Thermally conductive polymer composition, material for forming thermally conductive polymer composition, and thermally conductive polymer

By increasing the amount of urethane bonds in liquid rubber, a urethane bond network is formed, which solves the problem of reduced adhesion of thermally conductive materials at high temperatures, and achieves a thermally conductive polymer with high thermal conductivity and shape following. The manufacturing process is reduced and costs are reduced.

CN119013341APending Publication Date: 2024-11-22MITSUBISHI MATERIALS CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280093866.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-24
Filing Date
2022-08-03
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

When the existing thermal conductivity is improved, the hardness of the existing thermal conductivity increases, making it difficult to follow the surface shape of the component without gaps, and the adhesion is reduced in high temperature environments, and the surface treatment increases manufacturing steps and costs.

Method used

By increasing the amount of urethane bonds in the liquid rubber, a urethane bond network is formed, and the adhesion and shape follow-up of the thermally conductive material are improved. Compositions of liquid rubber, solvents and curing agents are used, and solvents are not required to be removed after curing. A thermally conductive polymer with high thermal conductivity and low viscosity is formed.

Benefits of technology

It realizes the maintenance of high adhesion and shape following under high temperature environments, reduces the thermal resistance of the thermally conductive material, improves thermal conductivity and construction properties, and avoids additional surface treatment steps and costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005050011720000101
    Figure BDA0005050011720000101
  • Figure HDA0005050011730000011
    Figure HDA0005050011730000011
  • Figure HDA0005050011730000012
    Figure HDA0005050011730000012
Patent Text Reader

Abstract

The thermally conductive polymer composition is characterized by containing: a liquid rubber having two or more hydroxyl groups in one molecule; a solvent having one or more hydroxyl groups in one molecule; a curing agent having, in one molecule, two or more functional groups capable of reacting with both the hydroxyl groups of the liquid rubber and the hydroxyl groups of the solvent; and a filler, the thermally conductive polymer composition is mixed, then left to stand in the atmosphere at 25 DEG C for 24 hours or more and then cured to obtain a thermally conductive polymer, and the compressive modulus of elasticity at room temperature of the thermally conductive polymer is 4.5 N / mm2 or more and 5.5 N / mm2 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a thermally conductive polymer composition, a material for forming the thermally conductive polymer composition and a thermally conductive polymer.

[0002] The present invention claims priority based on Japanese Patent Application No. 2022-048513 filed on March 24, 2022, and the contents thereof are incorporated herein by reference. Background Art

[0003] Regarding the heat-conducting material that is disposed between the heating element and the heat-dissipating component and transfers heat, various forms of heat-conducting materials are known, such as grease type, gap filler type, sheet type, etc. By using these heat-conducting materials, for example, the heat generated in the heating element can be effectively dissipated from heat-dissipating components such as metal frames or radiators. Such a heat-conducting material can reduce the thermal resistance between the heating element and the heat-dissipating component by being disposed between the heating element and the heat-dissipating component.

[0004] In recent years, with the development of high performance and integration of various electronic devices, a structure with improved heat dissipation is required to effectively dissipate the heat generated by the operation of the components (heating element) to the outside. Therefore, a thermal conductive material is required that can further reduce the thermal resistance between the heating element and the heat dissipation component.

[0005] In order to reduce the thermal resistance between the heating element and the heat dissipation component, it is possible to consider increasing the thermal conductivity of the thermally conductive material itself or increasing the close contact between the thermally conductive material and the heating element or heat dissipation component connected to the thermally conductive material to reduce the thermal resistance generated at their interface (interface thermal resistance).

[0006] Conventionally, as a general thermally conductive material, a thermally conductive material obtained by filling silicone resin or the like with a filler having high thermal conductivity, such as alumina, is known (for example, refer to Patent Document 1).

[0007] Furthermore, there is also known a thermally conductive material which improves adhesion to the surface of each component by reducing hardness to reduce thermal resistance generated at the interface between the thermally conductive material and each component in contact therewith (see, for example, Patent Document 2).

