Method for manufacturing glass article

By using hydrogen fuel in glass manufacturing and controlling partial pressure of water vapor, combining carbonate and SO3 management, as well as multi-stage combustion and cover technology, the problem of carbon dioxide exhaust gas and bubble layer expansion is solved, and efficient glass items are achieved Production.

CN119013237APending Publication Date: 2024-11-22NIPPON ELECTRIC GLASS CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202380033391.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-01-10
Filing Date
2023-04-11
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

During the manufacturing process of glass articles, the carbon dioxide exhaust gas caused by the use of hydrocarbon fuel increases, resulting in an increase in the environmental load, and the partial pressure of water vapor generated when the hydrogen fuel is burned increases, causing the bubble layer to expand and reduce energy efficiency.

Method used

By using hydrogen fuel in the glass article manufacturing method for heating the melting process, and controlling the partial pressure of water vapor in the melting furnace to be less than 80% of the total atmospheric pressure, using carbonate and limiting the content of SO3, and entering the melting furnace The gas is supplied, and the molten glass surface is covered with a multi-stage combustion and a mixing layer to reduce the partial pressure of water vapor and the thickness of the bubble layer.

Benefits of technology

It effectively reduces the production of carbon dioxide in the melting process, improves energy efficiency, and ensures stable generation and efficient production of molten glass.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013237A_ABST
    Figure CN119013237A_ABST
Patent Text Reader

Abstract

In a melting step (S1) in which a glass raw material (Gr), which is a raw material for a glass article, is heated and melted in a melting furnace (10) to generate molten glass (Gm), a fuel (FH) containing hydrogen is burnt to heat and melt the glass raw material (Gr), and the partial pressure (Pp) of water vapor in the melting furnace (10) is set to 80% or less of the total atmospheric pressure (Pt).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a glass article. Background Art

[0002] The manufacturing process of glass articles includes a melting process of heating glass raw materials in a melting furnace to melt them. In the melting process, the following method is widely used: using a burner that burns fuel to form a flame, the glass raw materials are heated in the melting furnace to melt them (for example, Patent Document 1). As the fuel, hydrocarbon fuels such as natural gas are generally used. In addition, in the melting process, combustion heating using a burner and electric heating using an electrode are sometimes used in combination.

[0003] In order to remove bubbles generated by melting, a clarifier is added to the glass raw material. For example, in addition to substances such as tin oxide and antimony that release oxygen through redox reactions to promote defoaming, and substances such as fluorides and chlorides that promote defoaming through evaporation, there are also sulfate (SO3) raw materials. Sulfate raw materials are thermally decomposed by heating, releasing SO2 gas to expand bubbles. In the melting process, a bubble layer is sometimes generated on the upper part of the molten glass due to the action of the clarifier.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: International Publication No. 2011 / 136086 Summary of the invention

[0007] Problems to be solved by the invention

[0008] If hydrocarbon fuel is used as the fuel supplied to the burner, the amount of carbon dioxide contained in the exhaust gas generated in the melting step increases, resulting in a problem of increased environmental load.

[0009] Therefore, for example, hydrogen fuel is considered as the fuel supplied to the burner. If hydrogen fuel is used, water is mainly generated when it is burned to form a flame, so it can be expected that the carbon dioxide contained in the exhaust gas will be greatly reduced. On the other hand, due to the water generated by combustion, the partial pressure of water vapor in the melting furnace increases.

[0010] When hydrogen fuel is supplied to the burner to form a flame, the partial pressure of water vapor in the melting furnace rises, and as a result, bubbles generated by the action of the clarifier expand, and the thickness of the bubble layer increases. Since the bubble layer has the property of being difficult to transfer heat, if the thickness of the bubble layer increases, it is difficult for the heat generated by the flame of the burner to be transferred to the molten glass through the bubble layer, and the energy efficiency decreases.

[0011] In view of the above circumstances, the technical problem to be solved by the present invention is to reduce carbon dioxide contained in exhaust gas generated in a melting step and to produce molten glass efficiently and stably.

[0012] Means for solving problems

[0013] The above-mentioned problems can be solved by the following method for producing a glass article of the present invention.

[0014] (1) A method for producing a glass article, comprising: a melting step of heating and melting glass raw materials, which are raw materials for the glass article, in a melting furnace to produce molten glass, wherein in the melting step, a fuel containing hydrogen is burned to heat and melt the glass raw materials, and a water vapor partial pressure in the melting furnace is set to be less than 80% of the total pressure of atmospheric pressure.

