Method for circulating iron-based plating solution, method for producing iron-based plating solution, and method for producing alloyed hot-dip galvanized steel sheet

Through the combined treatment of vertical centrifugal separation solid-liquid separation device and final adjustment tank, the problems of low plating electrolytic efficiency and sludge in iron-based electroplating solution are solved, and efficient and stable circulation of iron-based electroplating solution is achieved, improving the efficiency and stability of iron-based electroplating solution. The quality and production efficiency of galvanized steel plates are provided.

CN119013441APending Publication Date: 2024-11-22JFE STEEL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280093563.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-18
Filing Date
2022-12-27
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing iron electroplating solution circulation methods have problems such as low plating electrolytic efficiency, sludge generation and high equipment cost, and it is difficult to completely remove fine sludge, affecting production efficiency and product quality.

Method used

The iron-based electroplating solution is circulated by using a vertical centrifugal separation solid-liquid separation device and a final adjustment tank. By measuring Fe3+ concentration, the iron source input is adjusted, and the pH value and temperature are controlled to ensure that the iron-based electroplating solution is in the reduction tank and the final adjustment tank. The treatment in the process achieves efficient reduction and sludge recovery.

Benefits of technology

It realizes high electrolytic efficiency, sludge-free, stable and power-saving iron electroplating solution circulation, improves the plating adhesion and appearance quality of galvanized steel plates, and reduces equipment demand and operating costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013441A_ABST
    Figure CN119013441A_ABST
Patent Text Reader

Abstract

Provided are a method for circulating an iron-based plating solution, a method for producing an iron-based plating solution, and a method for producing an alloyed hot-dip galvanized steel sheet, with which it is possible to produce an iron-based plating solution that has high electrolytic efficiency and is stable and power-saving without the inclusion of sludge, without the need for huge equipment. The present invention also provides a method for producing an iron-based plating solution, and a method for producing an alloyed hot-dip galvanized steel sheet. The method for circulating an iron-based plating solution performs circulation adjustment on an iron-based plating solution (P) used in a plating bath (10) for iron-based plating. An iron-based plating solution (P) used in a plating bath (10) is treated at least through a reduction bath (30), a vertical centrifugal solid-liquid separation device (40), and a final adjustment bath (50) in this order, and then is introduced into the plating bath (10). In the reduction tank (30), an iron source for reduction is introduced in accordance with the concentration of Fe < 3 + > (ferric ion) in the iron-based plating (P) solution transferred to the reduction tank (30).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for circulating an iron-based plating solution used in an electroplating tank, a method for producing an iron-based plating solution, and a method for producing an alloyed hot-dip galvanized steel sheet including a step of performing an iron-based plating treatment. Background Art

[0002] In recent years, there has been an increasing demand for high-tensile steel sheets (high-strength steel sheets) that can be used for lightweight structures, etc. in the fields of automobiles, home appliances, building materials, etc. As high-strength steel sheets, for example, it is known that steel sheets with good hole expandability are obtained by containing Si in steel, and steel sheets with good ductility are obtained by easily forming retained γ by containing Si, Al, and Mn.

[0003] However, when a high-tensile steel sheet containing a large amount (especially 0.2% by mass or more) of Si and Mn is used as a base material to manufacture an alloyed hot-dip galvanized steel sheet, the following problems exist. The alloyed hot-dip galvanized steel sheet is manufactured by heating and annealing the base material steel sheet at a temperature of about 600 to 900°C in a reducing atmosphere or a non-oxidizing atmosphere, hot-dip galvanizing the steel sheet, and further heating and alloying the galvanized steel sheet. Here, Si and Mn in the steel are easily oxidizable elements, and they will be selectively oxidized even in a generally used reducing atmosphere or a non-oxidizing atmosphere, and will be enriched on the surface of the steel sheet to form oxides. The oxide reduces the wettability with molten zinc during the plating process, resulting in unplating. Therefore, as the concentration of Si and Mn in the steel increases, the wettability decreases sharply, and unplating often occurs. In addition, even if unplating is not achieved, there is a problem of poor plating adhesion. Furthermore, if Si and Mn in the steel are selectively oxidized and concentrated on the surface of the steel sheet, there is also a problem that a significant alloying delay occurs in the alloying process after hot-dip galvanizing, which significantly impedes productivity.

[0004] To solve such a problem, for example, Patent Document 1 discloses a method for producing a high-tensile hot-dip galvanized steel sheet, wherein the base steel sheet is subjected to a 0.2 to 2 g / m 2 The steel is then plated with Fe, and then the direct-fired heating furnace (DFF) and the radiation heating furnace (RTF) are adjusted to the specified conditions, thereby inhibiting the surface diffusion of Si, Mn or Al, which are difficult-to-plate elements contained in the steel, to form oxides. By inhibiting the surface diffusion of Si, Mn or Al to form oxides, the unplated phenomenon can be prevented, excellent plating surface quality and plating adhesion can be ensured, high strength can be ensured, and further, the manufacturing cost can be reduced. However, it is known that there is Fe in the iron-based plating solution that is consumed by the electrolysis of the plating film. 2+ and Fe without electrolysis reaction 3+ , in Fe 3+Many plating solutions have the following problems: reduction in plating electrolytic efficiency, clogging of piping due to the generation of sludge (fine solid matter), adhesion of sludge to steel sheets, and limitation of continuous operation due to maintenance for removing sludge.

[0005] To address this problem, Patent Document 2 discloses a method for Fe 3+ When reducing, replenishing and dissolving ions in the plating solution and supplying iron powder, the stirring mechanism in the tank is used to efficiently reduce Fe 3+ method.