[0008] Furthermore, there is also known a two-liquid curing gap filler or putty-like thermally conductive material that can reduce the thermal resistance generated at the interface between the thermally conductive material and the components connected thereto by mixing and curing a plurality of fluids with high fluidity (for example, see Patent Documents 3 and 4).

[0009] Patent Document 1: Japanese Patent Application Publication No. 2005-006428

[0010] Patent Document 2: Japanese Patent Application Publication No. 2019-011423

[0011] Patent Document 3: Japanese Patent Application Publication No. 2020-050701

[0012] Patent Document 4: Japanese Patent Application Publication No. 2020-157554

[0013] However, the thermally conductive materials disclosed in Patent Documents 1 to 4 all increase the amount of filler added to improve thermal conductivity, which increases the hardness and makes it difficult to make the thermally conductive material follow the surface shape of each component and adhere to it without gaps.

[0014] In addition, it is also possible to consider performing surface treatment on the surface of the heating element or the heat dissipation component to improve the adhesion between the heating element and the heat dissipation component, but there will be an increase in the number of manufacturing steps due to the surface treatment and the increase in manufacturing costs. In addition, when the thermal conductive material is placed in a high temperature environment, the effect of improving the adhesion brought by the surface treatment may be reduced. Summary of the invention

[0015] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a thermally conductive polymer composition having high thermal conductivity, low viscosity, high shape-following property, and high workability without removing a solvent during curing, a thermally conductive polymer composition-forming material for forming the thermally conductive polymer composition, and a thermally conductive polymer obtained by curing the thermally conductive polymer composition. The shape-following property refers to the property of being able to deform along the shape of the bonding surface and to bond without a gap.

[0016] The present inventors focused on the amount of urethane bonds derived from liquid rubber contained in the thermal conductive material, and found that by increasing the amount of urethane bonds, the adhesion of the thermal conductive material in a high temperature environment and the adhesion after long-term storage in a high temperature environment can be improved. That is, when the amount of liquid rubber and curing agent is small, the liquid rubber is not easy to form a network, but by increasing the amount of liquid rubber and curing agent, the liquid rubber forms a urethane bond network after curing, making the thermal conductive material tougher, suppressing cohesive failure, and thus improving adhesion.

[0017] A thermally conductive polymer composition according to one embodiment of the present invention is characterized in that it comprises: a liquid rubber having two or more hydroxyl groups in one molecule; a solvent having one or more hydroxyl groups in one molecule; a curing agent having two or more functional groups in one molecule that can react with both the hydroxyl groups of the liquid rubber and the hydroxyl groups of the solvent; and a filler, wherein the thermally conductive polymer composition is mixed, and then left to stand in an atmosphere at 25° C. for 24 hours or more, and then cured to obtain a thermally conductive polymer, wherein the compressive elastic modulus of the thermally conductive polymer at room temperature is 4.5 N / mm 2 Above and 5.5N / mm 2 the following.

[0018] According to the thermally conductive polymer composition of the present invention, it is possible to obtain a thermally conductive polymer composition having high thermal conductivity after curing, low viscosity, high shape-conforming property, and high workability without removing a solvent during curing.

[0019] Furthermore, in the thermally conductive polymer composition according to the present invention, the thermal conductivity of the filler may be 10 W / (m·K) or more.

[0020] Furthermore, in the thermally conductive polymer composition according to the present invention, the liquid rubber may include one or two or more of polybutadiene, polyisoprene, and polyolefin having a plurality of hydroxyl groups.

[0021] Furthermore, in the thermally conductive polymer composition of the present invention, the solvent may include one or more of ethylene glycol, n-butyl carbitol, glycerol, polyethylene glycol monomethyl ether, ethylene glycol monobutyl ether, propylene glycol, ethylene glycol and tetraethylene glycol monomethyl ether.

[0022] Furthermore, in the thermally conductive polymer composition according to the present invention, the curing agent may be an isocyanate compound.

[0023] Furthermore, in the thermally conductive polymer composition according to the present invention, the thermally conductive polymer composition may further include a thickener.