[0015] As described above, in the present invention, the fuel containing hydrogen is burned to heat and melt the glass raw materials, so that the carbon dioxide contained in the exhaust gas generated in the melting process can be reduced compared with the case of using hydrocarbon fuel as in the past. In addition, in the present invention, the water vapor partial pressure in the melting furnace is made less than 80% of the total pressure of the atmospheric pressure. If the fuel containing hydrogen is burned to heat and melt the glass raw materials, water is generated, and thus, the water vapor partial pressure in the melting furnace rises. In particular, when the fuel containing hydrogen is burned as the main fuel, the water vapor partial pressure in the melting furnace rises significantly, and the bubble layer expands. Here, in the present invention, since the water vapor partial pressure in the melting furnace is made less than 80% of the total pressure of the atmospheric pressure, the expansion of the bubble layer on the molten glass can be suppressed. Thus, the reduction of energy efficiency can be suppressed.

[0016] (2) In the method for producing a glass article according to (1) above, the glass raw material may contain a carbonate.

[0017] As described above, by using a carbonate-containing substance as a glass raw material, carbon dioxide is generated as the glass raw material is heated and melted. The generation of carbon dioxide can reduce the water vapor partial pressure in the melting furnace.

[0018] (3) In the method for producing a glass article according to (2) above, the glass raw material may contain CaCO 3 as a carbonate, and the glass raw material may be prepared so that the glass article has a composition containing 5 to 35 wt % of CaO.

[0019] By preparing the glass raw materials as described above, specifically, by adding glass raw materials containing CaCO3 as carbonate and preparing the glass raw materials in a manner such that the glass article contains 5 to 35 wt % or more of CaO, carbon dioxide can be appropriately generated during the melting process, thereby reducing the water vapor partial pressure in the melting furnace.

[0020] (4) In the method for producing a glass article according to (1) or (2) above, the glass raw material may contain 1000 wtppm or less of SO3.

[0021] By limiting the content of SO 3 that functions as a clarifier as described above, the thickness of the bubble layer on the molten glass can be reduced. This can further suppress a decrease in energy efficiency.

[0022] (5) In the methods for producing glass articles according to (1) to (4) above, gas may be supplied into the melting furnace in the melting step.

[0023] By supplying gas (e.g., air) into the melting furnace during the melting process as described above, the atmosphere in the melting furnace is exhausted, thereby reducing the water vapor partial pressure in the melting furnace. Therefore, even glass raw materials with a small carbonate content or glass raw materials without carbonate can achieve heating and melting based on hydrogen combustion, and reduce the water vapor partial pressure. It should be noted that the atmosphere in the melting furnace can also be exhausted by using an exhaust device provided in the waste gas treatment equipment, while gas is supplied into the melting furnace.

[0024] (6) In the methods for producing glass articles according to (1) to (5) above, a mixed fuel containing hydrogen and a hydrocarbon fuel may be used in the melting step.

[0025] When the mixed fuel is used as described above, the amount of water generated during combustion can be reduced compared to when a fuel consisting of only hydrogen is used. Therefore, by using the mixed fuel, the partial pressure of water vapor in the melting furnace can also be reduced.

[0026] (7) In the method for producing a glass article according to (1) to (6) above, in the melting step, the maximum thickness dimension of the bubble layer generated by heating and melting the glass raw material can be set to 50 mm or less.

[0027] As described above, when the glass raw material is heated and melted (during the melting process), the thickness dimension of the largest portion of the bubble layer formed on the upper part of the molten glass is set to be less than 50 mm, thereby, a part of the bubble layer can be reliably prevented from solidifying, the bubble layer is easier to flow, and the continuous release of micro bubbles is more smoothly performed. Therefore, the temperature and flow rate of the molten glass are further stabilized.

[0028] (8) In the manufacturing method of the glass article of the above (1) to (7), in the melting step, the batch material layer of the glass raw material supplied to the melting furnace and the bubble layer generated by the heating and melting of the glass raw material can cover 80 to 100% of the surface of the molten glass.

[0029] As described above, the batch layer and the bubble layer cover 80 to 100% of the surface of the molten glass. Thus, the surface of the molten glass is appropriately covered with the heat insulating layer, thereby reducing heat dissipation from the surface of the molten glass and improving energy efficiency.

[0030] (9) In the method for producing a glass article according to (1) to (8) above, the batch material layer as the glass raw material supplied to the melting furnace may cover 20 to 70% of the surface of the molten glass.