[0006] Patent Document 3 discloses a method for supplying iron ions in iron alloy electroplating, wherein the relationship between the diameter and height of a cylindrical iron chip filling layer in an iron chip dissolving tank is specified, or the Fe ion content in the plating solution at the inlet side of the iron chip dissolving tank is set to 3+ The concentration is 5g / L or more, and the relative flow rate between the iron chips being dissolved and the plating solution being pressed in is 3m / min or more, thereby efficiently reducing Fe 3+ .

[0007] Patent Document 4 discloses a method for efficiently reducing trivalent Fe ions in an iron-based electroplating solution by reducing the surface area Sm of the iron powder filled in a stirring tank to 1.5 2 The amount of plating solution circulating to the stirring tank Qm 3 / hr ratio H (= S / Q) is 1≤H≤5, so that Fe 3+ reduction.

[0008] Patent document 5 discloses a sludge separation and treatment device for a continuous electroplating device, which, in order to efficiently remove the sludge generated in the electroplating solution, adds a coagulant precipitant to the plating solution containing sludge that is partially extracted and sent from a plating solution circulation tank in a sludge sedimentation tank, stirs and mixes the solution, thereby settling the sludge, and separates and recovers the sludge.

[0009] Although Patent Document 6 does not explicitly state that the centrifugal separator is used for electroplating, it discloses a horizontal centrifugal separator that has improved airtightness, is compact, and is capable of continuous operation as a general-purpose centrifugal separator.

[0010] Prior art literature

[0011] Patent Literature

[0012] Patent Document 1: International Publication No. 2013 / 100615

[0013] Patent Document 2: Japanese Patent Application Laid-Open No. 3-2399

[0014] Patent Document 3: Japanese Patent Application Laid-Open No. 3-243798

[0015] Patent Document 4: Japanese Patent Application Laid-Open No. 6-306697

[0016] Patent Document 5: Japanese Patent Application Publication No. 2012-188715

[0017] Patent Document 6: International Publication No. 2009 / 072209 Summary of the invention

[0018] However, the existing methods for supplying iron ions in iron-based alloy electroplating shown in Patent Document 2 and Patent Document 3, the efficient reduction method of trivalent Fe ions in an iron-based electroplating solution shown in Patent Document 4, the sludge separation treatment device for a continuous electroplating device shown in Patent Document 5, and the horizontal centrifugal separation device shown in Patent Document 6 have the following problems.

[0019] That is, in the iron ion supply method in iron-based alloy electroplating shown in Patent Documents 2 and 3, and the efficient reduction method of trivalent Fe ions in an iron-based electroplating solution shown in Patent Document 4, although efficient Fe 3+ However, in these methods, the amount of iron powder or iron filings to be added is unclear. Therefore, if the iron source is relatively large relative to the Fe 3+ Less, even if Fe 3+ The reduction efficiency of Fe 3+ will also remain, so the plating electrolysis efficiency is reduced, or Fe 3+ On the other hand, if the iron source is relatively large relative to the Fe 3+ If it is too much, there are problems such as increased damage to the piping due to the excess iron source, and increased sludge due to the increase in pH of the plating solution accompanying the reduction reaction, which also has an adverse effect on the operation.

[0020] In addition, the sludge separation treatment device of the continuous electroplating device shown in Patent Document 5 is a so-called sedimentation method in which a coagulation precipitant is added to a plating solution containing sludge in a sludge sedimentation tank and stirred and mixed to settle the sludge, and the sludge is separated and recovered. However, in the sludge separation treatment device of the continuous electroplating device shown in Patent Document 5, since the processing flow rate is small, a huge device is required to cope with the continuous production of the iron-based electroplating solution, which has problems in terms of cost and installation space.

[0021] Furthermore, in the case of the horizontal centrifugal separator shown in Patent Document 6, although it can be operated continuously, it cannot completely remove the fine sludge contained in the iron-based plating solution, and the separation rate of the sludge can only be about 70%.

[0022] Therefore, the present invention is made to solve the existing problems, and its purpose is to provide a circulation method for iron-based plating solution, a manufacturing method for iron-based plating solution, and a manufacturing method for alloyed hot-dip galvanized steel sheet, which can produce an iron-based plating solution with high electrolysis efficiency, no sludge mixing, stable and energy-saving without the need for huge equipment.

[0023] In order to solve the above-mentioned problems, a circulation method of an iron-based electroplating solution in one embodiment of the present invention is a circulation method of an iron-based electroplating solution used in an electroplating tank for iron-based electroplating, wherein the iron-based electroplating solution used in the electroplating tank is subjected to circulation adjustment, wherein the iron-based electroplating solution is subjected to circulation adjustment by at least passing through a reduction tank and a vertical centrifugal separation type solid-liquid separation device in sequence, and then is put into the electroplating tank, wherein in the reduction tank, the iron-based electroplating solution transferred to the reduction tank is subjected to circulation adjustment by at least passing through a reduction tank and a vertical centrifugal separation type solid-liquid separation device in sequence, and then is put into the electroplating tank, wherein the iron-based electroplating solution ... device in sequence, and then the iron-based electroplating solution is subjected to circulation adjustment by at least passing through a reduction tank and a vertical centrifugal separation device in sequence, and then the iron-based electroplating solution is subjected to circulation adjustment by at least passing through a reduction tank and a vertical centrifugal separation device in sequence, and then the iron-based 3+ (ferric ion) concentration is added into the iron source for reduction.

