Resin composition and molded article
By using phosphite and phosphorus flame retardant in the polyphenylene ether resin composition, combined with inorganic filler materials, the flame retardant ratio is optimized, and the problem of excellent flame retardant but poor heat resistance in the prior art is solved, and the problem of excellent flame retardant properties but poor heat resistance is achieved. A resin composition and molded product with excellent flame retardancy and heat resistance.
Patent Information
- Application Number
- CN202380033607.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-14
- Filing Date
- 2023-03-24
- Publication Date
- 2024-11-22
AI Technical Summary
Although the conventional polyphenylene ether resin composition has excellent flame retardancy, it has poor heat resistance, making it difficult to meet the requirements of miniaturization and high performance of components.
By using phosphites in the resin composition and precisely adjusting their mixing amount, combining phosphorus flame retardant and inorganic filler materials, the mass ratio of the flame retardant is optimized to achieve improved flame retardant and heat resistance.
The resin composition and molded products with excellent flame retardancy and heat resistance are achieved, meeting the needs of high performance and safety.
Smart Images

Figure BDA0005078985280000021 
Figure BDA0005078985280000041 
Figure BDA0005078985280000071
Abstract
Description
Technical Field
[0001] The present invention relates to a resin composition and a molded product, and particularly to a resin composition containing a polyphenylene ether resin as a main component. Background Art
[0002] A resin composition using a polyphenylene ether resin as a base resin (hereinafter, sometimes referred to as a "polyphenylene ether resin composition") has advantages such as heat resistance, electrical properties, dimensional stability, impact resistance, and low specific gravity. In addition, the polyphenylene ether resin composition can be flame-retarded without using halogen compounds and antimony compounds that have a large environmental burden, and therefore has been widely used in various electrical / electronic components, office equipment components, automobile components, building materials, various other exterior materials, industrial products, and the like.
[0003] In recent years, various performances have been required due to the miniaturization and improvement of performance of components.
[0004] For example, Patent Document 1 discloses a resin composition containing a polyphenylene ether resin, a phosphorus-based flame retardant, and a phosphorus-based antioxidant as a polyphenylene ether resin composition having excellent flame retardancy and long-term flame retardancy.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: International Publication No. 2017 / 077683 Summary of the invention
[0008] Problems to be solved by the invention
[0009] However, as a result of the present inventors' studies, they found that the resin composition described in Patent Document 1 is excellent in flame retardancy but may be inferior in heat resistance.
[0010] An object of the present invention is to solve the above-mentioned problems, and an object of the present invention is to provide a resin composition and a molded article having excellent flame retardancy and excellent heat resistance.
[0011] Solutions to the problem
[0012] Based on the above problems, the present invention has found that flame retardancy and excellent heat resistance can be achieved by generally using a phosphite and precisely adjusting the blending amount thereof and further precisely adjusting the blending amount of a flame retardant, thereby completing the present invention.
[0013] Specifically, the above-mentioned problems are solved by the following method.
[0014] <1> A resin composition comprising: (c) 15 to 20 parts by mass of a flame retardant; (d) 1.5 to 4.0 parts by mass of a phosphite; and (e) 10 to 100 parts by mass of an inorganic filler, relative to 100 parts by mass of a total of (a) 90 to 100% by mass of a polyphenylene ether resin and (b) 0 to 10% by mass of a styrene-based resin;
[0015] The total of the (a) polyphenylene ether resin and the (b) styrene resin accounts for 90% by mass or more of the resin component contained in the resin composition, and the mass ratio (c) / (d) of the (c) flame retardant and the (d) phosphite is 4.0 or more and 13.0 or less.
[0016] <2> The resin composition according to <1>, wherein
[0017] (c) The flame retardant is a phosphorus-based flame retardant.
[0018] <3> The resin composition according to <1> or <2>, wherein
[0019] (d) the phosphite has a structure represented by formula (P),
[0020] Formula (P)
[0021] [Chemical formula 1]
[0022]
[0023] In the formula (P), t-Bu represents a tert-butyl group, R represents a hydrocarbon group having 1 to 10 carbon atoms, n represents an integer of 0 to 2, and * represents a bonding position with other sites.
[0024] <4> A resin composition comprising: (c) 15 to 20 parts by mass of a flame retardant; (d) 1.5 to 4.0 parts by mass of a phosphite; and (e) 10 to 100 parts by mass of an inorganic filler, relative to 100 parts by mass of a total of (a) 90 to 100% by mass of a polyphenylene ether resin and (b) 0 to 10% by mass of a styrene-based resin;
[0025] The total amount of the (a) polyphenylene ether resin and the (b) styrene-based resin accounts for 90% by mass or more of the resin component contained in the resin composition.
[0026] <5> A molded article formed from the resin composition according to any one of <1> to <4>.
[0027] Effects of the Invention
[0028] Effect of the Invention According to the present invention, a resin composition and a molded article having excellent flame retardancy and excellent heat resistance can be provided. DETAILED DESCRIPTION
[0029] Hereinafter, a mode for implementing the present invention (hereinafter, simply referred to as "this embodiment") will be described in detail. It should be noted that the following this embodiment is an example for describing the present invention, and the present invention is not limited to this embodiment.
[0030] In addition, in this specification, "to" is used to mean that the numerical values described before and after it are included as a lower limit and an upper limit.
[0031] In this specification, various physical property values and characteristic values are values at 23° C. unless otherwise specified.
[0032] Unless otherwise specified, when the measurement method and the like described in the standards shown in this specification differ depending on the year, they refer to the standards based on the time of January 1, 2022.
[0033] In the resin composition of the present embodiment, relative to a total of 100 parts by mass of (a) 90 to 100% by mass of polyphenylene ether resin and (b) 0 to 10% by mass of styrene resin, 15 to 20 parts by mass of (c) flame retardant, 1.5 to 4.0 parts by mass of (d) phosphite, and 10 to 100 parts by mass of (e) inorganic filler, wherein the total of the above-mentioned (a) polyphenylene ether resin and (b) styrene resin accounts for more than 90% by mass of the resin component contained in the above-mentioned resin composition. In addition, in the above-mentioned resin composition, the mass ratio (c) / (d) of the above-mentioned (c) flame retardant and (d) phosphite is preferably 4.0 or more and 13.0 or less. By setting it as such a structure, a resin composition and a molded product with excellent flame retardancy and excellent heat resistance can be provided.
[0034] That is, although the flame retardant is added to improve the flame retardancy of the polyphenylene ether resin, the flame retardant used in the polyphenylene ether resin generally promotes the formation of char and inhibits combustion. It can be inferred that in the present embodiment, by adding the phosphite, the resin is decomposed by heat during combustion, effectively inhibiting the generation of combustion gas, and further, the free radicals that cause the thermal free radical decomposition of the resin are captured to inhibit the combustion reaction.
[0035] However, it is known that if the content of the phosphite or the flame retardant is too high, heat resistance is poor. In the present embodiment, heat resistance can be achieved by also adjusting the upper limit of the content of the phosphite.
[0036] <(a) Polyphenylene ether resin>
[0037] The resin composition of the present embodiment contains (a) a polyphenylene ether resin.