[0024] The thermally conductive polymer composition forming material according to the present invention is characterized in that it is used to form the thermally conductive polymer composition described in the above items, and the thermally conductive polymer composition forming material has a liquid A containing the liquid rubber and the solvent and a liquid B containing the curing agent, and at least one of the liquid A or the liquid B further contains the filler.

[0025] Furthermore, the thermally conductive polymer according to the present invention is obtained by curing the thermally conductive polymer composition described in the above items, and the urethane bonds derived from the liquid rubber in the thermally conductive polymer are 0.17 mol / 2000cc or more.

[0026] Furthermore, in the thermally conductive polymer of the present invention, the terminal group of the thermally conductive polymer may include -[(C2H4-O) m -C n H 2n+1 ](where m and n are arbitrary natural numbers).

[0027] Furthermore, in the present invention, the thermal conductivity of the thermally conductive polymer may be 1.5 W / (m·K) or more.

[0028] According to the present invention, there can be provided a thermally conductive polymer composition having high thermal conductivity after curing, low viscosity, high shape-conforming property, and high workability without removing a solvent during curing; a thermally conductive polymer composition-forming material for forming the thermally conductive polymer composition; and a thermally conductive polymer obtained by curing the thermally conductive polymer composition. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1A It is a perspective view showing the details of the tensile test in the inspection example.

[0030] Figure 1B It is a perspective view showing the details of the tensile test in the inspection example. DETAILED DESCRIPTION

[0031] Hereinafter, a thermally conductive polymer composition, a thermally conductive polymer composition forming material, and a thermally conductive polymer according to an embodiment of the present invention will be described with reference to the accompanying drawings. In addition, each embodiment shown below is specifically described for better understanding of the gist of the invention, and is not intended to limit the present invention unless otherwise specified.

[0032] (Thermal conductive polymer composition, thermal conductive polymer)

[0033] The thermally conductive polymer composition of the present embodiment forms a thermally conductive polymer by curing, and contains liquid rubber, a solvent, a curing agent, and a filler. The thermally conductive polymer composition of the present embodiment is in a state before curing (polymerization reaction), and the thermally conductive polymer of the present embodiment can be obtained by curing such a thermally conductive polymer composition.

[0034] The liquid rubber may be, for example, a liquid rubber having fluidity at room temperature, and may have two or more hydroxyl groups (—OH) in one molecule in its composition formula. The hydroxyl groups are preferably located at the ends of the molecules.

[0035] A part of the hydroxyl groups in such a liquid rubber reacts with the functional groups of the curing agent to form a chemical bond during curing of the thermally conductive polymer composition described later.

[0036] As specific examples of liquid rubber having two or more hydroxyl groups in one molecule on the terminal group, hydroxyl-containing polybutadiene, hydroxyl-containing polyisoprene, hydroxyl-containing polyolefin, etc. can be cited. Among them, hydroxyl-containing polybutadiene is preferred from the viewpoint of good filling property of filler. These hydroxyl groups can be located at the end of the molecule.

[0037] When the liquid rubber is, for example, a hydroxyl-containing polybutadiene, it may be Poly bd (registered trademark) series (hydroxyl number: 0.83 to 1.83 mol / kg, manufactured by Idemitsu Kosan Co., Ltd.), G series (hydroxyl number: 0.48 to 1.39 mol / kg, manufactured by Nippon Soda Co., Ltd., product name), Krasol LBH series (hydroxyl number: undisclosed, manufactured by Totalcrayvalley Co., Ltd., product name). Furthermore, when it is a hydroxyl-containing polyisoprene, it may be Poly ip (registered trademark) (hydroxyl number: 0.83 mol / kg, manufactured by Idemitsu Kosan Co., Ltd.).

[0038] The number average molecular weight of the liquid rubber is not particularly limited, and for example, a liquid rubber having a number average molecular weight in the range of 1000 to 3000 can be used, and a number average molecular weight in the range of 1500 to 3000 is more preferred. In addition, the hydroxyl value of the liquid rubber is preferably in the range of 0.5 to 2.0, and more preferably in the range of 0.5 to 1.8. In addition, the viscosity of the liquid rubber is not particularly limited, and for example, it may be in the range of 1.0 Pa·s to 1000 Pa·s, and more preferably in the range of 1.0 Pa·s to 900 Pa·s.