[0024] A method for producing an iron-based plating solution according to another aspect of the present invention is to produce an iron-based plating solution by performing circulation adjustment using the above-mentioned circulation method for an iron-based plating solution.

[0025] Furthermore, a method for producing an alloyed hot-dip galvannealed steel sheet according to another embodiment of the present invention is gist of including a step of performing an iron-based electroplating treatment on a steel sheet using an iron-based electroplating solution produced by the above-mentioned method for producing an iron-based electroplating solution.

[0026] According to the circulation method of the iron-based electroplating solution, the manufacturing method of the iron-based electroplating solution, and the manufacturing method of the alloyed hot-dip galvanized steel sheet of the present invention, there can be provided a circulation method of the iron-based electroplating solution, a manufacturing method of the iron-based electroplating solution, and a manufacturing method of the steel sheet, which can produce an iron-based electroplating solution with high electrolysis efficiency, no sludge mixing, stable and energy-saving without the need for huge equipment. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a schematic diagram of the structure of an electroplating facility to which a circulation method of an iron-based electroplating solution according to an embodiment of the present invention is applied. DETAILED DESCRIPTION

[0028] The embodiments of the present invention are described below with reference to the drawings. The embodiments shown below illustrate devices or methods for implementing the technical concept of the present invention, and the technical concept of the present invention does not limit the material, shape, structure, arrangement, etc. of the components to the following embodiments.

[0029] In addition, the drawings are schematic diagrams, so it should be noted that the relationship and ratio of thickness and plane dimensions are different from the actual ones, and the drawings also include portions where the relationship and ratio of dimensions are different from each other.

[0030] Figure 1 Detailed description of the drawings is given in the accompanying drawings. Detailed description of the drawings shows a schematic structure of an electroplating facility to which a circulation method of an iron-based electroplating solution according to an embodiment of the present invention can be applied.

[0031] Figure 1 The electroplating equipment 1 shown is equipped with an electroplating tank 10 for iron-based electroplating for performing iron-based electroplating treatment on a steel sheet S as a plated material. The electroplating tank 10 is a horizontal type plating tank, and uses a current-carrying roller 14 to make the steel sheet S move in the horizontal direction, and supplies the iron-based electroplating solution P in the treatment tank 11 to the gap between the steel sheet S and a pair of anodes 12, and conducts electricity between the plated surface of the steel sheet S as a cathode and the pair of anodes 12, so that the iron-based electroplating treatment is performed on both sides of the steel sheet S. Figure 1 In the figure, symbol 13 is a plating solution nozzle head. In the present embodiment, the electroplating tank 10 is a horizontal plating tank, but it can also be any form of a vertical plating tank or a radial tank, etc. In addition, the electroplating tank 10 can be connected to a plurality of these processing devices, and can also have an intermediate tank between the processing devices.

[0032] Here, the "iron-based plating solution" is defined as a plating solution containing metal ions and having an Fe ion concentration of 60% or more.

[0033] In addition, the electroplating equipment 1 is provided with a plating solution circulation tank 20 for supplying an iron-based plating solution P to the plating tank 10. In order to circulate the iron-based plating solution P, the treatment tank 11 of the plating tank 10 and the plating solution circulation tank 20 are connected by a pipe 15 for transferring the iron-based plating solution P from the treatment tank 11 to the plating solution circulation tank 20. In addition, one plating solution nozzle head 13 of the plating tank 10 and the plating solution circulation tank 20 are connected by a pipe 24 for supplying the iron-based plating solution P from the plating solution circulation tank 20 to one plating solution nozzle head 13 by a pump 25, and a pipe 26 branched from the pipe 24. In addition, another plating solution nozzle head 13 of the plating tank 10 and the plating solution circulation tank 20 are connected by a pipe 24 for supplying the iron-based plating solution P from the plating solution circulation tank 20 to another plating solution nozzle head 13 by a pump 25, and a pipe 27 branched from the pipe 24. In order to make the iron-based plating solution P in a non-oxidizing state without contacting with air, it is preferred to fill the plating solution circulation tank 20 with nitrogen (N 2 gas).

[0034] In addition, the electroplating equipment 1 has a method for circulating Fe in the iron-based electroplating solution P from the plating solution circulation tank 20. 3+ The plating solution circulation tank 20 and the reduction tank 30 are connected by a pipe 21 for supplying the iron-based electroplating solution P transferred from the treatment tank 11 to the plating solution circulation tank 20 to the reduction tank 30 by a pump 22. 3+ 23, the Fe 3+ The Fe content in the iron-based plating solution P is measured before the iron-based plating solution P is supplied to the reduction tank 30. 3+(ferric ion) concentration. Fe 3 + It can be used to determine Fe 3+ The concentration of (ferric ion) may be measured by any method, but for example, an absorptiophotometer may be used.

[0035] Then, in the reduction tank 30, according to the Fe 3+ Fe in iron-based plating solution P measured by the meter 3+ The concentration of iron (trivalent iron ions) is set to the iron source (iron powder or iron filings) for reduction. The iron source can be adjusted appropriately according to the reduction efficiency, preferably about Fe 3+ (ferric iron) concentration is 1.1 to 1.3 times. In addition, a stirrer 31 for stirring the iron-based electroplating solution P in the reduction tank 30 is provided in the reduction tank 30. In addition, a pH meter 32 for measuring the pH of the iron-based electroplating solution P in the reduction tank 30 is provided in the reduction tank 30. Since the pH of the iron-based electroplating solution P during reduction may increase due to the input of the iron source, thereby increasing the sludge, sulfuric acid is added in a manner to always maintain it below 2.3. There is no lower limit for the pH of the iron-based electroplating solution P during reduction, but from the viewpoint of reducing the pH readjustment process in the final adjustment tank 50 described later and reducing the amount of reagent adjustment, the pH is preferably above 1.0, and more preferably above 2.0. In addition, in order to make the iron-based electroplating solution P form a non-oxidizing state without contacting with the air, nitrogen (N 2 gas).