[0038] The (a) polyphenylene ether resin used in the resin composition of the present embodiment can use a known polyphenylene ether resin, for example, a polymer having a structural unit represented by the following formula in the main chain can be exemplified. The (a) polyphenylene ether resin can be any polymer in a homopolymer or a copolymer. In addition, the (a) polyphenylene ether resin can contain a group having -X(=O)- (X is a carbon atom, a sulfur atom or a phosphorus atom), and more preferably substantially does not contain it. Substantially not containing means that 90% by mass or more, more preferably 95% by mass or more, and further preferably 99% by mass or more of the structural units constituting the (a) polyphenylene ether resin are structural units that do not contain a group having -X(=O)-. As the group having -X(=O)-, a carbonyl group, an ester group, a phosphate group, a phosphite group, a hypophosphite group, a sulfoxide group, a sulfone group, a sulfone group, the like can be exemplified.
[0039] [Chemical formula 2]
[0040]
[0041] (In the formula, 2 R a Each of the two R b Each independently represents a hydrogen atom, a halogen atom, a primary or secondary alkyl group, an aryl group, a halogenated alkyl group, a hydrocarbonoxy group, or a halogenated hydrocarbonoxy group. a Not all are hydrogen atoms.)
[0042] As R a and R b , preferably independently a hydrogen atom, a primary alkyl group or a secondary alkyl group, or an aryl group. Suitable examples of primary alkyl groups include methyl, ethyl, n-propyl, n-butyl, n-pentyl, isopentyl, 2-methylbutyl, 2,3-dimethylbutyl, 2-, 3- or 4-methylpentyl, or heptyl. Suitable examples of secondary alkyl groups include, for example, isopropyl, sec-butyl, or 1-ethylpropyl. In particular, R a It is preferably a primary or secondary alkyl group having 1 to 4 carbon atoms, or a phenyl group. b Preferred is a hydrogen atom.
[0043] Examples of suitable homopolymers of the polyphenylene ether resin (a) include polymers of 2,6-dialkylphenylene ether such as poly(2,6-dimethyl-1,4-phenylene ether), poly(2,6-diethyl-1,4-phenylene ether), poly(2,6-dipropyl-1,4-phenylene ether), poly(2-ethyl-6-methyl-1,4-phenylene ether), and poly(2-methyl-6-propyl-1,4-phenylene ether). Examples of the copolymer include 2,6-dimethylphenol / 2,3,6-trimethylphenol copolymers, 2,6-dimethylphenol / 2,3,6-triethylphenol copolymers, 2,6-diethylphenol / 2,3,6-trimethylphenol copolymers, 2,6-dipropylphenol / 2,3,6-trimethylphenol copolymers and other 2,6-dialkylphenol / 2,3,6-trialkylphenol copolymers; graft copolymers obtained by graft-polymerizing styrene onto poly(2,6-dimethyl-1,4-phenylene ether); and graft copolymers obtained by graft-polymerizing styrene onto 2,6-dimethylphenol / 2,3,6-trimethylphenol copolymers.
[0044] The polyphenylene ether resin (a) in the present embodiment is particularly preferably poly(2,6-dimethyl-1,4-phenylene ether) and a 2,6-dimethylphenol / 2,3,6-trimethylphenol random copolymer. In addition, polyphenylene ether resins with limited terminal groups and copper content as described in Japanese Patent Application Laid-Open No. 2005-344065 can also be preferably used.
[0045] The intrinsic viscosity of the (a) polyphenylene ether resin at 30°C measured in chloroform is preferably 0.2 to 0.8 dL / g, more preferably 0.3 to 0.6 dL / g. By setting the intrinsic viscosity to 0.2 dL / g or more, the mechanical strength of the resin composition tends to be further improved, and by setting it to 0.8 dL / g or less, the fluidity is further improved, and there is a tendency to make molding processing easier. In addition, two or more (a) polyphenylene ether resins having different intrinsic viscosities can be used in combination and set to the range of the intrinsic viscosity.
[0046] The method for producing the polyphenylene ether resin (a) used in the present embodiment is not particularly limited, and can be based on a known method, such as a method of oxidative polymerization of monomers such as 2,6-dimethylphenol in the presence of an amine copper catalyst, in which case the intrinsic viscosity can be controlled to a desired range by selecting reaction conditions. The intrinsic viscosity can be controlled by selecting conditions such as polymerization temperature, polymerization time, and catalyst amount.
[0047] <(b) Styrene resin>
[0048] The resin composition of the present embodiment may contain (b) a styrene-based resin.
[0049] Examples of the styrene resin used in the present embodiment include polystyrene resin (PS), rubber-modified styrene resin (also called high-impact polystyrene, HIPS), acrylonitrile-styrene copolymer (AS resin), acrylonitrile-butadiene-styrene copolymer (ABS resin), methyl methacrylate-acrylonitrile-butadiene-styrene copolymer (MABS resin), acrylonitrile-acrylic rubber-styrene copolymer (AAS resin), acrylonitrile-ethylene propylene rubber-styrene copolymer (AES resin), styrene-IPN (Inter Penetration Network) type rubber copolymer and other resins, styrene-olefin block copolymers, or mixtures thereof.
[0050] In this embodiment, a rubber-modified styrene resin is preferred.
[0051] The rubber-modified styrene-based resin refers to the entire rubber-modified styrene-based resin including rubber particles containing a rubber polymer and one or more styrene-based resins.
[0052] Specifically, it is a resin in which rubber particles containing a rubber polymer are dispersed in a styrene resin matrix, and is a resin obtained by polymerizing a styrene compound alone or by polymerizing a styrene compound and a compound copolymerizable with the styrene compound in the presence of a rubber polymer.
[0053] The rubber particles including the rubber polymer may be rubber particles in which a styrene-based resin is enclosed inside the rubber polymer and / or rubber particles in which a styrene-based resin is grafted outside the rubber polymer.
[0054] As the rubbery polymer in the rubber-modified styrene resin, it is not particularly limited, and can use the acrylic rubbers such as diene rubbers such as polybutadiene, styrene-butadiene copolymer rubber, butadiene-butyl acrylate copolymer rubber, acrylonitrile-butadiene copolymer rubber, polybutyl acrylate, silicone-acrylic composite rubber, polyisoprene, polychloroprene, ethylene-propylene rubber, ethylene-propylene-diene terpolymer rubber, styrene-butadiene block copolymer rubber, styrene-isoprene block copolymer rubber and their hydrides etc. In these rubbery polymers, polybutadiene, styrene-butadiene copolymer rubber, acrylonitrile-butadiene copolymer rubber, polybutyl acrylate etc. can be preferably mentioned. These rubbery polymers can be used alone or in combination of two or more.
[0055] The content of the rubber polymer in the rubber-modified styrene resin is preferably 1% by mass or more, more preferably 2% by mass or more, further preferably 3% by mass or more, and further preferably 5% by mass or more. The content of the rubber polymer in the rubber-modified styrene resin is preferably 50% by mass or less, and from the viewpoint of the impact resistance and molding processability of the resin composition, it is preferably 45% by mass or less, further preferably 40% by mass or less, and further preferably 30% by mass or less.
