Laminated cured body, printed wiring board provided with same, and method for producing laminated cured body
By adopting a stacked cured body structure and multiple exposure development treatment on the printed circuit board, the problem of difficult ultraviolet light in the thick film of the photocurable resin composition is solved, and better adhesion and connection stability are achieved, thereby improving the The overall performance of the circuit board.
Patent Information
- Application Number
- CN202380030729.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-31
- Publication Date
- 2024-11-22
AI Technical Summary
Prior Art When using a photocurable resin composition to make thick films, ultraviolet light is difficult to reach the bottom of the resin layer sufficiently, resulting in undercutting and poor adhesion, especially when the colorant is included, which affects the circuit board. performance and connection stability.
A laminated cured body structure is adopted, in which the lower cured film and the upper cured film are cured by light and form a concave joint surface to ensure that ultraviolet light spreads throughout the film thickness, and through multiple exposure and development treatments, undercut is suppressed and adhesion is improved.
It effectively suppresses the undercut phenomenon, improves the adhesion of the printed circuit board and the connection stability of the conductor circuit and the mounting components, improves the photocuring reaction of the film thickness, and enhances heat and chemical resistance.
Smart Images

Figure CN119014133A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a laminated cured body used as an etching resist layer of a printed wiring board, a printed wiring board having the laminated cured body, and a method for producing the laminated cured body. Background Art
[0002] Generally, in the manufacture of printed circuit boards, a photocurable resin composition is used as an anti-etching agent for protecting the circuit pattern in the pre-process of mounting components such as LED elements on the circuit substrate. For example, Patent Document 1 describes the following scheme: a solder resist formed of a photocurable resin composition is applied to a substrate, the solder resist is cured by ultraviolet rays, and then the unexposed portion of the solder resist is developed. Thus, a circuit protection pattern based on the solder resist is formed. Various components are mounted on the substrate manufactured in this way to complete the printed circuit board.
[0003] On the other hand, in recent years, in order to improve the performance of electronic devices, the demand for thick copper substrates that can flow large amounts of power in small spaces has increased. In addition, in order to obtain thick copper substrates, the film thickness of the cured body of the photocurable resin composition needs to be thicker than before. Specifically, the film thickness of the cured body of the photocurable resin composition must be 40 μm to 500 μm.
[0004] In order to maximize the performance of electronic equipment, it is also important to improve the connection stability between the conductor circuit and the mounted components.
[0005] In the case of forming a cured body with a thick film thickness from a photocurable resin composition, when the resin layer formed by coating the photocurable resin composition on the substrate and drying is exposed, the ultraviolet light does not fully reach the bottom of the resin layer, so the photocuring reaction at the bottom of the resin layer is not fully carried out, and the resin layer that should have remained in the subsequent development process is removed, and it becomes easy to produce undercuts in which the bottom becomes thinner than the surface layer. In such a case, sometimes the adhesion between the resin layer and the substrate cannot be fully obtained. In particular, in display applications, for a photocurable resin composition containing a white colorant or a black colorant that can also be used as a reflective material or a light shielding agent, in order to improve reflectivity or light shielding, when a cured body is formed, as described above, the film thickness is sometimes made thicker than before by 40μm to 500μm. In such a case, in a photocurable resin composition containing these colorants, it becomes difficult for ultraviolet light to further reach the bottom of the resin layer, so it is easy to produce undercuts and it becomes difficult to fully obtain adhesion, so this concern should be eliminated in advance.
[0006] In this regard, Patent Document 1 discloses the following technology: in the exposure process, ultraviolet light is selectively diffused through a mask film having a mask pattern and a light diffusion film laminated and bonded thereunder, thereby enabling the black solder resist layer to be well cured. However, in the method disclosed in Patent Document 1, ultraviolet light is diffused to form a protective exposure portion that does not need to be exposed, so the protective exposure portion will remain during development, and there is a concern that the solder resist layer pattern of the target shape cannot be obtained.
[0007] Furthermore, the solder resist cured product of Patent Document 1 does not particularly contribute to improving the connection stability between the conductor circuit and the mounted component.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2012-199351 Summary of the invention
[0011] Problem that the invention aims to solve
[0012] In view of the above-mentioned problems of the prior art, the object of the present invention is to provide: a laminated cured body in which, when a cured body having a thick film thickness is formed from a photocurable resin composition, the curing is also good at the bottom, so that undercut formation is suppressed and the adhesion to the substrate is improved; a printed circuit board having the same; and a method for manufacturing a laminated cured body.