[0039] The solvent is a component that improves the plasticity of the thermally conductive polymer composition, and in the composition formula, it only needs to have one or two or more hydroxyl groups (-OH) in one molecule. The hydroxyl group may be located at the end of the molecule.

[0040] The hydroxyl group in such a solvent reacts with the functional group of the curing agent to form a chemical bond during curing of the thermally conductive polymer composition described below.

[0041] The boiling point of the solvent is preferably 100° C. to 250° C., more preferably 120° C. to 230° C. The viscosity of the solvent is preferably 500 mPa·s or less (25° C.), more preferably 400 Pa·s or less (25° C.).

[0042] The solvent may be a polyol.

[0043] The solvent may be a solvent compatible with the liquid rubber. The solvent compatible with the liquid rubber here refers to a liquid substance that maintains a mixed state to the extent that phase separation is not observed to the naked eye after the liquid rubber and the solvent are mixed in any proportion and left to stand for more than 10 minutes.

[0044] Specific examples of the solvent having one or more hydroxyl groups in one molecule include n-butyl carbitol (diethylene glycol monobutyl ether), glycerol, polyethylene glycol monomethyl ether, ethylene glycol monobutyl ether, propylene glycol, ethylene glycol, tetraethylene glycol monomethyl ether and the like.

[0045] Regarding the solvent contained in the conventional thermally conductive polymer composition, curing is performed by volatilizing and removing the solvent, so that the cured thermally conductive polymer contains almost no solvent components. On the other hand, the solvent contained in the thermally conductive polymer composition of the present embodiment forms a chemical bond with the liquid rubber through the curing agent during curing, thereby becoming a part of the constituent of the thermally conductive polymer. In other words, the thermally conductive polymer has a solvent-curing agent-liquid rubber bond. In addition, the curing agent will also bond with the solvent or with the liquid polymer, so it also has a solvent-curing agent-solvent or liquid rubber-curing agent-liquid rubber bond. Furthermore, when the curing agent is a multifunctional type, there are multiple bonds formed between the solvent and the liquid polymer via the curing agent, so it is more preferred.

[0046] For the above reasons, the solvent does not need to be a low-boiling-point solvent with high volatility, and a solvent having a wide boiling point range from a low-boiling-point solvent to a high-boiling-point solvent can be used according to the application. In particular, from the perspective of ease of construction work of the thermally conductive polymer composition, a medium-boiling-point solvent or a high-boiling-point solvent is preferred. Specifically, the boiling point of the solvent is preferably 100° C. or higher, more preferably 150° C. or higher, and further preferably 180° C. or higher.

[0047] The appropriate content ratio of the solvent to the liquid rubber is, for example, within the range of 5 parts by mass or more and 600 parts by mass or less relative to 100 parts by mass of the liquid rubber. By setting the content ratio of the solvent to the liquid rubber within such a range, the fluidity can be ensured and the workability can be improved during the construction of the thermally conductive polymer composition, and the curing of the liquid rubber component can be prevented from being hindered. In addition, the appropriate content ratio of the solvent to the liquid rubber is more preferably within the range of 5 parts by mass or more and 100 parts by mass or less relative to 100 parts by mass of the liquid rubber.

[0048] The curing agent only needs to have two or more functional groups that can react with the hydroxyl groups of the liquid rubber and the hydroxyl groups of the solvent molecules in one molecule. The curing agent of this embodiment only needs to chemically bond with the hydroxyl groups of the liquid rubber and the hydroxyl groups of the solvent, respectively. The multiple hydroxyl groups of the liquid rubber are preferably located at the ends of the molecule.

[0049] Specific examples of the curing agent having two or more functional groups reactive with a hydroxyl group in one molecule include isocyanate compounds, acid anhydrides, carboxylic acids, and amines.