[0056] Examples of the styrene resin contained in the rubber-modified styrene resin include polystyrene (PS), methyl methacrylate-acrylonitrile-butadiene-styrene copolymer (MABS resin), acrylonitrile-acrylic rubber-styrene copolymer (AAS resin), acrylonitrile-ethylene propylene rubber-styrene copolymer (AES resin), styrene-IPN type rubber copolymer, etc. These may be used alone or in combination of two or more.
[0057] <Mixing ratio of (a) polyphenylene ether resin and (b) styrene resin>
[0058] The resin composition of the present embodiment comprises (a) polyphenylene ether resin and (b) styrene resin in a ratio of 90 to 100% by mass and 0 to 10% by mass. In the resin composition of the present embodiment, when the total of (a) polyphenylene ether resin and (b) styrene resin is set to 100 parts by mass, the ratio of (a) polyphenylene ether resin is preferably 91 parts by mass or more, more preferably 92 parts by mass or more, further preferably 93 parts by mass or more, further preferably 94 parts by mass or more, further more preferably 95 parts by mass or more, and preferably less than 100 parts by mass. By setting it to more than the above lower limit, the effect of combining phosphite can be more effectively exerted, and there is a tendency for heat resistance to be further improved.
[0059] The resin composition of the present embodiment may contain only one kind of each of (a) polyphenylene ether resin and (b) styrene-based resin, or may contain two or more kinds of resins. When containing two or more kinds of resins, the total amount is preferably within the above range.
[0060] In the resin composition of the present embodiment, the total of (a) polyphenylene ether resin and (b) styrene resin accounts for more than 90 mass % of the resin components contained in the resin composition of the present embodiment, preferably accounts for more than 93 mass %, further preferably accounts for more than 95 mass %, further preferably accounts for more than 97 mass %, and further more preferably accounts for more than 99 mass %.
[0061] The total amount of (a) polyphenylene ether resin and (b) styrene resin in the resin combination of the present embodiment is preferably more than 30 mass %, more preferably more than 35 mass %, more preferably more than 40 mass %, more preferably more than 45 mass %, more preferably more than 50 mass %, more preferably more than 55 mass %, particularly preferably more than 60 mass %. By being set to more than the above-mentioned lower limit, there is a tendency that the polyphenylene ether resins and styrene resins such as heat resistance, electrical properties, dimensional stability, impact resistance, low specific gravity originally have. In addition, the total amount of (a) polyphenylene ether resin and (b) styrene resin in the resin combination of the present embodiment is preferably less than 83 mass %, more preferably less than 80 mass %, more preferably less than 75 mass %, more preferably less than 70 mass %. By being set to less than the above-mentioned upper limit, the modification of the additive component that gives the desired characteristic to the resin combination can be effectively played.
[0062] <(c) Flame retardant>
[0063] The resin composition of the present embodiment includes 15 to 20 parts by mass of (c) a flame retardant relative to 100 parts by mass of a total of 90 to 100% by mass of (a) a polyphenylene ether resin and 0 to 10% by mass of (b) a styrene resin. The resin composition of the present embodiment includes (c) a flame retardant to improve flame retardancy.
[0064] The type of the (c) flame retardant used in the present embodiment is not particularly limited, and phosphorus-based flame retardants, halogen-based flame retardants, organometallic flame retardants, etc. can be used. Preferably, it is a phosphorus-based flame retardant, and more preferably, it is a condensed phosphoric acid-based flame retardant.
[0065] Examples of the phosphorus-based flame retardant include ethylphosphinate metal salts, diethylphosphinate metal salts, melamine polyphosphate, condensed phosphate esters, and phosphazene compounds. Among them, condensed phosphate esters or phosphazenes are preferred, and condensed phosphate esters are more preferred.
[0066] The molecular weight of the phosphorus-based flame retardant is preferably 300 or more, more preferably 500 or more, and is preferably 1500 or less, more preferably 1200 or less, and further preferably 1000 or less.
[0067] The condensed phosphate ester is preferably a compound represented by the following formula (1).
[0068] Formula (1)
[0069] [Chemical formula 3]
[0070]
[0071] (In formula (1), R1, R2, R3 and R4 each independently represent a hydrogen atom or an organic group. However, the case where R1, R2, R3 and R4 are all hydrogen atoms is excluded. X represents a divalent organic group, and r represents an integer of 1 to 3.)
[0072] In the above formula (1), examples of the organic group include alkyl groups (e.g., alkyl groups having 1 to 5 carbon atoms), cycloalkyl groups (e.g., cycloalkyl groups having 6 to 12 carbon atoms), and aryl groups (e.g., aryl groups having 6 to 12 carbon atoms) which may or may not have a substituent, and are preferably aryl groups. Examples of the substituent include alkyl groups, alkoxy groups, alkylthio groups, aryl groups, aryloxy groups, arylthio groups, halogen atoms, halogenated aryl groups, and are preferably alkyl groups. In addition, groups in which these substituents are combined, or groups in which these substituents are combined via bonds such as oxygen atoms, sulfur atoms, and nitrogen atoms, may also be used. In addition, the divalent organic group refers to a divalent or higher group obtained by removing one hydrogen atom from the above organic group. Examples include: alkylene groups (e.g., alkylene groups having 1 to 5 carbon atoms), phenylene groups, substituted phenylene groups (e.g., phenylene groups optionally substituted with alkyl groups having 1 to 5 carbon atoms), and polynuclear phenylene groups derived from bisphenols.
[0073] In the present embodiment, in the formula (1), R1, R2, R3 and R4 are each independently preferably a phenyl group which may be substituted with an alkyl group having 1 to 5 carbon atoms (preferably a methyl group).
[0074] In formula (1), X is preferably a phenylene group or a group formed by a combination of a phenylene group and an alkylene group.
[0075] In formula (1), r is preferably 1 or 2, and more preferably 1.
[0076] The compound represented by formula (1) may be a mixture of compounds wherein r is 1 to 3.
[0077] Specific examples of the condensed phosphoric acid ester represented by the above formula (1) include trimethyl phosphate, triethyl phosphate, tributyl phosphate, trioctyl phosphate, triphenyl phosphate, tricresyl phosphate, tricresylphenyl phosphate, octyldiphenyl phosphate, diisopropylphenyl phosphate, tris(chloroethyl) phosphate, tris(dichloropropyl) phosphate, tris(chloropropyl) phosphate, bis(2,3-dibromopropyl) phosphate, bis(2,3-dibromopropyl)-2,3-dichlorophosphate, bis(chloropropyl)monoctyl phosphate, tetraphenylbisphenol A phosphate, tetracresylbisphenol A diphosphate, tetra(xylyl)bisphenol A diphosphate, tetraphenylhydroquinone diphosphate, tetracresylhydroquinone phosphate, tetra(xylyl)hydroquinone diphosphate and the like.
[0078] In addition, as commercially available condensed phosphates, for example, those sold by Daihachi Chemical Industry Co., Ltd. under the trade names of "CR733S" (resorcinol bis(diphenyl phosphate)), "CR741" (bisphenol A bis(diphenyl phosphate)), and "PX-200" (resorcinol bis(di(xylyl) phosphate)), and those sold by ADEKA under the trade name of "ADK STAB FP-900L" (phosphate ester of 1,1'-biphenyl)-4,4'-diol and phenol), can be easily obtained.