[0031] By making the batch material layer that also functions as a heat insulating layer cover 20 to 70% of the surface of the molten glass as described above, the heat dissipation from the surface of the molten glass can be reduced, and the energy efficiency is improved. In addition, by setting the area covered by the batch material layer to less than 70%, even if the conditions in the furnace change due to the change of the flow rate, etc., so that the glass raw material is easily trapped, the input of the glass raw material can be continued by making the batch material layer flow into the area not covered by the batch material layer. Therefore, the molten glass can be stably and continuously generated.

[0032] (10) In the methods for producing glass articles according to (1) to (9) above, in the melting step, the fuel containing hydrogen may be subjected to multi-stage combustion.

[0033] By performing multi-stage combustion as described above, the temperature of the flame is reduced, and the concentration of nitrogen oxides in the exhaust gas can be reduced. In particular, when the gas is supplied to the melting furnace using the exhaust device provided in the exhaust gas treatment equipment, the concentration of nitrogen oxides in the exhaust gas tends to increase, so the effect of reducing the concentration of nitrogen oxides in the exhaust gas by multi-stage combustion becomes significant.

[0034] Effects of the Invention

[0035] As described above, according to the present invention, it is possible to reduce carbon dioxide contained in exhaust gas generated in the melting step and to produce molten glass efficiently and stably. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 This is a longitudinal sectional view of a melting furnace according to one embodiment of the present invention.

[0037] Figure 2 It is along Figure 1 Cross-sectional view of the melting furnace at line AA.

[0038] Figure 3 is set at Figure 1 A combustion system diagram of a burner of a melting furnace is shown. DETAILED DESCRIPTION

[0039] The following is based on Figure 1 to Figure 3One embodiment of the present invention will be described.

[0040] The manufacturing device of the glass article of the present embodiment comprises: a melting furnace for generating molten glass, a clarification chamber for performing clarification treatment on the molten glass, a homogenization chamber for homogenizing the molten glass subjected to the clarification treatment by stirring, etc., and a forming device for forming a predetermined glass article from the homogenized molten glass. Figure 1 A longitudinal cross-sectional view of a melting furnace 10 as one element of the above-mentioned manufacturing apparatus is shown. Figure 2 Indicates along Figure 1 The cross-sectional view of the melting furnace 10 along the line AA is shown. It should be noted that the manufacturing device with the above-mentioned structure is only an example, and for example, some of the above-mentioned elements may be omitted. Alternatively, elements other than the above-mentioned elements may be further provided.

[0041] The melting furnace 10 is used to implement the melting step S1 of the present embodiment, and is configured to melt glass raw material Gr continuously introduced into a space (melting space 11) in the melting furnace 10 to generate molten glass Gm. Specifically, the melting furnace 10 includes the melting space 11, a plurality of walls 12a to 12e that define and form the melting space 11, a raw material supply device 13, and heating devices 14 and 15.

[0042] Here, the glass raw material Gr can use a known raw material (natural raw material, chemically synthesized raw material, cullet, etc.). In the present embodiment, a raw material containing carbonate is used for the glass raw material Gr. In this case, for example, the glass raw material Gr can be prepared in such a way that the glass raw material contains CaCO3 as a carbonate and the finished glass article has a composition containing 5 to 35 wt% (preferably 5 to 25 wt%) of CaO (more preferably CaO derived from CaCO3).

[0043] As a suitable example of the above composition, D glass can be cited, and as more suitable examples, E glass, NE glass, C glass, A glass, and soda-lime glass can be cited. E glass, for example, has a composition containing, by weight%, 52 to 62% of SiO2, 10 to 16% of Al2O3, 0 to 8% of B2O3, 0 to 5% of MgO, 16 to 25% of CaO, and 0 to 2% of R2O (wherein R is at least one of Li, Na, and K).

[0044] Soda-lime glass has a composition containing, by weight%, 48 to 70% SiO2, 5 to 15% Al2O3, 0 to 5% MgO, 0 to 5% CaO, 0 to 15% BaO, 0 to 15% SrO, 0 to 5% ZrO2, and 0 to 15% R2O (wherein R is at least one of Li, Na, and K).