[0050] The method for curing the thermally conductive polymer composition using such a curing agent is not particularly limited, and examples thereof include a curing method in which the curing is carried out by allowing the polymerization reaction to proceed at room temperature, and a method in which the curing is accelerated by increasing the reaction rate by heating.

[0051] The appropriate content ratio of the curing agent to the liquid rubber is, for example, within a range of 50 parts by mass or more and 400 parts by mass or less relative to 100 parts by mass of the liquid rubber. By setting the content ratio of the curing agent to the liquid rubber within such a range, the curing agent can be polymerized sufficiently with the hydroxyl groups of the liquid rubber and the hydroxyl groups of the solvent to form a thermally conductive polymer with appropriate hardness, and the situation in which the brittleness is increased due to excessive hardness can be prevented.

[0052] The content ratio of the curing agent in the liquid rubber is preferably 50 parts by mass or more and 360 parts by mass or less, and more preferably 90 parts by mass or more and 200 parts by mass or less, based on 100 parts by mass of the liquid rubber.

[0053] The filler is a component that improves the thermal conductivity of the cured thermally conductive polymer and preferably has thermal conductivity. For example, it is preferable to use a filler having a thermal conductivity of 10 W / (m·K) or more.

[0054] As fillers, for example, metals, metal oxides, metal hydroxides, metal nitrides, carbon, etc. can be used. Examples of metals include gold (319), silver (428), copper (403), aluminum (236), tungsten (177), titanium (22), nickel (94), iron (84), and alloys formed by using two or more of these metals. In addition, the numerical values ​​in parentheses of the above metals are examples of thermal conductivity expressed in units of W / (m·K). The thermal conductivity of these metals is 10 W / (m·K) or more.

[0055] Examples of metal oxides used as fillers include aluminum oxide (20-35), magnesium oxide (45-60), beryllium oxide (272), zinc oxide (54), silicon oxide (2), and titanium oxide (8). Examples of metal hydroxides include aluminum hydroxide. Examples of metal nitrides include aluminum nitride (150-250), boron nitride (30-50), and silicon nitride (20-90). The values ​​in parentheses of the above oxides are thermal conductivities expressed in units of W / (m·K).

[0056] Further, examples of carbon include graphite (100), carbon fiber (94 to 149), fullerene (0.4 in the case of C60), graphene (3000 to 5300), carbon nanotube (650 to 830 in the case of multilayer), etc. In addition, the numerical values ​​in parentheses of the above metals are examples of thermal conductivity expressed in units of W / (m·K).

[0057] Among them, aluminum oxide is particularly preferred as a constituent material of the filler from the viewpoint of being cheap and readily available. Moreover, among these metal oxides, metal hydroxides, and carbon, the thermal conductivity of materials other than silicon oxide, titanium oxide, and fullerene is 10 W / (m·K) or more. In addition, the thermal conductivity of materials other than fullerene is 2 W / (m·K) or more.

[0058] The filler preferably includes one or two or more of the above-mentioned material examples, more preferably includes one or two or more of metal oxides, metal hydroxides and metal nitrides, and particularly preferably includes aluminum oxide.

[0059] The filler may be in the form of particles, but spherical particles, disc-shaped particles, or rounded particles with few edges and corners (round particles) are preferably used from the viewpoint of providing the thermally conductive elastomer composition with excellent shape conformability and high thermal conductivity after curing.

[0060] Regarding the particle size distribution of the filler, from the perspective of ensuring both filling and processability, it can have multiple peaks. Therefore, the filler can include a plurality of filler particles with different average particle sizes (d50) (analysis method: laser diffraction scattering particle size distribution measurement, measuring device: particle size distribution measuring device (Microtrac MT3300EX II), measurement conditions: ultrasonic (US) dispersion using sodium hexametaphosphate for 1 minute). In the case where the filler includes two filler particles with different average particle sizes (d50), it is preferred that, for example, the peak on the small particle size side is within the range of 0.3 μm or more and 10 μm or less and the peak on the large particle size side is within the range of 20 μm or more and 100 μm or less.