[0079] The phosphazene compound is an organic compound having a -P=N- bond in the molecule, and is preferably at least one compound selected from the following: a cyclic phosphazene compound represented by formula (2), a chain phosphazene compound represented by formula (3), and a cross-linked phosphazene compound obtained by cross-linking at least one phosphazene compound selected from formula (2) and formula (3) through a cross-linking group.
[0080] Formula (2)
[0081] [Chemical formula 4]
[0082]
[0083] In formula (2), a is an integer of 3 to 25, R 1 and R 2 are optionally the same or different and represent an alkyl group, a cycloalkyl group, an alkenyl group, an alkynyl group, an aryloxy group, an amino group, a hydroxyl group, an aryl group or an alkaryl group.
[0084] Formula (3)
[0085] [Chemical formula 5]
[0086]
[0087] In formula (3), b is an integer from 3 to 10,000, and R 3 and R 4 are optionally the same or different and represent an alkyl group, a cycloalkyl group, an alkenyl group, an alkynyl group, an aryloxy group, an amino group, a hydroxyl group, an aryl group or an alkaryl group.
[0088] R 5 represents a group selected from -N=P(OR 3 )3 base, -N=P(OR 4 )3 base, -N=P(O)OR 3 Base, -N=P(O)OR 4 At least one of the groups, R 6 Indicates selected from -P(OR 3 )4 base, -P(OR 4 )4-base, -P(O)(OR 3 )2-base, -P(O)(OR 4) at least one of the 2 groups.
[0089] In the above formula (2) and formula (3), examples of the alkyl group include methyl, ethyl, propyl, isopropyl, butyl, tert-butyl, pentyl, hexyl, octyl, decyl, dodecyl and the like. Preferred are alkyl groups having 1 to 6 carbon atoms, such as methyl, ethyl, propyl, isopropyl, butyl, tert-butyl, pentyl, hexyl and the like. Particularly preferred are alkyl groups having 1 to 4 carbon atoms, such as methyl, ethyl, propyl and the like.
[0090] Examples of the cycloalkyl group include cycloalkyl groups having 5 to 14 carbon atoms, such as cyclopentyl and cyclohexyl groups, and cycloalkyl groups having 5 to 8 carbon atoms are preferred.
[0091] Examples of the alkenyl group include alkenyl groups having 2 to 8 carbon atoms, such as vinyl and allyl groups. Examples of the cycloalkenyl group include cycloalkenyl groups having 5 to 12 carbon atoms, such as cyclopentyl and cyclohexyl groups.
[0092] Examples of the alkynyl group include alkynyl groups having 2 to 8 carbon atoms such as ethynyl and propynyl, and alkynyl groups having an aryl group as a substituent such as ethynylphenyl.
[0093] Examples of the aryl group include aryl groups having 6 to 20 carbon atoms, such as phenyl, methylphenyl (ie, tolyl), dimethylphenyl (ie, xylyl), trimethylphenyl, and naphthyl. Among them, aryl groups having 6 to 10 carbon atoms are preferred, and phenyl is particularly preferred.
[0094] Examples of the alkylaryl group include aralkyl groups having 6 to 20 carbon atoms, such as benzyl, phenethyl, and phenylpropyl. Among them, aralkyl groups having 7 to 10 carbon atoms are preferred, and benzyl is particularly preferred.
[0095] Among them, R in formula (2) 1 and R 2 , R in formula (3) 3 and R 4 Preferably, the aromatic phosphazene is an aryl group or an arylalkyl group. By using such an aromatic phosphazene, the thermal stability of the thermoplastic resin composition can be effectively improved. 1 , R 2 , R 3 and R 4 An aryl group is more preferred, and a phenyl group is particularly preferred.
[0096] Examples of the cyclic and / or chain phosphazene compounds represented by formula (2) and formula (3) include (poly) tolyloxyphosphazenes such as phenoxyphosphazene, o-tolyloxyphosphazene, m-tolyloxyphosphazene and p-tolyloxyphosphazene, (poly) xylyloxyphosphazenes such as o- / m-xylyloxyphosphazene, o- / p-xylyloxyphosphazene and m- / p-xylyloxyphosphazene, o- / m- / p-trimethylphenoxyphosphazene, phenoxyo-tolyloxyphosphazene, phenoxym-tolyloxyphosphazene and phenoxyp-tolyloxyphosphazene, (poly) phenoxytolyloxyphosphazenes such as phenoxyo- / m-xylyloxyphosphazene, phenoxyo- / p-xylyloxyphosphazene, phenoxym- / p-xylyloxyphosphazene, (poly) phenoxytolyloxyxylyloxyphosphazenes such as phenoxyo- / m- / p-trimethylphenoxyphosphazene, and the like are preferred. Cyclic and / or chain phenoxyphosphazenes are preferred.
[0097] As the cyclic phosphazene compound represented by formula (2), R 1 and R 2 Cyclic phenoxyphosphazene in which the phenyl group is present. Examples of such cyclic phenoxyphosphazene compounds include compounds such as phenoxycyclotriphosphazene, octaphenoxycyclotetraphosphazene, decaphenoxycyclopentaphosphazene, etc., which are obtained by separating cyclic chlorophosphazenes such as hexachlorocyclotriphosphazene, octachlorocyclotetraphosphazene, and decachlorocyclopentaphosphazene from a mixture of cyclic and linear chlorophosphazenes obtained by reacting ammonium chloride and phosphorus pentachloride at a temperature of 120 to 130° C., and then replacing them with phenoxy groups. In addition, the cyclic phenoxyphosphazene compound is preferably a compound in which a in formula (2) is an integer of 3 to 8, and may be a mixture of compounds in which a is different.
[0098] The average value of a is preferably 3 to 5, more preferably 3 to 4. In addition, it is preferably a mixture of compounds in which the compound with a=3 is 50 mass % or more, the compound with a=4 is 10 to 40 mass % and the total of compounds with a=5 or more is 30 mass % or less.
[0099] As the chain phosphazene compound represented by formula (3), R 3 and R 4 A chain phenoxyphosphazene in which the phenyl group is a chain phenoxyphosphazene. Such a chain phenoxyphosphazene compound may be, for example, a compound obtained by subjecting the hexachlorocyclotriphosphazene obtained by the above method to ring-opening polymerization at a temperature of 220 to 250° C., and then substituting the obtained linear dichlorophosphazene having a polymerization degree of 3 to 10,000 with a phenoxy group. In the formula (3) of the above linear phenoxyphosphazene compound, b is preferably 3 to 1,000, more preferably 3 to 100, and even more preferably 3 to 25.
[0100] Examples of the cross-linked phosphazene compound include compounds having a 4,4'-sulfonyldiphenylene (i.e., bisphenol S residue) cross-linked structure, compounds having a 2,2-(4,4'-diphenylene)isopropyl cross-linked structure, compounds having a 4,4'-oxydiphenylene cross-linked structure, compounds having a 4,4'-thiodiphenylene cross-linked structure, and the like.