[0045] SO3 in glass raw material plays a role as a clarifier, and by limiting SO3 content, the thickness of the bubble layer on the molten glass can be reduced. Thus, the reduction of energy efficiency can be further suppressed. From this viewpoint, the SO3 content of glass raw material Gr is preferably less than 1000wtppm, more preferably less than 700wtppm, further more preferably less than 500wtppm, and most preferably less than 400wtppm. SO3 is an inevitable impurity, and even if it is not intentionally added, it will also be mixed into other component raw materials. With the reduction of SO3 content, the cost rises, therefore, SO3 content is preferably more than 200wtppm.

[0046] On the other hand, the more SO3 content of the glass raw material Gr, the more significant the effect of suppressing the expansion of the bubble layer on the molten glass by making the water vapor partial pressure Pp of the melting space 11 described later below 80% of the atmospheric pressure total pressure Pt. From this viewpoint, the SO3 content of the glass raw material Gr is preferably 200wtppm or more, more preferably 300wtppm or more, and further more preferably 500wtppm or more. In this case, the upper limit is preferably 1000wtppm or less.

[0047] The walls 12a to 12e of the melting furnace 10 are formed of refractory bricks {eg, zirconia fused bricks, alumina fused bricks, alumina / zirconia fused bricks, AZS (Al—Zr—Si) fused bricks, dense sintered bricks, etc.}.

[0048] The front wall portion 12a of the melting furnace 10 is provided with an inlet 16 for feeding glass raw material Gr. The inlet 16 is provided with a screw feeder 17 as a raw material supply device 13 for supplying glass raw material Gr to the space (melting space 11) in the melting furnace 10. The raw material supply device 13 may also be other known mechanisms such as a push rod and a vibration feeder. The number and arrangement position of the raw material supply device 13 may be appropriately changed according to the size of the melting furnace 10, etc.

[0049] The rear wall portion 12b of the melting furnace 10 is provided with a discharge port 18 for discharging the molten glass Gm. The discharge port 18 is connected to a transfer flow path 19, and the molten glass Gm reaching the downstream end of the melting furnace 10 is sequentially transferred to the next process (e.g., a clarification process) through the transfer flow path 19. It should be noted that, although not shown in the figure, in the case of manufacturing glass articles at multiple locations at the same time, the discharge ports 18 may be provided at multiple locations of the melting furnace 10, and the molten glass Gm may be transferred to the next process by using the transfer flow paths 19 connected to the discharge ports 18 at each location.

[0050] A plurality of burners 20 as heating devices 14 are provided on the side walls 12c on both sides of the melting furnace 10 to burn fuel and form flames F. The flames F of the burners 20 heat at least one of the glass raw material Gr and the molten glass Gm from a position above the liquid level of the molten glass Gm. The number and arrangement positions of the burners 20 can be appropriately changed according to the size of the melting furnace 10, etc.

[0051] like Figure 3 As shown, a fuel supply path 21 for supplying fuel, etc. is connected to each burner 20. The fuel supply path 21 includes at least a hydrogen fuel pipe 22 for supplying hydrogen fuel (equivalent to the fuel containing hydrogen of the present invention) FH. In the present embodiment, the fuel supply path 21 also includes a hydrocarbon fuel pipe 23 for supplying hydrocarbon fuel FC and a combustion-supporting gas pipe 24 for supplying oxygen as a combustion-supporting gas.

[0052] The hydrogen fuel pipe 22 is provided with a flow regulating valve 25 for regulating the flow of the hydrogen fuel FH, a switching valve 26 for switching the opening and closing of the flow path of the hydrogen fuel FH having the regulated flow, and a check valve 27 for preventing the backflow of the hydrogen fuel FH and other fuels. A hydrogen fuel source 28 is connected to the upstream end of the hydrogen fuel pipe 22.

[0053] The hydrocarbon fuel piping 23 is provided with a flow regulating valve 29 for regulating the flow of the hydrocarbon fuel FC, a switching valve 30 for switching the opening and closing of the flow path of the hydrocarbon fuel FC whose flow is regulated, and a check valve 31 for preventing the backflow of fuel such as the hydrocarbon fuel FC. A hydrocarbon fuel source 32 is connected to the upstream end of the hydrocarbon fuel piping 23. As the hydrocarbon fuel FC, for example, butane, propane, petroleum gas, natural gas, etc. can be used. However, from the viewpoint of further reducing the carbon dioxide contained in the exhaust gas, it is preferable to use natural gas as the hydrocarbon fuel FC.