[0013] Solutions for solving problems
[0014] The present inventors have conducted intensive research and found that the above-mentioned object of the present invention can be solved by a laminated cured body, wherein the laminated cured body is used as an anti-etching layer of a printed circuit board, and the laminated cured body has:
[0015] a lower cured film which is laminated on any one of the surfaces of the printed circuit board and is formed of a photocurable resin composition which is photocured; and,
[0016] one or more upper cured films, which are laminated on the lower cured film and are formed from a photocurable resin composition which is separately photocured,
[0017] The end surface of each cured film cured by stacking has one or more recessed portions extending in the peripheral direction along the bonding surface between the lower cured film and the upper cured film or along the bonding surfaces of a plurality of upper cured films.
[0018] The laminated cured body of the present invention is preferably laminated so as to surround a conductor portion provided on a printed wiring board, and the recessed portion is formed along the inner peripheral surface of the laminated cured body.
[0019] The laminated cured body of the present invention is preferably laminated so as to face each other on both sides of a conductor portion laminated on a substrate, and the recessed portions are formed in the end surfaces facing each other.
[0020] In addition, the object of the present invention is achieved by a printed wiring board comprising a laminated cured body.
[0021] Furthermore, the object of the present invention is achieved by a method for producing a laminated cured body, the method for producing a laminated cured body being characterized in that it is a method for producing a laminated cured body used as an anti-etching layer of a printed circuit board, the method comprising the following steps:
[0022] (1) a step of forming an uncured film of a lower layer, wherein a photocurable resin composition is applied to any one of the surfaces of a printed circuit board and dried to form an uncured film of a lower layer;
[0023] (2) a lower cured film forming step of exposing and curing the lower uncured film;
[0024] (3) an upper uncured film forming step of coating the upper surface of the lower cured film with a photocurable resin composition which is the same as or different from the photocurable resin composition and drying the composition to form an upper uncured film; and,
[0025] (4) An upper cured film forming step of exposing and curing the upper uncured film.
[0026] The manufacturing method of the present invention preferably further comprises the following step after the one or more steps of forming an upper uncured film and forming an upper cured film:
[0027] (5) a development step of applying a development treatment to the laminated lower cured film and upper cured film; and,
[0028] (6) A thermal curing step of thermally curing the laminated lower layer cured film and upper layer cured film after development.
[0029] The photocurable resin composition used in the production method of the present invention preferably contains (A) a carboxyl group-containing resin, (B) a photopolymerization initiator, (C) an epoxy resin, (D) a colorant, and (E) a photopolymerizable compound.
[0030] The colorant (D) used in the production method of the present invention contains a white colorant, and the amount of the white colorant blended is preferably 50 to 500 parts by mass, more preferably 100 to 450 parts by mass, based on 100 parts by mass of the carboxyl group-containing resin (A).
[0031] The colorant (D) used in the production method of the present invention contains a black colorant, and the amount of the black colorant blended is preferably 1 to 50 parts by mass based on 100 parts by mass of the carboxyl group-containing resin (A).
[0032] Effects of the Invention
[0033] The stacked cured body of the present invention is well cured as a whole, which is formed by the lower cured film and the upper cured film. Therefore, the occurrence of undercut at the bottom of the cured body is suppressed, and the stacked cured body has excellent adhesion to the substrate. The stacked cured body having a concave portion at the end can improve the connection stability of the components through the anchoring effect.
[0034] In addition, according to the manufacturing method of the present invention, a laminated cured body having the above-mentioned effects can be manufactured smoothly and reliably. Furthermore, the printed wiring board of the present invention has excellent connection stability of mounted components by using the laminated cured body of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is a schematic cross-sectional view of a printed wiring board for explaining a state where a laminated cured body according to one embodiment of the present invention is laminated.
[0036] Figure 2 To show Figure 1 An illustration of a printed circuit board with components mounted thereon.
[0037] Figure 3 for Figure 1 Schematic top view of a printed circuit board.
[0038] Figure 4 This is a schematic cross-sectional view of a laminated solid body according to one embodiment of the present invention.
[0039] Figure 5 It is a schematic diagram for explaining the shape of a laminated solid body according to one embodiment of the present invention.