[0036] In addition, the electroplating equipment 1 is provided with a vertical centrifugal separation type solid-liquid separator 40 for separating sludge in the iron-based electroplating solution P from the iron-based electroplating solution P. The reduction tank 30 and the solid-liquid separator 40 are connected by a pipe 33 for supplying the iron-based electroplating solution P reduced in the reduction tank 30 to the solid-liquid separator 40 by a pump 34. The solid-liquid separator 40 is a vertical centrifugal separator 40. Figure 1A vertical centrifugal separation type in which a screw 43 is arranged in a manner extending in the vertical direction (in the vertical direction) of the centrifugal separation cylinder 41, and a screw outer cylinder 42 that rotates differentially with each other and a screw 43 arranged in the screw outer cylinder 42 are provided in the centrifugal separation cylinder 41 so that solids (sludge) and liquids in the iron-based electroplating solution P as a raw liquid are centrifugally separated by specific gravity difference. Moreover, the rotating shaft 44 of the screw 43 is formed in a cylindrical shape so that the iron-based electroplating solution P as a raw liquid is guided from the screw 43 into the screw outer cylinder 42, and a diffusion opening 48 is formed on the side of the rotating shaft 44. The screw outer cylinder 42 and the screw 43 are equipped in the centrifugal separation cylinder 41. Moreover, the rotating shaft 44 of the screw 43 in the centrifugal separation cylinder 41 is formed with a raw liquid supply port 45 for supplying the iron-based electroplating solution P as a raw liquid from the pipe 33 to the diffusion opening 48. In addition, a separation water outlet 46 is provided on the side of the centrifugal separation drum 41, and a solid outlet 47 for discharging solids (sludge) is provided on the bottom surface of the centrifugal separation drum 41. As the vertical centrifugal separation type solid-liquid separator 40, for example, the solid-liquid separator described in Japanese Patent Application Laid-Open No. 2007-38068 can be used.

[0037] If such a vertical centrifugal separation type solid-liquid separator 40 is used, even if the sludge in the iron-based electroplating solution P contains a wide range of particle sizes including 0.5 to 100 μm, the sludge can be separated and recovered at a recovery rate of more than 90%. However, even with this solid-liquid separator 40, if the centrifugal force is increased, the fine sludge below 5 μm will not be separated, but will be brought to the cleaning liquid side, which reduces the separation efficiency. Therefore, the centrifugal force is preferably 1000 to 1800 G, and the speed difference between the screw 43 and the screw outer cylinder 42 is preferably 1.0 to 2.0 rpm. When the centrifugal force is less than 1000 G, the centrifugal force is insufficient, the separation effect is small, and the separation performance is reduced. When the speed difference between the screw 43 and the screw outer cylinder 42 is less than 1.0 rpm, the scraping time of the screw 43 is short and the separation efficiency is reduced. When the speed difference exceeds 2.0 rpm, although the scraping time of the screw 43 becomes longer, the mixing of particles in the cleaning liquid increases, so as a result, the separation efficiency is reduced, which is not preferred.

[0038] Furthermore, a solid receiving tank 49 for receiving the solid (sludge) discharged from the solid discharge port 47 is provided below the solid-liquid separation device 40 .

[0039] In addition, the electroplating equipment 1 preferably includes a final adjustment tank 50 for adjusting the iron-based electroplating solution P from which solids (sludge) are separated in the solid-liquid separation device 40 to a plating solution state suitable for effective iron-based electroplating. The separation water outlet 46 of the solid-liquid separation device 40 and the final adjustment tank 50 are preferably connected by a pipe 55 for supplying the iron-based electroplating solution P from which solids (sludge) are separated in the solid-liquid separation device 40 to the final adjustment tank 50. The final adjustment tank 50 is provided with a measuring device for measuring the Fe content in the iron-based electroplating solution P.3+ (ferric ion) concentration of Fe 3+ The final adjustment tank 50 is provided with a pH meter 51 for measuring the pH of the iron-based plating solution P in the final adjustment tank 50 .

[0040] In the final adjustment tank 50, the iron-based plating solution P from which the solid (sludge) is separated in the solid-liquid separation device 40 is adjusted to a plating solution state suitable for efficient iron-based plating. 3+ The concentration of (trivalent iron ions) is adjusted to 4.0 g / L or less, the pH of the iron-based plating solution P in the final adjustment tank 50 is adjusted to 2.0 to 2.3, and the liquid temperature of the iron-based plating solution P is adjusted to 40 to 55°C using pure water, dilute sulfuric acid, and a heater. By making the iron-based plating solution P in this liquid state, an electroplating efficiency of 70% or more can be achieved, and power-saving production can be achieved. It is further preferred to adjust the Fe content of the iron-based plating solution P to 2.0 to 2.3, and the liquid temperature of the iron-based plating solution P to 40 to 55°C. 3+ The (trivalent iron ion) concentration is adjusted to below 2.0 g / L, the pH of the iron-based plating solution P in the final adjustment tank 50 is adjusted to 2.2-2.3, and the liquid temperature of the iron-based plating solution P is adjusted to 40-45°C. At this time, a plating efficiency of more than 80% can be achieved.