[0054] The downstream ends of the hydrogen fuel pipe 22 and the hydrocarbon fuel pipe 23 are connected to each other and connected to the burner 20 via the common fuel pipe 33. The regulated fuel whose mixing ratio of the hydrogen fuel FH and the hydrocarbon fuel FC is regulated by the flow regulating valves 25 and 29 and / or the switching valves 26 and 30 flows through the common fuel pipe 33. The common fuel pipe 33 is provided with a switching valve 34 for switching the opening and closing of the flow path of the regulated fuel.

[0055] From the viewpoint of reducing carbon dioxide contained in the exhaust gas, the regulating fuel preferably contains 50wt% or more of hydrogen fuel FH, more preferably contains 70wt% or more of hydrogen fuel FH, more preferably contains 90wt% or more of hydrogen fuel FH, and most preferably does not contain hydrocarbon fuel FC and is composed only of hydrogen fuel FH. In addition, the higher the content of hydrogen fuel FH, the higher the water vapor partial pressure Pp of the melting space 11, and the more difficult it is to become less than 80%, so the effect of the present invention becomes significant.

[0056] A flow regulating valve 35 for regulating the flow of oxygen and a switching valve 36 for switching the opening and closing of the flow path of oxygen having regulated the flow are provided on the combustion-supporting gas piping 24. An oxygen source 37 is connected to the upstream end of the combustion-supporting gas piping 24, and a burner 20 is connected to the downstream end of the combustion-supporting gas piping 24. By utilizing the combustion-supporting gas piping 24 to supply oxygen to the burner 20, the fuel is regulated to mix with oxygen, and the regulated fuel becomes easy to burn, and the temperature of the flame F formed by the burner 20 is easily increased. It should be noted that, as the combustion-supporting gas, air can be used instead of oxygen. In addition, when oxygen is used as the combustion-supporting gas, the oxygen concentration can be set to more than 50wt%, preferably more than 70wt%, and more preferably more than 90wt%. The higher the oxygen concentration, the easier the fuel is to burn, and the easier it is to increase the temperature of the flame F formed by the burner 20.

[0057] The burner 20 is preferably a multi-stage combustion burner. The multi-stage combustion burner, for example, includes a main nozzle that sprays a mixture of fuel and a combustion-supporting gas, and a staged nozzle (not shown) that sprays the combustion-supporting gas. The mixed gas sprayed from the main nozzle is mixed in such a way that the combustion-supporting gas is insufficient relative to the fuel. Therefore, most of the fuel contained in the mixed gas sprayed from the main nozzle reacts with the combustion-supporting gas contained in the mixed gas and burns, and the remaining fuel reacts with the combustion-supporting gas sprayed from the staged nozzle and burns. If such a multi-stage combustion is used, the flame becomes longer and its temperature decreases. As a result, the concentration of nitrogen oxides in the exhaust gas can be reduced.

[0058] In addition, in the present embodiment, a plurality of rod-shaped electrodes 38 as the heating device 15 are provided on the bottom wall portion 12d of the melting furnace 10. Each electrode 38 is electrically heated to the molten glass Gm in a state immersed in the molten glass Gm. The number of electrodes 38 (one or more than two) can be appropriately changed according to the size and shape of the melting furnace 10. The form of the electrode 38 is arbitrary, for example, it can also be plate-shaped. In addition, the configuration of the electrode 38 is also arbitrary in principle, for example, although the figure is omitted, the electrode 38 can be configured on the lower side of the side wall portion 12c. It should be noted that in the present embodiment, the burner 20 and the electrode 38 are used in combination to heat at least one of the molten glass Gm and the glass raw material Gr, but the electrode 38 can also be omitted according to the situation. Of course, from the viewpoint of improving energy efficiency, it is preferred to use the electrode 38 to suppress the output power of the burner 20.

[0059] The melting furnace 10 is provided with a partial pressure measuring device 39 for measuring the water vapor partial pressure Pp of the melting space 11. The partial pressure measuring device 39 includes, for example, a pressure gauge 40, a hygrometer 41, a thermometer 42, and a computing device 43. The computing device 43 can calculate the water vapor partial pressure Pp of the melting space 11 (for example, the ratio relative to the atmospheric total pressure Pt) based on the air pressure (the atmospheric total pressure Pt), humidity, and temperature of the melting space 11 measured by these pressure gauges 40, hygrometers 41, and thermometers 42. It should be noted that in the present embodiment, the case where the pressure gauge 40, the hygrometer 41, and the thermometer 42 of the partial pressure measuring device 39 are arranged on the side wall portion 12c of the melting furnace 10 is illustrated (see Figure 2 ), but of course, part or all of these pressure gauges 40, hygrometers 41 and thermometers 42 may be arranged at other locations (e.g., top wall portion 12e, upstream side of flue). It should be noted that the water vapor partial pressure Pp may also be calculated from the measured values ​​of the exhaust gas composition, exhaust gas flow rate, regulated fuel flow rate, etc.