[0101] In addition, as the crosslinked phosphazene compound, from the viewpoint of flame retardancy, R in the formula (2) is preferably 1 , R 2 A cross-linked phenoxyphosphazene compound formed by cross-linking a cyclic phenoxyphosphazene compound in which a phenyl group is cross-linked by the cross-linking group, or a cross-linked phenoxyphosphazene compound in which R 3 , R 4 The cross-linked phenoxyphosphazene compound is formed by cross-linking a chain phenoxyphosphazene compound having phenyl groups through the cross-linking group, and more preferably, the cross-linked phenoxyphosphazene compound is formed by cross-linking a cyclic phenoxyphosphazene compound through the cross-linking group.
[0102] In addition, the content of phenylene groups in the cross-linked phenoxyphosphazene compound is usually 50 to 99.9%, preferably 70 to 90%, based on the total number of phenyl groups and phenylene groups in the cyclic phosphazene compound represented by formula (2) and / or the chain phenoxyphosphazene compound represented by formula (3). In addition, the cross-linked phenoxyphosphazene compound is particularly preferably a compound having no free hydroxyl group in its molecule.
[0103] In this embodiment, from the viewpoint of flame retardancy and mechanical properties of the thermoplastic resin composition, the phosphazene compound is preferably at least one selected from a cyclic phenoxyphosphazene compound represented by formula (2) and a cyclic phenoxyphosphazene compound represented by formula (3) formed by cross-linking through a cross-linking group.
[0104] Examples of commercially available products of the phosphazene compound include FP-110 manufactured by Fushimi Pharmaceutical Co., Ltd.
[0105] Relative to 100 parts by mass of (a) 90-100% by mass of polyphenylene ether resin and (b) 0-10% by mass of styrene resin, the content of (c) flame retardant in the resin composition of the present embodiment is 15 parts by mass or more, preferably 16 parts by mass or more, and more preferably 17 parts by mass or more. By setting it to above the above lower limit, there is a tendency for flame retardancy to be further improved. In addition, relative to 100 parts by mass of (a) 90-100% by mass of polyphenylene ether resin and (b) 0-10% by mass of styrene resin, the content of (c) flame retardant is 20 parts by mass or less, preferably 19 parts by mass or less, and more preferably 18 parts by mass or less. By setting it to below the above upper limit, there is a tendency for heat resistance to be further improved.
[0106] The resin composition of the present embodiment may contain only one (c) flame retardant or two or more thereof. When containing two or more thereof, the total amount is preferably within the above range.
[0107] <(d) Phosphites>
[0108] The resin composition of the present embodiment contains 1.5 to 4.0 parts by mass of (d) phosphite relative to a total of 100 parts by mass of (a) 90 to 100% by mass of polyphenylene ether resin and 0 to 10% by mass of (b) styrene resin. The resin composition of the present embodiment can improve heat resistance and flame retardancy by containing (d) phosphite.
[0109] The type of the (d) phosphite used in the present embodiment is not particularly limited, but the (d) phosphite preferably has a structure represented by formula (P). By setting such a configuration, the effects of the present invention can be more effectively exerted.
[0110] Formula (P)
[0111] [Chemical formula 6]
[0112]
[0113] (In formula (P), t-Bu represents a tert-butyl group, R represents a hydrocarbon group having 1 to 10 carbon atoms, and n represents an integer of 0 to 2. * represents a bonding position with other sites.)
[0114] In formula (P), R is preferably an alkyl group or aryl group having 1 to 10 carbon atoms. The alkyl group is preferably an alkyl group having 1 to 5 carbon atoms, and more preferably a tert-butyl group. The aryl group is preferably a phenyl group. In addition, the phenyl group may be substituted with an alkyl group having 1 to 5 carbon atoms.
[0115] The formula (P) is preferably represented by the formula (P1).
[0116] [Chemical formula 7]
[0117]
[0118] In the present embodiment, the compound of formula (P) is preferably bonded to any structure in the following structure. In the following structure, * is the bonding position to formula (P). In addition, the compound of formula (P) is preferably bonded to any structure in the following structure, and has a substituent R on the benzene ring. Here, R has the same meaning as R in formula (P), and the preferred range is also the same.
[0119] [Chemical formula 8]
[0120]
[0121] [Chemical formula 9]
[0122]
[0123] Among the above, the compound represented by the following structure is preferred.
[0124] [Chemical formula 10]
[0125]
[0126] The molecular weight of the phosphite used in the present embodiment, particularly the phosphite having a structure represented by formula (P), is preferably 300 or more, more preferably 400 or more, and further preferably 500 or more. In addition, the molecular weight of the phosphite used in the present embodiment, particularly the phosphite having a structure represented by formula (P), is preferably 1500 or less, more preferably 1200 or less, and further preferably 1000 or less. By setting it to be above the lower limit and below the upper limit, there is a tendency that the effect of the present embodiment is further improved.
[0127] Relative to the total of 100 parts by mass of (a) 90-100% by mass of polyphenylene ether resin and (b) 0-10% by mass of styrene resin, the content of (d) phosphite in the resin composition of the present embodiment is 1.5 parts by mass or more, can be 1.6 parts by mass or more, can be 1.8 parts by mass or more, can be 2.2 parts by mass or more, can be 2.5 parts by mass or more, can also be 3.0 parts by mass or more. By setting it to above the lower limit, there is a tendency that the mechanical strength and flame retardancy of the obtained molded article are further improved. In addition, relative to the total of 100 parts by mass of (a) 90-100% by mass of polyphenylene ether resin and (b) 0-10% by mass of styrene resin, the content of (d) phosphite is 4.0 parts by mass or less, preferably 3.8 parts by mass or less, can be 3.4 parts by mass or less, can be 3.0 parts by mass or less, can be 2.5 parts by mass or less, can also be 2.0 parts by mass or less. By setting it to below the upper limit, there is a tendency that heat resistance is further improved. In addition, phosphite is preferred because it is unlikely to bleed out from the obtained molded article.
[0128] The resin composition of the present embodiment may contain only one type of (d) phosphite, or may contain two or more types. When containing two or more types, the total amount is preferably within the above range.
[0129] In the resin composition of the present embodiment, the mass ratio (c) / (d) of the flame retardant (c) and the phosphite (d) is preferably 4.0 or more, more preferably 4.5 or more, and further preferably 5.0 or more. In addition, as the upper limit of (c) / (d), it is preferably 13.0 or less, more preferably 12.0 or less, further preferably 11.0 or less, and further preferably 10.0 or less. By setting (c) / (d) within the range, heat resistance can be maintained and flame retardancy can be further improved.
[0130] <(e) Inorganic fillers>
[0131] Relative to 100 parts by mass of (a) 90-100% by mass of polyphenylene ether resin and (b) 0-10% by mass of styrene resin, the resin composition of the present embodiment further comprises 10-100 parts by mass of (e) inorganic filler. By including (e) inorganic filler, the mechanical strength of the obtained molded product can be improved. In addition, it can be inferred that when an inorganic filler, particularly a fibrous inorganic filler, is included in the resin composition, the combustible decomposition gas from the resin easily passes through the gap between the fibrous inorganic filler and the resin in the molded product. In the present embodiment, by combining phosphite, the generation of gas from the decomposition of the resin can be effectively suppressed, and therefore, it is effective for the resin composition combined with an inorganic filler, particularly a fibrous inorganic filler.