[0061] In the thermally conductive polymer composition of this embodiment, in addition to the above-mentioned liquid rubber, solvent, curing agent, and filler, lubricants, antioxidants, flame retardants, thickeners, etc. can be further added. By further adding, for example, a flame retardant, it can also be used as a flame-retardant thermally conductive component between a battery cell and a casing (heat sink) of a lithium ion secondary battery.

[0062] The thermally conductive polymer of this embodiment obtained by curing the thermally conductive polymer composition having the above structure is obtained by curing the thermally conductive polymer composition through a polymerization reaction. The compressive elastic modulus of the thermally conductive polymer of this embodiment at room temperature (25°C) is 4.5 N / mm 2 Above and 5.5N / mm 2 Below. The compressive elastic modulus of the thermally conductive polymer at room temperature (25°C) is more preferably 4.7 N / mm2 or more and 5.3 N / mm2 or less. In addition, the thermal conductivity of the thermally conductive polymer is preferably 1.5 W / (m·K) or more. The compressive elastic modulus of the thermally conductive polymer at room temperature (25°C) can be measured using the method described in the embodiments described below. By keeping the compressive elastic modulus within the above range, the shape tracking property can be improved. The compressive elastic modulus is less than 4.5 N / mm 2 When the adhesion is insufficient, it is greater than 5.5N / mm 2 When the material is too hard, it will become difficult to discharge and apply the material.

[0063] The thermally conductive polymer of this embodiment focuses on the amount of urethane bonds derived from the liquid rubber in the thermally conductive polymer composition, and increases the amount of urethane bonds after curing. As a result, the compressive elastic modulus of the thermally conductive polymer falls within the above range, and the adhesion in a high temperature environment and the adhesion after long-term storage in a high temperature environment are improved.

[0064] As in the past, when the amount of liquid rubber and curing agent in the thermally conductive polymer composition was small, the liquid rubber was not easy to form a network of urethane bonds. However, by using a thermally conductive polymer composition with increased liquid rubber and curing agent as in the present embodiment, the liquid rubber forms a network of urethane bonds after curing, thereby increasing the strength and suppressing cohesive failure, thereby obtaining a thermally conductive polymer with improved adhesion.

[0065] In the thermally conductive polymer of the present embodiment, the amount of urethane bonds derived from the liquid rubber is 0.17 mol / 2000cc or more, preferably 0.20 mol / 2000cc or more. If the amount of urethane bonds is greater than the above value, a network of urethane bonds is fully formed when the thermally conductive polymer composition is cured, thereby improving the strength of the thermally conductive polymer and the adhesion to the applicable parts. The amount of urethane bonds of the thermally conductive polymer can be calculated using the method described in the examples described later.

[0066] In the thermally conductive polymer of this embodiment, for example, the terminal group is -[(C2H4-O) m -C n H 2n+1] (wherein m and n are arbitrary natural numbers). The thermal conductivity of such a thermally conductive polymer measured by a conventional method is, for example, in the range of 1.5 W / (m·K) to 5 W / (m·K).

[0067] (Thermal Conductive Polymer Composition Forming Material)

[0068] The thermally conductive polymer composition forming material used to form the thermally conductive polymer composition of the present embodiment is a two-liquid mixed thermally conductive polymer material, comprising a liquid A containing the above-mentioned liquid rubber and a solvent, and a liquid B containing a curing agent. In addition, at least one of the liquid A or the liquid B, or both of them, further contains a filler.

[0069] In addition, regarding liquid A and liquid B, the density was about the same when the filler loading amount reached 2000 parts by mass, based on 100 parts by mass of the total amount of the liquid rubber and the solvent or 100 parts by mass of the total amount of the curing agent and the flame retardant.

[0070] When using the thermally conductive polymer composition forming material of the present embodiment, liquid A and liquid B are mixed, and the hydroxyl groups of the liquid rubber of liquid A and the hydroxyl groups of the solvent are contacted with the curing agent contained in liquid B to chemically bond and cure. As a construction method, for example, a method can be used in which a two-liquid mixing dispenser is used to dispense the liquid A and liquid B in equal volumes, mix them, and form a thermally conductive polymer composition, and the thermally conductive polymer composition is directly applied to the surface of a component on which a thermally conductive polymer is provided.