[0060] The tendency of the water vapor partial pressure Pp can be easily grasped by the calculation based on the measured value by the partial pressure measuring device 39, but in the present invention, when judging whether the water vapor partial pressure in the melting furnace is 80% or less of the total pressure of the atmospheric pressure, the moisture content (volume %) in the exhaust gas is measured by the method of using a moisture absorption tube according to 7.1 of JIS Z8808:2013, and the measured moisture content value (volume %) is used as the water vapor partial pressure Pp of the melting space 11. In this case, a point near the center of the cross section of the exhaust port provided at the melting furnace 10 is used as the measurement point.

[0061] In addition, in the present embodiment, a gas supply device 44 for supplying a gas (e.g., atmospheric air, dry air, clean dry air, oxygen, etc.) K to the melting space 11 is provided in the melting furnace 10. The gas supply device 44 has a supply port 45 opened to the melting space 11, and the gas K can be supplied to the melting space 11 through the supply port 45. It should be noted that the supply amount of the gas K can be adjusted by a flow control device (not shown) such as a regulating valve.

[0062] Next, a method for producing a glass article using the production apparatus configured as described above will be described.

[0063] As described above, the manufacturing method of the glass article of the present embodiment comprises a melting step S1, and further comprises a clarification step of subjecting the molten glass Gm obtained in the melting step S1 to clarification treatment as needed, a homogenization step of homogenizing the molten glass Gm after the melting step S1 by stirring, etc., and a forming step of forming a glass article from the molten glass Gm after the homogenization step.

[0064] like Figure 1and Figure 2 As shown, in the melting step S1, the glass raw material Gr continuously and at a constant flow rate introduced into the melting space 11 in the melting furnace 10 is heated and melted using a burner 20 that burns a fuel to form a flame F. In the present embodiment, in the melting step S1, from the viewpoint of improving energy efficiency, the glass raw material Gr is not only heated by the combustion of the burner 20, but also electrically heated by the electrode 38 for the glass raw material Gr and / or the molten glass Gm.

[0065] Hydrogen fuel FH is used as fuel when combustion is performed by the burner 20. In addition, the water vapor partial pressure Pp in the melting space 11 is set to be 80% or less of the atmospheric pressure total pressure Pt.

[0066] At this time, in order to make the water vapor partial pressure Pp of the melting space 11 less than 80% of the atmospheric total pressure Pt, it is preferable to supply gas K to the melting space 11 through the supply port 45 of the gas supply device 44, thereby reducing the water vapor partial pressure Pp of the melting space 11. In addition, it is preferable to use a glass raw material Gr containing carbonate, so that carbon dioxide is generated along with the heating and melting of the glass raw material Gr, thereby reducing the water vapor partial pressure Pp of the melting space 11. In order to reduce the water vapor partial pressure Pp of the melting space 11 to less than 30% by supplying gas K to the melting space 11, a large amount of gas K needs to be supplied. Therefore, the atmospheric temperature of the melting space 11 decreases, the energy efficiency decreases, or the bubbles of the bubble layer BL become less likely to break, and the bubble layer BL may become thicker. In the method of reducing the water vapor partial pressure Pp of the melting space 11 by using the glass raw material Gr containing carbonate, there is a limit on the content of carbonate in the glass raw material according to the CaO content of the glass composition. Therefore, the water vapor partial pressure Pp of the melting space 11 is preferably 30% or more.

[0067] In this case, the batch material layer GBL of the glass raw material Gr put into the melting space 11 of the melting furnace 10 and the bubble layer BL generated by the heating and melting of the glass raw material Gr preferably cover 80 to 100% of the surface of the molten glass Gm, more preferably 90 to 100%, and even more preferably 95 to 100%. On the other hand, the batch material layer GBL of the glass raw material Gr put into the melting space 11 of the melting furnace 10 preferably covers 20 to 70% of the surface of the molten glass Gm.

[0068] The maximum thickness BL of the bubble layer generated by heating and melting the glass raw material is preferably 50 mm or less, more preferably 45 mm or less, and even more preferably 40 mm or less. The lower limit thereof can be, for example, 10 mm or more, and preferably 15 mm or more.