[0132] As the inorganic filler material that can be contained in the resin composition of the present embodiment, a commonly used inorganic filler material for plastics that has the effect of improving the mechanical properties of the resin composition obtained by being mixed with the resin can be used. Fibrous inorganic fillers such as glass fiber, carbon fiber, basalt fiber, wollastonite, potassium titanate fiber, etc. can be preferably used. In addition, granular or amorphous fillers such as calcium carbonate, titanium oxide, feldspar minerals, clay, organic clay, glass beads, etc.; plate-like fillers such as talc; flaky inorganic fillers such as glass flakes, mica, and graphite can also be used. Among them, from the aspect of mechanical strength and heat resistance, it is preferred to use fibrous fillers, particularly glass fibers. As glass fibers, any cross-sectional shape in a circular cross-sectional shape or a special-shaped cross-sectional shape can be used.
[0133] In order to improve the adhesion with the resin, the inorganic filler is preferably one that has been surface treated with a surface treatment agent such as a coupling agent. Glass fibers to which a surface treatment agent is attached tend to have excellent durability, resistance to moisture and heat, resistance to hydrolysis, and resistance to thermal shock.
[0134] As a surface treatment agent, any known surface treatment agent can be used, and specifically, various coupling agents such as aminosilanes, epoxysilanes, allylsilanes, vinylsilanes, and titanates can be preferably cited. Among them, aminosilanes, epoxysilanes, and vinylsilane surface treatment agents are preferably cited, and specifically, for example, γ-aminopropyl triethoxysilane, γ-aminopropyl trimethoxysilane, and γ-(2-aminoethyl)aminopropyl trimethoxysilane, γ-glycidoxypropyl trimethoxysilane, vinyl trichlorosilane, vinyl triethoxysilane, and γ-methacryloxypropyl trimethoxysilane are preferred examples. Silane compounds can be used alone or in combination. In addition, as needed, materials having been surface treated with lubricants such as fatty acid amide compounds, silicone oils, antistatic agents such as quaternary ammonium salts, epoxy resins, carbamate resins, and resins having film-forming ability, and mixtures of resins having film-forming ability and heat stabilizers, flame retardants, etc. can also be used.
[0135] The glass fiber in the present embodiment refers to a fibrous inorganic material, and more specifically, preferably a chopped shape in which 1,000 to 10,000 glass fibers are bundled and cut into a given length.
[0136] The number average fiber length of the glass fiber in the present embodiment is preferably 0.5 to 10 mm, more preferably 1 to 5 mm. By using glass fibers with such a number average fiber length, the mechanical strength can be further improved. For the number average fiber length, the glass fibers of the object for measuring the fiber length are randomly extracted from the image obtained by observation under an optical microscope and the long sides are measured, and the number average fiber length is calculated based on the obtained measured value. The observation magnification is set to 20 times and the number of roots is set to more than 1000. The number average fiber length is approximately equivalent to the cut length.
[0137] In addition, the cross section of glass fiber can be any shape such as circle, ellipse, oblong, rectangle, the shape formed by merging two short sides of semicircle and rectangle, cocoon type, preferably circle.The circle here is also included in the shape that is usually called circle in the technical field of present embodiment except the circle on geometric meaning.
[0138] The lower limit of the number average fiber diameter of the glass fiber is preferably 4.0 μm or more, more preferably 4.5 μm or more, and further preferably 5.0 μm or more. The upper limit of the number average fiber diameter of the glass fiber is preferably 15.0 μm or less, more preferably 14.0 μm or less. By using a glass fiber with a number average fiber diameter in such a range, there is a tendency to obtain a molded product with better mechanical strength. It should be noted that for the number average fiber diameter of the glass fiber, the glass fiber of the object of measuring the fiber diameter is randomly extracted from the image obtained by observation of an electron microscope, and the fiber diameter is measured at a position close to the central part, and the measured value is calculated. The observation magnification is set to 1000 times, and the number of roots is set to 1000 or more. The number average fiber diameter of the glass fiber with a cross-section other than a circle is set to the number average fiber diameter when converted to a circle with the same area as the cross-sectional area.
[0139] Glass fiber can be obtained by melt spinning of commonly supplied E glass (Electrical glass), C glass (Chemical glass), A glass (Alkali glass), S glass (High strength glass), D glass and alkali-resistant glass, and any fiber can be used as long as it can be made into glass fiber without special limitation. In this embodiment, it is preferred to include E glass.
[0140] Glass fiber can be obtained as a commercial product, for example, T-286H, T-756H, T-127, T-289H, T-852H manufactured by Nippon Electric Glass Co., Ltd., DEFT2A manufactured by Owens Corning Co., Ltd., HP3540 manufactured by PPG Co., Ltd., CSG3PA820 manufactured by Nittobo Co., Ltd., etc.
[0141] In the case where the resin composition of the present embodiment includes an inorganic filler, relative to a total of 100 parts by mass of (a) 90 to 100% by mass of polyphenylene ether resin and (b) 0 to 10% by mass of styrene resin, its content is 10 parts by mass or more, preferably 30 parts by mass or more, more preferably 35 parts by mass or more, more preferably 40 parts by mass or more, and more preferably 45 parts by mass or more. By setting it to above the lower limit, there is a tendency that the mechanical strength of the obtained molded product is further improved. In addition, relative to a total of 100 parts by mass of (a) 90 to 100% by mass of polyphenylene ether resin and (b) 0 to 10% by mass of styrene resin, the upper limit of the content of the above-mentioned inorganic filler is 100 parts by mass or less, preferably 80 parts by mass or less, more preferably 70 parts by mass or less, more preferably 65 parts by mass or less, and more preferably 60 parts by mass or less. By setting it to below the above upper limit, the effect brought about by adding an inorganic filler can be exerted while maintaining molding processability without damaging the fluidity of the resin.
[0142] The resin composition of the present embodiment may contain only one kind of (e) inorganic filler, or may contain two or more kinds of inorganic fillers. When containing two or more kinds of inorganic fillers, the total amount is preferably within the above range.
[0143] <(f) Stabilizer>
[0144] The resin composition of the present embodiment may contain stabilizers such as a heat stabilizer, an antioxidant, etc. It should be noted that in the present invention, phosphite is not included in the stabilizer.
[0145] As stabilizers, inorganic heat stabilizers such as phenol stabilizers, amine stabilizers, phosphorus stabilizers, thioether stabilizers, zinc oxide, etc. can be cited. Among them, in the present embodiment, phenol stabilizers and zinc oxide are preferred. Regarding stabilizers, reference can be made to the records of paragraphs 0036 of International Publication No. 2019 / 026689 and paragraphs 0044 to 0046 of Japanese Patent Publication No. 2022-001624, and their contents are introduced into this specification.