[0041] Furthermore, the final adjustment tank 50 and the plating solution circulation tank 20 are preferably connected by a pipe 53 for supplying the iron-based electroplating solution P finally adjusted in the final adjustment tank 50 to the plating solution circulation tank 20 by a pump 54 .

[0042] Next, a liquid circulation method of the iron-based plating solution in the plating equipment 1 will be described.

[0043] As the iron-based plating solution P, a mixed solution of iron sulfate and sodium sulfate is mainly used. 2+ (divalent Fe ions), but the insoluble anode surface in the electroplating tank 10 inevitably produces anodization:

[0044] Fe 2+ →Fe 3+ +e - .

[0045] In addition, by stirring the iron-based plating solution P with air, air oxidation will also occur:

[0046] 2Fe 2+ +1 / 2O 2 +H 2 O→2Fe 3+ +2OH - ,

[0047] Fe in iron-based plating solution P 3+If the iron-based plating solution P is used without modification, the Fe 3+ (ferric iron) is too much, the plating electrolysis efficiency decreases. 3+ When the (trivalent iron ion) increases and the pH of the iron-based plating solution P becomes 2.4 or more, the following reaction is promoted to generate fine sludge called sodium iron alum.

[0048] 3Fe 3+ +7 / 2SO 4 2- +2OH - +1 / 2Na 2 SO 4 +4H 2 O

[0049] →NaFe3(SO 4 ) 2 (OH) 6 (Sodium iron sulfate) + 2H 2 SO 4

[0050] If the sludge is left standing, it will become coarse and cause clogging of pipes and poor appearance due to adhesion to steel plates, so it needs to be removed when it is fine. Therefore, as described in the background art, the iron-based plating solution P must be reduced before the reaction progresses.

[0051] Therefore, in the circulation method of the iron-based plating solution of the present embodiment, first, the iron-based plating solution P used in the plating tank 10 and discharged from the plating tank 10 is transferred to the plating solution circulation tank 20 via the pipe 15 .

[0052] Next, the iron-based plating solution P is sucked out by the pump 22 from the pipe 21 provided in the plating solution circulation tank 20 at a position close to the iron-based plating solution P discharged from the plating tank 10 , and is transferred to the reduction tank 30 .

[0053] Here, before the iron-based plating solution P is supplied to the reduction tank 30, the Fe 3+ 23 Determination of Fe contained in iron-based plating solution P 3+ (ferric ion) concentration.

[0054] Next, after the iron-based plating solution P is added to the reduction tank 30, the Fe 3+ The concentration of iron (trivalent iron ions) is set to a certain level. The iron source (iron powder or iron filings) used for reduction can be appropriately adjusted according to the reduction efficiency. As mentioned above, it is preferably approximately Fe 3+ (ferric iron) concentration is 1.1 to 1.3 times. 3+When the (trivalent iron ion) concentration is 4.0 g / L, it is preferred to add 4.4 to 5.2 g / L of iron source. The iron-based plating solution P in the reduction tank 30 is always stirred by the stirrer 31, and the pH of the iron-based plating solution P is always measured and monitored by the pH meter 32. As described above, the pH of the iron-based plating solution P during reduction may rise due to the addition of the iron source, which increases the sludge. Therefore, sulfuric acid is added to the reduction tank 30 in such a way as to always maintain it below 2.3. Here, there is no lower limit for the pH of the iron-based plating solution P during reduction, but as described above, from the viewpoint of reducing the pH readjustment process in the final adjustment tank 50 described later and reducing the amount of reagent adjustment, the pH is preferably above 1.0, and more preferably above 2.0. In addition, in order to make the iron-based plating solution P form a non-oxidizing state without contacting with the air, nitrogen (N 2 gas).

[0055] Next, the iron-based electroplating liquid P reduced in the reduction tank 30 is transferred to the solid-liquid separation device 40 via the pipe 33 through the pump 34. The solid-liquid separation device 40 used in this embodiment is a vertical centrifugal separation type solid-liquid separation device having the above-mentioned structure. The iron-based electroplating liquid P is put into the stock liquid supply port 45 formed on the rotating shaft 44 of the screw 43 from the pipe 33, and is supplied to the diffusion opening 48. Then, the iron-based electroplating liquid P is introduced into the screw outer cylinder 42 from the diffusion opening 48, where it is centrifugally separated into solids (sludge) and liquids by specific gravity difference. Then, the liquid is transferred from the separation water outlet 46 to the final adjustment tank 50 via the pipe 55. On the other hand, the solid (sludge) is discharged from the solid outlet 47 to the solid receiving tank 49.

[0056] Here, since the solid-liquid separation device 40 is a vertical centrifugal separation type solid-liquid separation device, as described above, even if the sludge in the iron-based electroplating solution P contains a wide range of particle sizes including 0.5 to 100 μm, the sludge can be separated and recovered at a recovery rate of more than 90%. However, even with this solid-liquid separation device 40, if the centrifugal force is increased, the fine sludge below 5 μm will not be separated, but will be brought to the cleaning liquid side, resulting in a decrease in separation efficiency. Therefore, as described above, the centrifugal force is preferably 1000 to 1800 G, and the speed difference between the screw 43 and the screw outer barrel 42 is preferably 1.0 to 2.0 rpm. When the centrifugal force is less than 1000 G, the centrifugal force is insufficient, the separation effect is small, and the separation performance is reduced. When the speed difference between the screw 43 and the screw outer barrel 42 is less than 1.0 rpm, the scraping time of the screw 43 is short, and the separation efficiency is reduced. When the speed difference exceeds 2.0 rpm, the scraping time of the screw 43 becomes longer, but the mixing of particles in the cleaning liquid increases, and as a result, the separation efficiency decreases, which is not preferred. It should be noted that since the solid-liquid separation device 40 does not require regular cleaning inside the device, it can cope with 24-hour continuous operation, and there is no need for production adjustment or interruption caused by sludge.