[0069] As described above, in the manufacturing method of the glass article of the present embodiment, in the melting step S1, the hydrogen fuel FH is burned to heat and melt the glass raw material Gr put into the melting space 11, so that the carbon dioxide contained in the exhaust gas generated in the melting step S1 can be reduced. In addition, in the melting step S1, the water vapor partial pressure Pp in the melting furnace 10 is set to 80% or less of the atmospheric pressure total pressure Pt, so that the bubble layer BL (see Figure 1 ) expansion. Thus, it is possible to suppress the reduction of energy efficiency.

[0070] As mentioned above, although one embodiment of the present invention has been described, the manufacturing method of the glass article of the present invention is not limited to the above embodiment, and various modes can be adopted within the scope of the present invention.

[0071] In the above embodiment, the water vapor partial pressure Pp of the melting space 11 is reduced by using the gas supply device 44 and / or the glass raw material Gr containing carbonate, but the water vapor partial pressure Pp of the melting space 11 can also be reduced by adjusting the usage ratio (mixing ratio) of the hydrogen fuel FH and the hydrocarbon fuel FC. In this case, the water vapor partial pressure Pp of the melting space 11 is also preferably 30% or more.

[0072] In the above embodiment, the gas supply device 44 is used, but an exhaust device (not shown) for exhausting the melting space 11 may be used instead of the gas supply device 44, or an exhaust device for exhausting the melting space 11 may be used in addition to the gas supply device 44. When the exhaust device is used, an observation hole provided in the side wall of the melting furnace, a joint of the refractory, etc. may be used as a gas supply port.

[0073] [Example 1]

[0074] Hereinafter, examples of the method for producing a glass article of the present invention will be described. It should be noted that the following examples are merely illustrative, and the present invention is not limited to the following examples at all.

[0075] In the examples of the present invention (Test Nos. 1 to 3 and 5 to 7), glass raw materials (glass raw materials for E glass) containing CaCO3 as carbonate are supplied to a melting furnace, and the glass raw materials are heated and melted in the melting furnace to generate molten glass. At this time, the water vapor partial pressure in the melting furnace is adjusted to 80% or less by adjusting the amount of air supplied to the melting furnace.

[0076] In addition, in the comparative examples (Test Nos. 4 and 8), the supply of atmospheric air into the melting furnace was stopped, and glass raw materials containing CaO instead of CaCO3 (glass raw materials for E glass) were supplied into the melting furnace. As a result, the water vapor partial pressure in the melting furnace became greater than 80%.

[0077] It should be noted that in any test, the flow rate of the glass raw material to be fed was set constant, the flow rate of the hydrogen fuel supplied to the burner was set to 20 Nm3 / h, and the flow rate of the oxygen as the combustion-supporting gas was set to 10 Nm3 / h. 3 / h. In addition, the heating value based on the electrode is kept constant, and the water vapor partial pressure in the melting furnace, the maximum thickness of the bubble layer and the temperature of the molten glass are measured under a stable state. In the melting furnace, the batch layer and the bubble layer cover 100% of the surface of the molten glass. The CaO content of the obtained glass article is 25wt%. In test No. 1 to 4, glass raw materials with an SO3 content of 800wtppm are used, and in test No. 5 to 8, glass raw materials with an SO3 content of 300wtppm are used. The test conditions and measurement results are shown in Table 1.

[0078] [Table 1]

[0079]

[0080] In the comparative examples (Test No. 4 and 8), the supply of air to the melting furnace was stopped, and glass raw materials containing CaO instead of CaCO3 were used, and the water vapor partial pressure became a value exceeding 80% of the total atmospheric pressure. In this case, along with the expansion of the bubble layer, the maximum thickness of the bubble layer increased and exceeded 50 mm, and the heat generated by the flame of the burner was difficult to be conducted to the molten glass through the bubble layer, and the temperature of the molten glass decreased.

[0081] In contrast, in the examples (test Nos. 1 to 3 and 5 to 7), the water vapor partial pressure was reduced by using glass raw materials containing CaCO3. In addition, in the examples, the water vapor partial pressure was adjusted to 80% or less of the atmospheric pressure total pressure by supplying air into the melting furnace. Therefore, the maximum thickness of the bubble layer became 50 mm or less, which could suppress the expansion of the bubble layer and the temperature rise of the molten glass. It can be seen from these that by setting the water vapor partial pressure to 80% or less of the atmospheric pressure total pressure, the expansion of the bubble layer can be suppressed, and as a result, the reduction in energy efficiency can be suppressed.

