table 1)
[0171]
[0172] <Evaluation Results>
[0173] (Examples 1 to 6)
[0174] As shown in Table 1, in Examples 1 to 6, the hardness was high, and the arithmetic mean value of the "test force when the sample was confirmed to be broken" for 10 particles obtained by the method specified in JIS Z8844 with the loading speed set to 0.4462 mN / sec was 1.0×10 1 ~2.0×10 1 mN, and the number of fragmented particles is reduced, and among the 200 particles observed in the SEM image, the number of particles with a circularity of 0.7 or less is 20 or less. This can be achieved by, as in the production method of the present invention, gelling the fumed silica dispersion in a liquid to obtain a gel, drying the gel by spray drying under appropriate drying conditions to suppress aggregation of particles, and calcining under appropriate calcining conditions.
[0175] In addition, the D50 of the porous spherical silica obtained in Examples 1 to 6 was all in the range of 2 to 200 μm, the D10 / D90 was 0.3 or more, the pore volume based on the BJH method was in the range of 0.5 to 8 ml / g, the mode value of the pore radius based on the BJH method was in the range of 5 nm to 50 nm, and the specific surface area based on the BET method was 50 m 2 / g and above 400m 2 / g or less, and the alkali metal content is 50 ppm or less.
[0176] In Examples 1 to 6, porous spherical silica with various D50 values were obtained, but all of them were controlled by adjusting the droplet diameter of the W / O emulsion by changing the rotation speed during emulsification. The manufacturing method of the present invention can easily control the D50 value of the porous spherical silica without major changes in the manufacturing process.
[0177] (Comparative Example 1)
[0178] The pore volume of the porous spherical silica in Comparative Example 1 using sodium silicate as a raw material becomes smaller. This is because the sodium residue from the raw material causes a decrease in melting point during firing, resulting in pore blockage. Therefore, when sodium silicate is used as a raw material, it is difficult to obtain a porous spherical silica with high hardness while maintaining the pore volume.
[0179] (Comparative Example 2)
[0180] The test force at the time of destruction of the porous spherical silica of Comparative Example 2 obtained by spray drying the fumed silica dispersion is lower. This is because the bonding strength between the primary particles of the base material before firing is low. Thus, when granulation is performed by spray drying, it is difficult to obtain porous spherical silica of the target hardness.
[0181] (Comparative Example 3)
[0182] The porous spherical silica of Comparative Example 3, which was dried in a vacuum dryer after the gel was recovered, had an increased number of fragmentary particles. This is because the particles aggregated during the drying and were subjected to a crushing process, resulting in the generation of fragmentary particles. Thus, it is difficult to obtain porous spherical silica with a reduced number of fragmentary particles by drying.
[0183] (Comparative Example 4)
[0184] The porous spherical silica of Comparative Example 4, which did not undergo the calcination step, had a low test force at the time of destruction. Therefore, it is difficult to obtain porous spherical silica having high hardness without undergoing the calcination step.
[0185] (Comparative Example 5)
[0186] The test force at the time of destruction of the porous spherical silica of Comparative Example 5 was low. Therefore, if the calcination conditions are not appropriate, it is difficult to obtain porous spherical silica having high hardness.
Claims
1. A porous spherical silica, characterized in that: The volume-based cumulative 50% particle size (D50) measured by the Coulter counter method is in the range of 2 μm or more and 200 μm or less, Similarly, the ratio (D10 / D90) of the cumulative 10% particle size (D10) to the cumulative 90% particle size (D90) is 0.3 or more. The pore volume based on the BJH method is 0.5 ml / g or more and 8 ml / g or less, The mode value of the pore radius based on the BJH method is 5 nm or more and 50 nm or less. The specific surface area based on the BET method is 50 m 2 / g and above 400m 2 / g or less, The arithmetic mean of the "test force until the sample is broken" for 10 particles, obtained by the method specified in JIS Z8844 with the loading speed set to 0.4462 mN / s, is 1.0×10 1 mN or more and 2.0×10 1 Below mN, Among the 200 particles observed in the SEM image, less than 20 particles had a circularity of 0.7 or less. The alkali metal content is 50 ppm or less.
2. A catalyst carrier comprising the porous spherical silica according to claim 1.
3. A cosmetic comprising the porous spherical silica according to claim 1. An analytical column comprising the porous spherical silica according to claim 1 . An abrasive comprising the porous spherical silica according to claim 1 . A resin composition comprising the porous spherical silica according to claim 1 .
7. A method for producing porous spherical silica, comprising the following steps: A step of preparing a W / O emulsion comprising an aqueous phase in which fumed silica is dispersed and an organic phase having a water-insoluble solvent as a main component; The step of heating the emulsion to gel the aqueous phase to obtain a gel dispersion; The step of recovering the generated gel from the liquid and spray drying it; and A step of calcining the obtained porous spherical silica at a temperature of 900 to 1500° C. for 10 to 25 hours.
8. The method for producing porous spherical silica according to claim 7, characterized in that: The spray drying method is a two-fluid nozzle method.
Citation Information
Patent Citations
Porous silica particles and method for producing same
CN111527047A
Ceramic particle and method of manufacturing the same
JP2010100503A
Production method of porous spherical metal oxide
JP2014210671A
Hollow silica particles and method for producing the same
JP2020079165A
Porous silica particles
JP2020193144A