[0040] Figure 6 This is a schematic enlarged cross-sectional view of a laminated solid body according to one embodiment of the present invention.
[0041] Figure 7 This is a schematic cross-sectional view of a laminated cured body obtained in Comparative Example 1 (only one exposure). DETAILED DESCRIPTION
[0042] The laminated cured body of the present invention is used as an anti-etching layer of a printed circuit board, and comprises: a lower cured film laminated on any one of the surfaces of the printed circuit board and formed of a photocurable resin composition that has been photocured; and one or more upper cured films laminated on the lower cured film and formed of a photocurable resin composition that has been photocured separately. The end faces of each laminated and cured cured film have one or more recessed portions extending in the peripheral direction along the bonding surface between the lower cured film and the upper cured film, or along the bonding surface of a plurality of upper cured films.
[0043] It should be noted that, in the present invention, the lower layer refers to a layer that is in contact with and stacked on the substrate, and the upper layer refers to a layer that is isolated and stacked from the upper surface of the lower layer, that is, the substrate. In the case where there are multiple layers on the upper surface of the lower layer, the multiple layers are respectively referred to as upper layers. The upper layer farthest from the substrate is also referred to as the uppermost layer, and the upper layer between the lower layer and the uppermost layer is also referred to as the intermediate layer.
[0044] Hereinafter, the laminated cured body of the present invention will be described with reference to the drawings.
[0045] Figure 1 It is a schematic cross-sectional view of a printed circuit board 10 in which a laminated cured body 3 of the present invention is laminated on a circuit substrate 1. A copper-based conductor circuit is drawn on the surface of the circuit substrate 1, and the laminated cured body 3 covers the periphery 5a of a conductor portion 5 which is a part of the conductor circuit so as to surround it.
[0046] Figure 2 To show Figure 1 FIG. 1 is an explanatory diagram of a state where components are mounted on a printed circuit board 10 . Figure 2 Shown in Figure 1 The illustrated laminated solid body 3 has solder 9 attached to the opening 7 , whereby components 11 such as LEDs are mounted.
[0047] Figure 3 for Figure 1 FIG. 1 is a schematic top view of a printed circuit board 10 . Figure 3 In the figure, a copper conductor portion 5 (hereinafter also referred to as copper 5) is drawn in a circular shape on the circuit board 1, and the laminated solid body covers and surrounds the periphery 5a of the copper 5 (the area surrounded by the solid line and the dotted line in the same figure).
[0048] It should be noted that Figure 3 In the description, the application of the circular conductor part to the laminated solid body is described, but the shape of the conductor part is not particularly limited as long as it can be used for patterning of the circuit substrate in a square, rectangular, elliptical, linear, etc. Figure 3In the embodiment, the laminated solid body surrounds the conductor part to ensure the periphery, but the conductor part does not need to be completely surrounded by the laminated solid body, and the connection part between the conductor part and other circuits may also have a part not surrounded by the laminated solid body. Figure 3 , the laminated solid body is shown covering a portion of the conductor portion when viewed from the upper surface.
[0049] The laminated cured body of the present invention is a laminated cured body based on a plurality of cured films of two or more layers as described below in relation to its manufacturing method. After the uncured lower film formed of the photocurable resin composition is cured by exposure, an uncured upper film formed of the photocurable resin composition is formed on the obtained lower cured film, and then further exposed. Therefore, the irradiated light reaches all the way to the bottom of each layer, and the entire coating is well cured even when the film thickness is thick. For this reason, when the laminated cured body after photocuring is developed, the occurrence of undercut at the bottom of the laminated cured body is suppressed, and the area of the bottom surface of the laminated cured body is fully ensured, so that the laminated cured body has excellent adhesion to the substrate.
[0050] When the laminated cured body of the present invention is laminated so as to surround a conductor portion provided on a substrate, it is preferred that a portion of the end surface thereof corresponding to the inner periphery of the bonding surface between the lower and upper cured films has a recess extending in the peripheral direction.
[0051] Figure 1 In the example shown, the conductor portions 5 shown at two locations are both surrounded by the laminated cured body 3. On the end surface of the laminated cured body 3, along the junction surface between the upper surface of the lower layer cured film 3A and the lower surface of the upper layer cured film 3B, a recessed portion 3C extending in the peripheral direction of the laminated cured body 3 is formed. When the upper layer cured film is made of two or more layers, the recessed portions 3C are formed at a plurality of positions on the end surface of the laminated cured body 3 corresponding to the junction between the respective cured films.