[0071] Thus, according to the thermally conductive polymer composition forming material of the present embodiment, by separating the liquid A containing the liquid rubber and the solvent and the liquid B containing the curing agent from each other, the liquid A and the liquid B can be mixed and cured at any time to form a thermally conductive polymer, and a thermally conductive polymer composition forming material with excellent storage properties can be achieved.

[0072] Above, an embodiment of the present invention has been described, but this embodiment is only an example and is not intended to limit the scope of the invention. This embodiment can be implemented in various other ways, and various omissions, substitutions, and changes can be made without departing from the scope of the main purpose of the invention. This embodiment or its modification is included in the scope or main purpose of the invention, and is included in the invention described in the scope of the claims and its equivalent.

[0073] Example

[0074] The A liquid and the B liquid of the thermally conductive polymer composition forming material of each sample of the composition shown in Table 1 were mixed in equal volumes, and allowed to stand in an atmosphere at 25°C for more than 24 hours to cure, thereby obtaining thermally conductive polymers of Inventive Examples 1 to 6 and Comparative Examples 1 to 5. Then, the amount of urethane bonds derived from the liquid rubber, the compressive elastic modulus at 25°C, and the adhesion at 25°C and 50°C were examined for each thermally conductive polymer.

[0075] Table 1 summarizes the compositions of liquid A and liquid B, and the urethane bond content, compressive elastic modulus, and adhesion of the obtained thermally conductive polymer.

[0076] In addition, the details of each component are as follows.

[0077] [Liquid rubber]

[0078] ·Hydroxy-terminated polybutadiene: Poly bd (registered trademark) series (manufactured by Idemitsu Kosan Co., Ltd.)

[0079] [Solvent]

[0080] n-Butyl carbitol: (manufactured by Tokyo Chemical Industry Co., Ltd.)

[0081] [filler]

[0082] · Tridisperse alumina: DAB series (manufactured by Denka Company Limited, product name)

[0083] [Curing agent]

[0084] ·Multifunctional isocyanate: MILLIONATE MR series (manufactured by TOSOH CORPORATION, product name)

[0085] [Flame retardant]

[0086] Phosphorus flame retardant: TCP (manufactured by DAIHACHI CHEMICAL INDUSTRY CO., LTD., product name)

[0087] (Calculation method of the amount of urethane bonds derived from liquid rubber)

[0088] Assuming that a thermally conductive polymer composition was prepared by discharging 1000cc of liquid A and 1000cc of liquid B each time, the amount of urethane bonds derived from the liquid rubber was calculated based on the amount of hydroxyl groups in the liquid rubber, the amount of hydroxyl groups in the solvent, and the molar amount of the functional groups that chemically bond in the curing agent, assuming that the functional groups of the curing agent react preferentially with the hydroxyl groups in the solvent.

[0089] For example, suppose the density of liquid A and liquid B is 3.3 g / cm 3 The amount of urethane bonds derived from the liquid rubber was calculated based on the following: the amount of hydroxyl groups in the liquid rubber (Poly bd) was 1.83 mol / kg, the amount of hydroxyl groups in the solvent (n-butyl carbitol) was 6.17 mol / kg, and the amount of isocyanate in the curing agent (MR) was 7.62 mol / kg.

[0090] (Method for measuring compression elastic modulus)

[0091] For the compression test, the thermally conductive polymer composition of each sample was left to stand for more than 24 hours in an atmosphere at 25°C to cure, and the resulting thermally conductive polymer was molded into a size of 28 mm x 2 mm thick, and the sample was compressed using a tensile tester (product name: AGS-X: manufactured by Shimadzu Corporation). The displacement and test force were measured until the test force reached 1000 N, and the elastic modulus was calculated in the range of 10 to 20 N of test force. The test environment was set at 25°C.