[0146] As the phenol stabilizer, a hindered phenol stabilizer can be preferably used. Specific examples of the hindered phenol stabilizer include pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, diethylene sulfide bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], N,N'-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide], 2,4-dimethyl-6-(1-methylpentadecyl)phenol, diethyl[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]phosphate, 3,3',3",5,5',5"-hexa-tert-butyl-a,a',a"-( mesityl-2,4,6-triyl) tri-p-cresol, 4,6-bis(octylthiomethyl)-o-cresol, ethylenebis(oxyethylene)bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate], hexamethylenebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 2,6-di-tert-butyl-4-(4,6-bis(octylthio)-1,3,5-triazine-2-ylamino)phenol, 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)ethyl]-4,6-di-tert-pentylphenyl acrylate, etc.
[0147] Among them, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate are preferred. Specific examples of such hindered phenol stabilizers include "Irganox (registered trademark, hereinafter the same) 1010" and "Irganox 1076" manufactured by BASF, and "ADEKA STAB AO-50" and "ADEKA STAB AO-60" manufactured by ADEKA.
[0148] Relative to 100 parts by mass of the resin composition, the content of the stabilizer in the resin composition of the present embodiment is preferably 0.001 parts by mass or more, more preferably 0.005 parts by mass or more, further preferably 0.01 parts by mass or more, and further preferably 0.1 parts by mass or more, and preferably less than 5 parts by mass, more preferably less than 4 parts by mass, further can be less than 3 parts by mass, less than 2 parts by mass, less than 1 part by mass. By setting the content of the stabilizer to the above range, the addition effect of the stabilizer can be more effectively exerted.
[0149] The resin composition of the present embodiment may contain only one type of stabilizer or two or more types. When containing two or more types, the total amount is preferably within the above range.
[0150] <(g) Coloring agent>
[0151] The resin composition of the present embodiment may contain a colorant. By containing a colorant, a color tone can be given to the obtained molded article, and there is a tendency that the designability is improved.
[0152] The colorant may be a pigment or a dye, and is preferably a pigment.
[0153] Examples of the pigment include inorganic pigments (black pigments such as carbon black, red pigments such as red iron oxide, orange pigments such as molybdenum chrome orange, white pigments such as titanium oxide), organic pigments (yellow pigments, orange pigments, red pigments, blue pigments, green pigments, etc.), etc., preferably inorganic pigments, more preferably white pigments, and still more preferably titanium oxide.
[0154] When a colorant is blended into the resin composition of the present embodiment, the colorant may be blended in the form of a masterbatch.
[0155] When the resin composition in the present embodiment includes a colorant, the content thereof is preferably 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, and further preferably 0.5 parts by mass or more relative to 100 parts by mass of the resin composition. In addition, the content of the colorant is preferably 10.0 parts by mass or less, more preferably 5.0 parts by mass or less, and further preferably 3.0 parts by mass or less relative to 100 parts by mass of the resin composition.
[0156] The resin composition of the present embodiment may contain only one colorant or two or more colorants. When containing two or more colorants, the total amount is preferably within the above range.
[0157] <Other ingredients>
[0158] The resin composition of the present embodiment may contain other components besides the above.
[0159] Specific examples include thermoplastic resins such as polyamide resins, polyester resins, polyphenylene sulfide resins, liquid crystal polyester resins, polycarbonate resins, polyacetal resins, polyacrylonitrile resins, acrylic resins, polyethylene resins, and thermosetting resins such as epoxy resins, melamine resins, and silicone resins. Two or more of these thermoplastic resins and thermosetting resins may be used in combination.
[0160] In addition, the resin composition of the present embodiment may include a resin additive. Specifically, it may include an internal lubricant (fatty acid metal salt, polyethylene wax, etc.), a heat stabilizer (zinc oxide, etc.), a release agent (silicone oil, fatty acid, fatty acid ester, etc.), a weathering improver, a nucleating agent, an impact modifier, a plasticizer, a fluidity improver, etc. When containing these components, when combined, the total content is preferably set to the range of 0.01 to 5% by mass of the resin composition.
[0161] The resin composition of the present embodiment can be prepared such that the total of (a) polyphenylene ether resin, (b) styrene resin, (c) flame retardant, (d) phosphite, and (e) inorganic filler, and other components as required are 100% by mass. In addition, for the resin composition of the present embodiment, the total of (a) polyphenylene ether resin, (b) styrene resin, (c) flame retardant, (d) phosphite, and (e) inorganic filler, (f) stabilizer, and (g) pigment preferably accounts for 95% by mass or more of the resin composition, more preferably 97% by mass or more, and further preferably 99% by mass or more.
[0162] <Method for producing resin composition>
[0163] As a method for producing the resin composition of the present embodiment, any method can be adopted.
[0164] For example, the following method can be cited: (a) polyphenylene ether resin, (b) styrene resin, (c) flame retardant, (d) phosphite and other components are mixed using a mixing device such as a V-type blender to prepare a total mixed product, and then melt-kneading is performed through an extruder with a vent to form pellets. Alternatively, as a two-step mixing method, the following method can be cited: after a part of the components are fully mixed in advance, melt-kneading is performed through an extruder with a vent to produce pellets, and then the pellets are mixed with other components and melt-kneaded through an extruder with a vent.
[0165] When (e) an inorganic filler is added, side feeding may be performed.
[0166] <Characteristics of resin composition>
[0167] The resin composition of the present embodiment can particularly satisfy the following properties.
[0168] The resin composition of the present embodiment, when molded into an ISO3167:93A type test piece, preferably has a deflection temperature under load (DTUL) based on ISO-75-1 of 139°C or more, more preferably 140°C or more, further preferably 141°C or more, further preferably 142°C or more, and further more preferably 143°C or more. The upper limit of the deflection temperature under load is not particularly limited, but is actually 170°C or less, and may also be 160°C or less. Such a deflection temperature under load can be achieved by precisely adjusting the blending amounts of the flame retardant and the phosphite, respectively.
[0169] The flame retardancy of the resin composition of the present embodiment preferably satisfies V-0, which is based on a vertical flammability test (UL94V test: 1.5 mmt) of 5 groups in accordance with the UL94 standard. Such a load deflection temperature can be achieved by precisely adjusting the amount of the flame retardant and the phosphite, respectively.
[0170] <Application of resin composition>
[0171] The resin composition of the present embodiment can be widely used for applications in which a polyphenylene ether resin is generally used, and in particular, a blend of a polyphenylene ether resin and a styrene-based resin is used.
[0172] For example, they can be used for automobile exterior / exterior panel parts, automobile interior parts, and automobile engine compartment parts. Specifically, they are suitable for exterior / exterior panel parts such as bumpers, fenders, door panels, decorative strips, emblems, engine covers, wheel covers, roof panels, spoilers, engine covers, and interior parts such as engine compartment parts, instrument panels, and console decorative strips.
[0173] In addition, it can also be used as cabinets, bases, refrigerators, air conditioners, LCD projectors, etc. for various computers and their peripherals, other OA equipment, televisions, video recorders, various CD players, etc.