[0052] According to this structure, when installing components near or in contact with the stacked solid body 3, the solder used penetrates into one or more recesses 3C, and when the solder is fixed, an anchoring effect is generated between the solid body having the recess and the fixed solder. Figure 1 In a printed wiring board having a laminated cured body in a form, the connection stability between the printed wiring board and the mounted component is improved.
[0053] Figure 4A schematic partial cross-sectional view for illustrating one embodiment of the stacked cured body 3 is shown in the figure. The stacked cured body 3 is composed of a lower cured film 3A and an upper cured film 3B formed thereon. The lower cured film 3A may be formed by applying a photocurable resin composition on the circuit substrate 1, drying it, and exposing it to the light, or may be formed by pre-manufacturing a dry film of a photocurable resin composition, forming an uncured film on the circuit substrate 1 with the dry film, and curing it by exposure. Similarly, the upper cured film 3B may be formed by applying a photocurable resin composition on the upper surface of the lower cured film 3A, drying it, and exposing it to the light, or may be formed by pre-manufacturing a dry film of a photocurable resin composition, providing an uncured film on the lower cured film 3A with the dry film, and curing it by exposure. After exposure, the upper cured film 3B is subjected to at least a developing step, and more preferably further subjected to a thermal curing step, to become Figure 4 The shape of the partial cross-sectional view.
[0054] In this embodiment, the ends of the lower layer cured film 3A and the upper layer cured film 3B are formed into a shape that bulges in the extension direction of the cured film. The cross-sectional shape of the bulging portion of the end is as follows: Figure 4 As shown, a roughly arc shape can be formed. Figure 4 In the embodiment, the end faces 3Aa and 3Ba of the lower layer solidified film 3A and the upper layer solidified film 3B are bulged outward or have the largest diameter at the thickness positions 3Ad and 3Bd which are approximately half of the film thickness 3Ab and 3Bb (3Ab1=3Ab2, 3Bb1=3Bb2), respectively, so as to be configured to have an arc-shaped cross section. The bulged out portion of the end faces 3Aa and 3Ba may be above or below the thickness positions 3Ad and 3Bd. Furthermore, the upper surface ( Figure 4 , corresponding to the upper end of the arc-shaped end portion 3Aa) and the lower surface of the cured film 3B connected thereto ( Figure 4 A recessed portion 3C is formed around the bonding surface (end surface) corresponding to the lower end of the arc-shaped end portion 3Ba, that is, around a portion or the entirety of the stacked solid body 3.
[0055] The cross-sectional shape of the bulge at the end 3Aa of the lower cured film 3A and the end 3Ba of the upper cured film 3B may be a shape other than the above-mentioned substantially circular arc shape, for example, a sharp-edged shape, or may be asymmetrical. Figure 5 That kind of trapezoidal bulge.
[0056] There is no restriction on the film thickness 3Ab and 3Bb of the lower cured film 3A and the upper cured film 3B, and they are usually set to 10 to 40 μm, and in particular, 20 to 30 μm. By setting it to 10 μm or more, halation during exposure can be suppressed, and by setting it to 40 μm or less, undercutting can be suppressed, and the effect of the present invention can be obtained more effectively. In addition, the film thickness of the lower cured film 3A and the upper cured film 3B can be different from each other. In addition, the film thickness of the entire laminated cured body can be selected according to the laminated position of the laminated cured body on the printed circuit board. For the laminated cured body of the present invention, when the overall film thickness is thicker, for example, when the overall film thickness exceeds 40 μm, the photocuring reaction is fully carried out until the bottom of the resin layer, so undercutting can be suppressed. By appropriately selecting the film thickness of the lower cured film 3A and the upper cured film 3B and the film thickness of the entire laminated cured body, the position (height) of the various recessed portions 3C relative to the height of the entire laminated cured body 3 is determined. It should be noted that in the present invention, the film thickness refers to the average film thickness.
[0057] The position of the recessed portion 3C in the laminated solid body 3 is preferably the bottom surface of the laminated solid body 3 (bottom surface 3A of the cured film 3A). bottom ) and the upper surface of the laminated solidified body 3 (the upper surface 3B of the solidified film 3B) top For example, it is preferred that the bottom surface 3A bottom 5μm or more higher than the upper surface 3B top A concave portion is formed at a position lower than 5 μm.