[0057] Next, in the final adjustment tank 50 to which the iron-based plating solution P is transferred, the iron-based plating solution P from which the solid (sludge) is separated in the solid-liquid separation device 40 is adjusted to a plating solution state suitable for efficient iron-based plating. Specifically, as described above, it is preferred that the Fe content in the iron-based plating solution P be 0.1% or 0.2%; 3+ The concentration of (trivalent iron ions) is adjusted to 4.0 g / L or less, the pH of the iron-based plating solution P in the final adjustment tank 50 is adjusted to 2.0 to 2.3, and the liquid temperature of the iron-based plating solution P is adjusted to 40 to 55°C using pure water, dilute sulfuric acid, and a heater. By making the iron-based plating solution P in this liquid state, an electroplating efficiency of 70% or more can be achieved, and power-saving production can be achieved. It is more preferable to adjust the Fe content of the iron-based plating solution P to 2.0 to 2.3, and the liquid temperature of the iron-based plating solution P to 40 to 55°C. 3+ The (trivalent iron ion) concentration is adjusted to below 2.0 g / L, the pH of the iron-based plating solution P in the final adjustment tank 50 is adjusted to 2.2-2.3, and the liquid temperature of the iron-based plating solution P is adjusted to 40-45°C. At this time, a plating efficiency of more than 80% can be achieved.

[0058] Then, the iron-based plating solution P finally adjusted in the final adjustment tank 50 is transferred to the plating solution circulation tank 20 via the pipe 53 by the pump 54 .

[0059] Finally, the iron-based plating solution P transferred to the plating solution circulation tank 20 is supplied to a plating solution nozzle head 13 of the plating tank 10 via the pipe 24 and the pipe 26 through the pump 25, and is supplied to another plating solution nozzle head 13 of the plating tank 10 via the pipe 24 and the pipe 27 through the pump 25, thereby ending the circulation of the iron-based plating solution P.

[0060] Then, in the method for producing an iron-based plating solution, circulation adjustment is performed by the circulation method of the iron-based plating solution, thereby producing the iron-based plating solution P.

[0061] It should be noted that in the electroplating tank 10, the iron-based electroplating solution P circulated and adjusted in this way is used to perform an iron-based electroplating treatment on the steel sheet S. Then, in a post-process, the steel sheet S subjected to the iron-based electroplating treatment is subjected to heating annealing, the steel sheet S after the heating annealing is subjected to hot-dip galvanizing treatment, and the galvanized steel sheet is further subjected to heating alloying, thereby manufacturing an alloyed hot-dip galvanized steel sheet.

[0062] That is, the method for manufacturing an alloyed hot-dip galvanized steel sheet includes a step of electroplating a steel sheet S using an iron-based electroplating solution manufactured by the above-mentioned method for manufacturing an iron-based electroplating solution. Then, in a post-process, the steel sheet S subjected to the iron-based electroplating treatment is subjected to heat annealing, the steel sheet S after the heat annealing is subjected to hot-dip galvanizing, and the galvanized steel sheet is further heat-alloyed, thereby manufacturing an alloyed hot-dip galvanized steel sheet.

[0063] Thus, according to the circulation method of the iron-based plating solution, the method for producing the iron-based plating solution, and the method for producing the alloyed hot-dip galvanized steel sheet of the present embodiment, the iron-based plating solution P used in the plating tank 10 is processed by at least sequentially passing through the reduction tank 30, the vertical centrifugal separation type solid-liquid separator 40, and the final adjustment tank 50, and then is put into the plating solution. Then, in the reduction tank 30, the Fe content in the iron-based plating solution P transferred to the reduction tank 30 is adjusted. 3+ (ferric ion) concentration is added into the iron source for reduction.

[0064] As a result, it is possible to produce an iron-based electroplating solution that has high electrolysis efficiency, is free of sludge mixing, is stable, and can save electricity without requiring huge equipment.

[0065] In addition, according to the circulation method of the iron-based plating solution, the method for producing the iron-based plating solution, and the method for producing the alloyed hot-dip galvanized steel sheet of the present embodiment, sulfuric acid is added to the reduction tank 30 so that the pH of the iron-based plating solution P in the reduction tank 30 is maintained at 2.3 or less. This can avoid the possibility of an increase in sludge due to an increase in the pH of the iron-based plating solution P caused by the addition of the iron source.

[0066] In addition, according to the iron-based plating solution circulation method, the iron-based plating solution manufacturing method, and the alloyed hot-dip galvanized steel sheet manufacturing method of the present embodiment, nitrogen gas is sealed in the reduction tank 30. Thus, the iron-based plating solution P in the reduction tank 30 can be made into a non-oxidized state without contacting with air.