[0174] In addition, it can be used as fuel casings for solid methanol batteries, secondary battery cells, fuel cell water pipes, cold water tanks, boiler casings, ink peripheral parts / components and bases for inkjet printers, as well as molded products such as water pipes and joints.
[0175] The molded article of the present embodiment is formed from the resin composition of the present embodiment.
[0176] The manufacture method of the molded product in the present embodiment is not particularly limited, and the molding method usually adopted for resin combination can be arbitrarily adopted. If its example is cited, the hollow molding methods such as injection molding, ultra-high speed injection molding, injection compression molding, double color molding, gas-assisted, the molding method using a heat insulation mold, the molding method using a rapid heating mold, foam molding (also comprising supercritical fluid), insert molding, IMC (intermetallic compound molding) molding method, extrusion molding, sheet molding, thermoforming, rotational molding, stacking molding, compression molding, blow molding, etc. can be cited. In addition, the molding method using a hot runner mode can also be utilized.
[0177] Example
[0178] Below, enumerate embodiment and the present invention is further specifically described.As long as the material, dosage, ratio, processing content, processing step etc. shown in the following embodiment do not depart from the gist of the present invention, just can be appropriately changed.Therefore, the scope of the present invention is not limited to the specific example shown below.
[0179] When the measuring equipment used in the examples is difficult to obtain due to discontinuation of production or the like, other equipment having equivalent performance may be used for the measurement.
[0180] 1. Raw materials
[0181] The raw materials described in the following Table 1 were used.
[0182] [Table 1]
[0183]
[0184] 2. Examples 1 to 7, Comparative Examples 1 to 12
[0185] The components were mixed in the ratios (parts by mass) shown in Tables 2 to 4 below, and melt-kneaded using a twin-screw extruder (TEM18SS manufactured by Shibaura Machine Co., Ltd.) at a barrel temperature of 290°C, a die temperature of 300°C, and a screw speed of 300 rpm to obtain a resin composition (pellets).
[0186] The following evaluations were performed using the obtained resin composition (pellets).
[0187] <Flame retardancy>
[0188] After drying the pellets obtained by the above-mentioned manufacturing method at 120°C for 2 hours, a test piece for a flammability test having a length × width × thickness = 125 mm × 13 mm × 1.5 mm was molded by an injection molding machine (manufactured by Shibaura Machine Co., Ltd., "EC75SX") at a cylinder temperature of 300°C and a mold temperature of 100°C.
[0189] The obtained test pieces for the flammability test were subjected to two vertical flammability tests (UL94V test: 1.5mmt) in accordance with the UL94 standard for five groups. The grades are classified into V-0, V-1, and V-2 in order from the good grade. Each group was judged according to the grade based on the vertical flammability test, as shown in Tables 2 to 4. At this time, the results with long burning times and inability to be classified into V-0, V-1, and V-2 were recorded as NG. It should be noted that when the results of the two tests were different, the result of the low flame retardancy grade was adopted.
[0190] <Deflection Temperature Under Load(DTUL)(℃)>
[0191] After drying the pellets obtained by the above-mentioned manufacturing method at 120°C for 2 hours, ISO3167:93A type test pieces (hereinafter referred to as "ISO test pieces") were injection molded using an injection molding machine (manufactured by Shibaura Machine Co., Ltd., "EC75SX") at a cylinder temperature of 300°C and a mold temperature of 100°C based on ISO-15103.
[0192] The deflection temperature under load of 1.80 MPa (unit: °C) was measured using a strip-shaped test piece of 80 mm×10 mm×4 mm prepared by machining the parallel portion of the ISO test piece in accordance with ISO-75-2.
[0193] <Charpy impact strength with notch (kJ / m 2 )>
[0194] Based on ISO-179-1 and ISO179-2, the ISO test piece obtained above was cut to remove the clamping parts at both ends and to form a notch (notch) in the center to form a notched Charpy impact test piece. The notched Charpy impact strength (unit: kJ / m2) at 23°C was measured for the obtained notched Charpy impact test piece based on ISO-179-1 and ISO179-2. 2 ) was used as the impact resistance evaluation.
[0195] <Tensile strength(MPa)>
[0196] The tensile strength was measured based on ISO-527 using the ISO test piece obtained above.
[0197] <Flexural strength (MPa) and flexural modulus (MPa)>
[0198] The flexural strength (unit: MPa) and flexural modulus (unit: MPa) were measured in an environment of temperature 23°C and humidity 50% in accordance with ISO-178 using a 80 mm×10 mm×4 mm long test piece prepared by machining the parallel portion of the ISO test piece.
[0199]
[0200]
[0201]
[0202] From the above results, it is clear that the resin composition of the present invention can improve flame retardancy without reducing heat resistance by adding phosphite (Examples 1 to 7).
[0203] In contrast, when the phosphite is not included or the content is insufficient (Comparative Examples 1 to 4), the flame retardancy is poor. In addition, in the above resin composition, if the content of the flame retardant is increased to compensate for the flame retardancy (Comparative Examples 5 and 9), the load deflection temperature is low and the heat resistance is poor.
[0204] On the other hand, when the content of the phosphite was too large (Comparative Examples 6, 7, and 8), the deflection temperature under load was low and the heat resistance was poor.
[0205] In addition, when the ratio of the styrene-based resin was too large (Comparative Example 10), heat resistance and flame retardancy were inferior.
[0206] Furthermore, since the resin composition of the present invention contains an inorganic filler, even if (c) / (d) is appropriate, the flame retardancy is poor if the amounts of (c) the flame retardant and (d) the phosphite are small (Comparative Examples 11 and 12).
Claims
1. A resin composition, in, The composition comprises 15 to 20 parts by mass of a flame retardant, 1.5 to 4.0 parts by mass of a phosphite, and 10 to 100 parts by mass of an inorganic filler, relative to 100 parts by mass of a total of (a) 90 to 100 parts by mass of a polyphenylene ether resin and (b) 0 to 10 parts by mass of a styrene-based resin. The total amount of the (a) polyphenylene ether resin and the (b) styrene-based resin accounts for 90% by mass or more of the resin components contained in the resin composition. The mass ratio (c) / (d) of the (c) flame retardant to the (d) phosphite is 4.0 or more and 13.0 or less.
2. The resin composition according to claim 1, in, (c) The flame retardant is a phosphorus-based flame retardant.
3. The resin composition according to claim 1 or 2, in, (d) the phosphite has a structure represented by formula (P), Formula (P) In the formula (P), t-Bu represents a tert-butyl group, R represents a hydrocarbon group having 1 to 10 carbon atoms, n represents an integer of 0 to 2, and * represents a bonding position with other sites.
4. A resin composition, in, The composition comprises 15 to 20 parts by mass of a flame retardant, 1.5 to 4.0 parts by mass of a phosphite, and 10 to 100 parts by mass of an inorganic filler, relative to 100 parts by mass of a total of (a) 90 to 100 parts by mass of a polyphenylene ether resin and (b) 0 to 10 parts by mass of a styrene-based resin. The total amount of the (a) polyphenylene ether resin and the (b) styrene-based resin accounts for 90% by mass or more of the resin component contained in the resin composition.
5. A molded article formed from the resin composition according to claim 1, 2 or 4.