[0058] Figure 6 A schematic enlarged cross-sectional view of a laminated solid body according to one embodiment of the present invention is shown in FIG. Figure 6 With Figure 2 Similarly, a laminated cured body 3 composed of a lower cured film 3A and an upper cured film 3B disposed thereon is laminated on the circuit board 1. Figure 6 In, if used Figure 3 As described above, the laminated solid body 3 is laminated so as to surround the conductor portion 5 .
[0059] Figure 2 In the embodiment, the solder 9 is in the state of a solder ball which has not yet melted, but Figure 6 , the solder 9 is molten by the heating of the reflow process and penetrates into the recess 3C. In this state, if the temperature is lowered, the solder 9 is fixed in the recess 3C of the laminated solid body 3, thereby improving the bonding state of the solder 9 and the laminated solid body 3, so-called anchoring effect. As a result, the component 11 mounted by the solder 9 is stably bonded to the circuit board 1, so the reliability of the electronic component obtained thereby is improved.
[0060] Hereinafter, an example of setting the positions at which recessed portions are formed in the stacked structure will be described.
[0061] like Figure 5 As shown, the laminated cured body 300 is formed of a lower cured film 300A and an upper cured film 300B, and a concave portion 300C is formed on the bonding surface of the lower cured film 300A and the upper cured film 300B in a manner that satisfies the following conditions. Figure 5 As shown, from the upper surface 300B of the stacked cured body 300 top Also low distance t t Position P1 to bottom surface 300A bottom Also high distance t b Position P m Between, determine the position P1 and the ratio position P1 for each distance t n (e.g. 5 μm) at each position (height) P n (Not shown in the picture. Figure 5 In the equation, it is equivalent to the distance t n Next, at position P n The width W of the stacked solid body 300 is measured. n ( Figure 5 Then, the two widths W corresponding to the adjacent positions (heights) are compared. n With W n+1 (For example, W6 and W7). The width of the concave portion 300C (W upper ) is larger than the width below (W lower ) is still narrow (W upper <W lower ) is formed in at least one or more ways. Figure 5 In the embodiment, the width W6 is narrower than the width W7, and therefore a recess 300C is formed between W6 and W7.
[0062] It should be noted that, in this embodiment, the upper surface 300B is listed top and bottom surface 300A bottom All are horizontal planes, with widths W1, W2 and W1 being equal. n Also with 300B top and bottom surface 300A bottom The case of parallel and horizontal surfaces is taken as an example. The film surface of the laminated solid body is not smooth, and the upper surface 30B top If the upper surface 300B is not horizontal, top The point with the largest film thickness is used as the reference to determine the position P1, and the W n comparison.
[0063] In addition, the distance t b ,tt All are 5μm.
[0064] It should be noted that the above Figure 5 The cross-sectional shape shown is formed, for example, in Figure 3 That is, between any two adjacent conductor parts 5, usually as Figure 5 As shown in the laminated solid body, the two end faces have a substantially symmetrical cross-sectional shape. Figure 3 around the conductor portion 5.
[0065] On the other hand, a laminated solidified body such as Figure 3 The periphery of the upper right conductor portion 5 extends over the area where the conductor portion on the printed circuit board 10 does not exist (for example, more than Figure 3 (Partial Figure) The outer area of the outer periphery) is formed, and the end face on the conductor part 5 side and the other end face in the cross-sectional shape may not necessarily have a symmetrical shape. In this case, the other end face may be uncertain or an indefinite shape that cannot be formed as a reference, and a uniform width W is also assumed. n In this case, Figure 5 Position P n , will be 300A from the bottom bottom To the upper surface 300B of the stacked solid body 300 top The arbitrary perpendicular line drawn is used as a reference line segment, and the distance between one end of the stacked solid body 300 and the reference line segment is taken as the distance W n , respectively find out the n The corresponding distance W n , and W is performed in the same manner as above. n By comparing the above data, the position of the recess 300C is determined.
[0066] In addition, as described above, the laminated solidified body of the present invention may include, in addition to the above-mentioned upper solidified film, a second, third, etc., further upper solidified film sequentially laminated thereon, and the number of layers of the solidified film in the laminated solidified body is usually set to 2 to 10, preferably 2 or 3. In addition, in the laminated solidified body, a recessed portion can be formed along the bonding surface of two adjacent layers of solidified film, and therefore, the number of recessed portions is set to be one layer less than the number of layers of the solidified film.