[0067] In addition, according to the circulation method of the iron-based plating solution, the manufacturing method of the iron-based plating solution, and the manufacturing method of the alloyed hot-dip galvanized steel sheet of the present embodiment, the vertical centrifugal separation type solid-liquid separation device 40 is provided with a screw outer cylinder 42 that rotates differentially with each other and a screw 43 disposed in the screw outer cylinder 42 so that the solid and liquid of the stock solution are centrifugally separated by specific gravity difference. Moreover, the rotating shaft 44 of the screw 43 is formed into a cylindrical shape so that the stock solution is led out from the screw 43 into the screw outer cylinder 42, and a diffusion opening 48 is formed on the side of the rotating shaft 44. Thus, the iron-based plating solution P moved to the solid-liquid separation device 40 is supplied from the rotating shaft 44 of the screw 43 to the diffusion opening 48, and is introduced into the screw outer cylinder 42 from the diffusion opening 48. Then, in the screw outer cylinder 42, it is centrifugally separated into solid (sludge) and liquid by specific gravity difference. Therefore, even if the sludge has a wide range of particle sizes including 0.5 to 100 μm, which is contained in the iron-based electroplating solution P, the sludge can be separated and recovered at a recovery rate of 90% or more.

[0068] In addition, according to the circulation method of the iron-based plating solution, the method for producing the iron-based plating solution, and the method for producing the alloyed hot-dip galvanized steel sheet of the present embodiment, in the final adjustment tank 50, the Fe 3+The concentration of (trivalent iron ions) is adjusted to 2.0 g / L or less, the pH of the iron-based electroplating solution P is adjusted to 2.0 to 2.3, and the liquid temperature of the iron-based electroplating solution P is adjusted to 40 to 55° C. by using sulfuric acid and pure water. Thus, by making the iron-based electroplating solution P in this liquid state, it is possible to achieve an electroplating efficiency of 70% or more, and realize power-saving production.

[0069] In addition, by using the iron-based plating solution P that has been circulated and adjusted by the circulation method of the iron-based plating solution of this embodiment to perform iron-based plating treatment, the plated appearance of the alloyed hot-dip galvanized steel sheet produced can be free of sludge marks and be beautiful.

[0070] Although the embodiments of the present invention have been described above, the present invention is not limited thereto, and various changes and improvements can be made.

[0071] For example, sulfuric acid does not necessarily need to be added to the reduction tank 30 so that the pH of the iron-based plating solution P in the reduction tank 30 is maintained at 2.0 to 2.3.

[0072] In addition, it is not necessarily necessary to seal nitrogen gas in the reduction tank 30 .

[0073] In the final adjustment tank 50, it is not necessary to remove Fe 3+ The (ferric ion) concentration was adjusted to 2.0 g / L or less.

[0074] In addition, in the final adjustment tank 50, the pH of the iron-based plating solution P does not necessarily need to be adjusted to 2.0 to 2.3.

[0075] Furthermore, in the final adjustment tank 50, the liquid temperature of the iron-based plating solution P does not necessarily need to be adjusted to 40 to 55°C.

[0076] In addition, although the iron-based plating solution P used in the electroplating tank 10 is processed in sequence through the plating solution circulation tank 20, the reduction tank 30, the vertical centrifugal separation type solid-liquid separation device 40 and the final adjustment tank 50 and then put into the electroplating tank 10, it does not necessarily need to pass through the plating solution circulation tank 20.

[0077] Example

[0078] In order to verify the effect of the present invention, the electrical power consumption rate (kWh / T), electrolysis efficiency (%), and appearance of the alloyed hot-dip galvanized steel sheet of the product were investigated for Comparative Examples 1 to 3 and Examples 1 to 5. The alloyed hot-dip galvanized steel sheet is manufactured by subjecting the steel sheet to an iron-based electroplating treatment, then heating and annealing the steel sheet subjected to the iron-based electroplating treatment in a post-process, subjecting the steel sheet subjected to the heat-annealing treatment to a hot-dip galvanizing treatment, and further heat-alloying the galvanized steel sheet.

[0079] In Examples 1 to 5, the use and Figure 1 The electroplating apparatus 1 of the structure shown is the same as the electroplating apparatus.

[0080] In Comparative Examples 1 to 3, the plating tank, plating solution circulation tank, and final adjustment tank were the same as those in Examples 1 to 5, and the reduction tank was the reduction tank used in Patent Document 4 (the surface area Sm of the iron powder filled in the reduction tank was 2.37 m / s). 2 The amount of plating solution circulating to the reduction tank Qm 3 / hr ratio H (= S / Q) is 1≤H≤5). In Comparative Example 1, as a solid-liquid separation device, a sedimentation type sludge settling tank similar to that used in Patent Document 5 was used. In Comparative Examples 2 and 3, as a solid-liquid separation device, a horizontal centrifugal separation device similar to that used in Patent Document 6 was used.

[0081] For the electroplating tanks in Examples 1 to 5 and Comparative Examples 1 to 3, the length of the electrode in one tank in the long side direction is 2 m, the distance between the steel plate and the electrode is 30 mm on one side, and two tanks are connected. The iron-based electroplating solution (plating bath) is a sulfuric acid bath, and its composition includes 55 to 65 g / L of iron and 5 to 7 g / L of sodium.

[0082] The results of the investigation on the specific power consumption (kWh / T), electrolysis efficiency (%), and appearance of the galvannealed steel sheet of the product are shown in Table 1. The "appearance after plating" in Table 1 refers to the appearance of the galvannealed steel sheet of the product.

[0083] [Table 1]

[0084]

[0085] For Comparative Examples 1 to 3, in the reduction tank, there was no 3+ (ferric iron) concentration into the iron source. Therefore, it is not possible to fully reduce Fe 3+ (Trivalent iron) concentration (In the final adjustment tank of Comparative Examples 1 to 3, since Fe 3+ (ferric iron) concentration, so Fe 3+ (ferric iron) concentration is 5.5 g / L or more), and the electrolysis efficiency (%) is 54% or less, which is relatively low. In addition, the unit power consumption (kWh / T) is also 112 kWh / T or more, which is relatively high. In addition, since a sedimentation or horizontal centrifugal separation device is used as a solid-liquid separation device, the sludge cannot be completely removed, and traces of sludge remain on the appearance of the alloyed hot-dip galvanized steel sheet of the product.