[0082] In Test No. 1 to 4, glass raw materials with an SO3 content of 800 wtppm were used, and in Test No. 5 to 8, glass raw materials with an SO3 content of 300 wtppm were used. When compared under conditions of the same water vapor partial pressure, the maximum thickness of the bubble layer in Test No. 5 to 8 with an SO3 content of 300 wtppm was smaller than that in Test No. 1 to 4. This shows that the maximum thickness of the bubble layer can be reduced by reducing the SO3 content.

[0083] Description of Reference Numerals

[0084] 10 Melting furnace

[0085] 11 Molten Space

[0086] 12a~12e Wall

[0087] 13. Raw material supply device

[0088] 14, 15 Heating device

[0089] 16 Input port

[0090] 17 Screw Feeder

[0091] 18 Exhaust port

[0092] 19 Transfer flow path

[0093] 20 Burner

[0094] 21 Fuel supply line

[0095] 22 Hydrogen fuel piping

[0096] 23 Hydrocarbon fuel piping

[0097] 24 Combustion-supporting gas piping

[0098] 25, 29, 35 flow control valve

[0099] 26, 30, 34, 36 switching valve

[0100] 27, 31 Check valve

[0101] 28 Hydrogen fuel source

[0102] 32 Hydrocarbon fuel sources

[0103] 33 Common fuel piping

[0104] 37 Oxygen Source

[0105] 38 Electrodes

[0106] 39. Partial pressure measuring device

[0107] 40 Pressure gauge

[0108] 41. Hygrometer

[0109] 42 Thermometer

[0110] 43 Computing Device

[0111] 44 Gas supply device

[0112] 45 Supply port

[0113] BL Bubble Layer

[0114] F Flame

[0115] FC Hydrocarbon Fuel

[0116] FH Hydrogen Fuel

[0117] GBL batch layer

[0118] Gm Molten glass

[0119] Gr Glass Raw Materials

[0120] K Gas

[0121] t Thickness

Claims

1. A method for manufacturing a glass article, characterized in that: The method comprises: a melting step of heating and melting glass raw materials, which are raw materials for glass articles, in a melting furnace to generate molten glass; In the melting step, the glass raw material is heated and melted by burning a fuel containing hydrogen, and the partial pressure of water vapor in the melting furnace is set to be 80% or less of the total pressure of atmospheric pressure.

2. The method for manufacturing a glass article according to claim 1, wherein: The glass raw material includes carbonate.

3. The method for manufacturing a glass article according to claim 2, wherein: The glass raw material contains CaCO3 as the carbonate, The glass raw materials are prepared so that the glass article has a composition containing 5 wt % to 35 wt % of CaO.

4. The method for producing a glass article according to any one of claims 1 to 3, wherein: The glass raw material contains 1000 wtppm or less of SO3.

5. The method for producing a glass article according to any one of claims 1 to 3, wherein: In the melting step, gas is supplied into the melting furnace.

6. The method for producing a glass article according to any one of claims 1 to 3, wherein: In the melting step, a mixed fuel containing the hydrogen and a hydrocarbon fuel is used as the fuel.

7. The method for producing a glass article according to any one of claims 1 to 3, wherein: In the melting step, the maximum thickness of the bubble layer generated by heating and melting the glass raw material is set to 50 mm or less.

8. The method for producing a glass article according to any one of claims 1 to 3, wherein: In the melting step, the batch material layer of the glass raw material supplied into the melting furnace and the bubble layer generated as the glass raw material is heated and melted cover 80% to 100% of the surface of the molten glass.

9. The method for producing a glass article according to any one of claims 1 to 3, wherein: The batch material layer as the glass raw material supplied into the melting furnace covers 20% to 70% of the surface of the molten glass.

10. The method for producing a glass article according to any one of claims 1 to 3, wherein: In the melting step, the fuel containing hydrogen is combusted in multiple stages.

Citation Information

Patent Citations

  • Glass article production apparatus and production method thereof

    CN109890767A

  • Method for producing glass article and glass-melting furnace

    CN111566055A

  • Water enhanced fining process method to reduce toxic emissions from glass melting furnaces

    CN1201763A

  • Arc discharge method, arc discharge apparatus, and fused silica crucible manufacturing apparatus

    EP2166820A1

  • Glass melting furnace

    JP2005015299A