[0067] [Method for producing laminated cured body]
[0068] The laminated cured body of the present invention is produced by the following production method, which includes the following steps:
[0069] (1) a step of forming an uncured film of a lower layer (step (1)), wherein a photocurable resin composition is applied to any one of the surfaces of a printed wiring board and dried to form an uncured film of a lower layer;
[0070] (2) a lower cured film forming step (step (2)) of exposing and curing the lower uncured film;
[0071] (3) a step of forming an upper uncured film (step (3)), wherein a photocurable resin composition which is the same as or different from the photocurable resin composition is applied to the upper surface of the lower cured film and dried to form an upper uncured film; and,
[0072] (4) Upper layer cured film forming step (step (4)): the upper layer uncured film is exposed to light and cured.
[0073] Furthermore, the manufacturing method of the present invention preferably includes the following steps after the above-mentioned one or more upper uncured film forming steps and upper cured film forming steps: (5) a developing step of applying a developing treatment to the stacked lower cured film and upper cured film; and, (6) a thermal curing step of thermally curing the stacked lower cured film and upper cured film after development.
[0074] In the above, if the combination of step (3) and step (4) is performed once, a laminated cured body consisting of two layers, namely, the lower cured film 3A and the upper cured film 3B thereon, is formed. If the combination of step (3) and step (4) is performed two or more times, a laminated cured body consisting of a total of three or more layers, namely, the lower cured film 3A and two or more upper cured films 3B sequentially formed thereon, is manufactured.
[0075] In the present invention, it is preferred that after the upper layer (uppermost layer) is cured, a step (step (5)) of applying a development treatment to the laminated lower layer cured film and upper layer cured film is performed. Step (5) is a step of exposing and treating the entire cured film with a developer. Depending on the circumstances, a part of the lower layer or the upper layer may be developed in advance before the step. However, after the entire uncured film is exposed to form a cured film, the unexposed part is simultaneously subjected to a development treatment, and the development treatment is not performed before that, thereby simplifying and smoothing the processing process.
[0076] In the present invention, it is preferred to perform a step of thermally curing the laminated lower cured film and upper cured film after development (step (6)). Step (6) is a step of further heating the laminated cured body of the present invention obtained after development to a temperature of about 100 to 180° C. and thermally curing (post-curing). By performing the heat treatment, the heat resistance, chemical resistance, moisture absorption resistance, adhesion, electrical properties, etc. of the cured product are improved.
[0077] In any case, in the production method of the present invention, after curing the uncured film, an upper uncured film is provided thereon and separately exposed, thereby obtaining a laminated cured body in which both the lower and upper cured films are in a well-cured state.
[0078] Steps (1) to (6) are described in further detail.
[0079] [Process (1)]
[0080] In the method for producing a laminated cured body of the present invention, as step (1), a photocurable resin composition is used to form an uncured film of a lower layer, for example, on a circuit board 1. As the photocurable resin composition, any one commonly used in the production of solder resist layers can be used without particular limitation.
[0081] In step (1), the photocurable resin composition is applied to a circuit substrate or the like by a method such as screen printing, curtain coating, spray coating, or roller coating, and the organic solvent contained in the composition is volatilized and dried at a temperature of, for example, 70 to 90° C., thereby forming an uncured film of the lower layer. Alternatively, a dry film of the photocurable resin composition is prepared in advance, and the uncured film can be formed on the circuit substrate using the dry film. The uncured film of the lower layer thus obtained is dried using a drying device such as a hot air circulation drying furnace, for example, at a temperature in the range of 60° C. to 90° C. for 10 to 30 minutes, and after drying, an uncured film having a film thickness of about 10 to 40 μm is formed.
[0082] [Step (2)]
[0083] In step (2), a photomask having a predetermined pattern is provided on the upper surface of the uncured film of the lower layer obtained in step (1), and active energy rays (light amount: 100 to 1000 mJ / cm 2 ), or directly depicted by irradiation with active energy rays, thereby exposing. As the photocurable resin composition of the present invention, the type in which the exposed part is cured is generally used. After step (2), the unexposed part can also be developed using an alkaline aqueous solution to form a pattern film, but as described later, it is preferred to omit development at this stage. At this time, from the perspective of the accuracy of the alignment of the formed pattern, it is preferred to use a direct exposure machine. In addition, as the irradiation light source of the active energy ray, a low-pressure mercury lamp, a medium-pressure mercury lamp, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, an LED, a xenon lamp or a metal halide lamp can be used.