[0086] On the other hand, in Examples 1 to 5, the Fe3+ (ferric iron) concentration into the iron source. Therefore, it is possible to fully reduce the Fe 3+ (Trivalent iron) concentration (in the final adjustment tank of Examples 1 to 5, since Fe 3+ (ferric iron) concentration, therefore, Fe 3+ (ferric iron ion) concentration is below 3.8g / L), and the electrolysis efficiency (%) is as high as 71% or more. In addition, the unit power consumption (kWh / T) is also below 66kWh / T, which is relatively low. In addition, since a vertical centrifugal separation type is used as a solid-liquid separation device, sludge can be fully removed, and the appearance of the alloyed hot-dip galvanized steel sheet of the product is beautiful.

[0087] It should be noted that the appearance of the products in Table 1 after plating was observed on the surface of the products (surface area 10m 2 ), the case where more than 50 sludge traces are found is set as "many sludge traces", the case where more than 10 but less than 50 sludge traces are found is set as "few sludge traces", and the case where less than 10 sludge traces are found is set as "beautiful".

[0088] Explanation of symbols

[0089] 1Electroplating equipment

[0090] 10 electroplating tanks

[0091] 11 Processing tank

[0092] 12 Anode electrode

[0093] 13 Plating liquid nozzle head

[0094] 14 Power roller

[0095] 15 piping

[0096] 20 plating solution circulation tank

[0097] 21Piping

[0098] 22 Pumps

[0099] 23Fe 3+ count

[0100] 24 piping

[0101] 25 pumps

[0102] 26 piping

[0103] 27Piping

[0104] 30 Restore tank

[0105] 31. Blender

[0106] 32PH meter

[0107] 33Piping

[0108] 34 Pumps

[0109] 40Solid-liquid separation device

[0110] 41 Centrifugal Separation Cylinder

[0111] 42 screw outer barrel

[0112] 43 screw

[0113] 44 Rotation axis

[0114] 45 stock solution supply port

[0115] 46 Separation water outlet

[0116] 47 Solids discharge port

[0117] 48 diffusion opening

[0118] 49 solid receiving tank

[0119] 50 Final Adjustment Slots

[0120] 51PH meter

[0121] 52Fe 3+ count

[0122] 53Piping

[0123] 54 Pumps

[0124] 55 piping

[0125] P Iron-based Plating Solution

Claims

1. A method for circulating an iron-based electroplating solution, characterized in that: The iron plating solution used in the iron plating tank is circulated and adjusted. The iron-based plating solution used in the plating tank is processed by at least passing through a reduction tank and a vertical centrifugal separation type solid-liquid separation device in sequence, and then put into the plating tank. In the reduction tank, the Fe 3+ That is, the concentration of ferric ions is the iron source used for reduction.

2. The method for circulating an iron-based electroplating solution according to claim 1, characterized in that: Sulfuric acid is added to the reduction tank so that the pH of the iron-based electroplating solution in the reduction tank is maintained at 2.3 or less.

3. The method for circulating an iron-based electroplating solution according to claim 1 or 2, characterized in that: Nitrogen is sealed in the reduction tank.

4. The method for circulating an iron-based electroplating solution according to any one of claims 1 to 3, characterized in that: The vertical centrifugal separation type solid-liquid separation device comprises a screw outer barrel that rotates differentially with each other and a screw arranged in the screw outer barrel so as to centrifugally separate the solid and liquid of the stock solution by the specific gravity difference. The rotating shaft of the screw is formed into a cylindrical shape so that the raw liquid can be guided from the screw into the screw outer cylinder, and a diffusion opening is formed on the side surface of the rotating shaft.

5. The method for circulating an iron-based electroplating solution according to any one of claims 1 to 4, characterized in that: The iron-based plating solution is treated by the vertical centrifugal separation type solid-liquid separator and then passed through a final adjustment tank. In the final adjustment tank, the Fe 3+ That is, the concentration of trivalent iron ions is adjusted to 4.0 g / L or less.

6. The method for circulating an iron-based electroplating solution according to claim 5, characterized in that: In the final adjustment tank, the pH of the iron-based plating solution is adjusted to 2.0 to 2.

3.

7. The method for circulating an iron-based electroplating solution according to claim 5 or 6, characterized in that: In the final adjustment tank, the temperature of the iron-based plating solution is adjusted to 40 to 55°C.

8. The method for circulating an iron-based electroplating solution according to any one of claims 1 to 4, characterized in that: The iron-based plating solution is treated by the vertical centrifugal separation type solid-liquid separator and then passed through a final adjustment tank. In the final adjustment tank, sulfuric acid and pure water are used to adjust the iron-based plating solution so that Fe 3+ That is, the concentration of trivalent iron ions is below 2.0 g / L, the pH of the iron-based electroplating solution is 2.0 to 2.3, and the liquid temperature of the iron-based electroplating solution is 40 to 55°C.

9. A method for producing an iron-based electroplating solution, characterized in that: The iron-based electroplating solution is produced by performing circulation adjustment using the circulation method for an iron-based electroplating solution according to any one of claims 1 to 8.

10. A method for manufacturing an alloyed hot-dip galvanized steel sheet, characterized in that: The method comprises the step of subjecting a steel sheet to an iron-based electroplating treatment using the iron-based electroplating solution produced by the method for producing an iron-based electroplating solution according to claim 9.