[0092] (Method for measuring adhesion at 25°C and 50°C)

[0093] Regarding the tensile test, as shown in FIG1 , two aluminum bars were prepared, and on one of the aluminum bars, the thermally conductive polymer composition of each sample was left to stand in an atmosphere at 25° C. for more than 24 hours to be cured to form a thermally conductive polymer in a rectangular shape of 25 mm in length×19 mm in width×1 mm in thickness, and the other aluminum bar was laminated and bonded thereon. Then, using a tensile tester (product name: AGS-X: manufactured by Shimadzu Corporation), as shown in FIG1 , Figure 1B As shown, the joint strength and elongation were measured by pulling from top to bottom, and the maximum stress of each sample was calculated based on the results. In addition, the test environment was set at 25°C and 50°C.

[0094]

[0095] According to the results shown in Table 1, the compressive elastic modulus of the thermally conductive polymer at room temperature (25°C) is 4.5 N / mm 2 Above and 5.5N / mm 2 When the viscosity is less than 0.05, the adhesion at 25° C. can be 0.08 MPa or more and the adhesion at 50° C. can be 0.026 MPa. This confirms that a thermally conductive polymer having excellent shape-conforming properties that can closely adhere to the surface shape of a component with little gap can be realized.

[0096] In Examples 1 to 6 of the present invention, in which the amount of urethane bonds derived from the liquid rubber is 0.17 mol / 2000cc or more and 0.32 mol / 2000cc or less, the adhesion at 25°C can be 0.08 MPa or more and the adhesion at 50°C can be 0.026 MPa. In particular, the compressive elastic modulus of the thermally conductive polymer at room temperature (25°C) is 5.0 N / mm 2 In the above-mentioned Examples 3 to 6 of the present invention, the adhesion at 50° C. was excellent and was 0.071 MPa or more.

Claims

1. A thermally conductive polymer composition, characterized in that contain: Liquid rubber, with two or more hydroxyl groups in one molecule; Solvents, which have more than one hydroxyl group in one molecule; a curing agent having two or more functional groups in one molecule that can react with both the hydroxyl groups of the liquid rubber and the hydroxyl groups of the solvent; and filler, After mixing the thermally conductive polymer composition, the composition is left to stand in an atmosphere at 25° C. for 24 hours or more and then cured to obtain a thermally conductive polymer having a compressive elastic modulus of 4.5 N / mm at room temperature. 2 Above and 5.5N / mm 2 the following.

2. The thermally conductive polymer composition according to claim 1, characterized in that The thermal conductivity of the filler is greater than 10 W / (m·K).

3. The thermally conductive polymer composition according to claim 1 or 2, characterized in that: The liquid rubber includes at least one of polybutadiene, polyisoprene, and polyolefin having a plurality of hydroxyl groups.

4. The thermally conductive polymer composition according to any one of claims 1 to 3, characterized in that The solvent comprises at least one of ethylene glycol, n-butyl carbitol, glycerol, polyethylene glycol monomethyl ether, ethylene glycol monobutyl ether, propylene glycol, ethylene glycol and tetraethylene glycol monomethyl ether.

5. The thermally conductive polymer composition according to any one of claims 1 to 4, characterized in that The curing agent is an isocyanate compound.

6. The thermally conductive polymer composition according to any one of claims 1 to 5, characterized in that The thermally conductive polymer composition further contains a thickener.

7. A thermally conductive polymer composition forming material, characterized in that: Used to form the thermally conductive polymer composition according to any one of claims 1 to 6, The thermally conductive polymer composition forming material includes a liquid A containing the liquid rubber and the solvent and a liquid B containing the curing agent, and at least one of the liquid A or the liquid B further contains the filler.

8. A thermally conductive polymer, characterized in that The thermally conductive polymer is a thermally conductive polymer obtained by curing the thermally conductive polymer composition according to any one of claims 1 to 6. The thermally conductive polymer has a urethane bond derived from the liquid rubber in an amount of 0.17 mol / 2000cc or more.

9. The thermally conductive polymer according to claim 8, characterized in that The terminal group of the thermally conductive polymer comprises -[(C2H4-O) m -C n H 2n+1 ], where m and n are any natural numbers.