[0084] [Step (3)]
[0085] In step (3), an upper uncured film formed of a photocurable resin composition is further formed on the upper surface of the lower cured film obtained in step (2). The photocurable resin composition used here may be the same as or different from the photocurable resin composition of step (1), and may be applied to the upper surface of the lower cured film (the opposite side of substrate 1), or may be formed into a dry film and then laminated. The laminate formed by the lower cured film and the upper uncured film thus obtained is dried to form a dry coating. The drying conditions may be the same as or different from those of step (1).
[0086] [Step (4)]
[0087] In step (4), the upper surface of the uncured film of the upper layer of the laminate is exposed in the same manner as in step (2). The conditions for exposure may be the same as or different from those in step (2).
[0088] Thus, a laminated cured body having two layers of cured films was obtained.
[0089] Furthermore, the laminated solidified body of the present invention can also have a total of more than 3 layers of cured films. In this case, the upper surface of the upper cured film is further subjected to steps (3) and (4) once to obtain a laminated solidified body having three layers of cured films, namely, a lower layer, an upper layer (middle layer), and an upper layer (uppermost layer). In addition, by repeating the same method, a laminated solidified body having more than 4 layers of cured films can also be obtained. In this way, the coating and exposure steps are repeated to produce a laminated solidified body of a desired film thickness.
[0090] [Step (5)]
[0091] Furthermore, in the step (5), the laminated cured body obtained as described above is developed.
[0092] As a developer, a sodium carbonate aqueous solution of 0.5 to 5% by weight is usually used, but other alkaline aqueous solutions may also be used. Examples of other alkaline aqueous solutions include alkaline aqueous solutions of potassium hydroxide, sodium hydroxide, potassium carbonate, sodium phosphate, sodium silicate, ammonia, and amines. The developing time varies depending on the film thickness, etc., but for example, 70 seconds to 210 seconds is set as a target.
[0093] In the present invention, it is preferred that the exposure of the upper (uppermost) uncured film is completed and the upper (uppermost) cured film is formed before simultaneous development is performed. However, the development step may be performed immediately after each exposure, such as after step (2) (exposure of the lower uncured film) and after step (4) (exposure of the upper uncured film).
[0094] [Step (6)]
[0095] The laminated solidified body of the present invention obtained after development can be further heated to a temperature of about 100 to 180° C. for thermal curing (post-curing). In the present invention, exposure is performed immediately after the formation of the uncured film, so even at the stage before development, a laminated solidified body with relatively high hardness has been obtained. However, further heat treatment is performed, thereby improving various properties of the cured product such as heat resistance, chemical resistance, moisture absorption resistance, adhesion, and electrical properties. Therefore, it is preferred to perform step (6). It should be noted that the film thickness in steps (4) to (6) does not change, so the film thickness of each cured film after step (6) is the same as the film thickness after drying in step (1) or step (3) of each cured film.
[0096] According to the manufacturing method of the stacked cured body of the present invention, each uncured film of the uncured film of the photocurable resin composition is exposed, that is, exposure (multiple exposure) is performed more than 2 times as a whole. At this point, according to the prior art, the uncured film of the photocurable resin composition with a film thickness corresponding to the whole of the stacked cured body is cured by only 1 light irradiation from above (opposite side to substrate), and the ultraviolet light irradiated from the surface of the uncured film is sometimes insufficient to reach the whole of the bottom (substrate side) of the uncured film. In this case, the photoreactivity of the cured film after exposure is monotonically reduced from the top of the cured film to the bottom. As a result, the stacked cured body of the undercut shape can be formed by the developing process. In contrast, according to the multiple exposure in the manufacturing method of the present invention, the uncured film of the film thickness of the whole of the stacked cured body is exposed in sequence, and therefore, the irradiation light from the top of the uncured film after the segmentation becomes fully reached throughout the whole of the bottom. Thus, the occurrence of undercut is suppressed.
[0097] In addition, when the lower cured film directly arranged on the substrate is exposed to the uncured film arranged on the upper layer closer to the top (directly above or above) than it, it is further cured by receiving the irradiated light of the exposure. Similarly, even if the amount of light is reduced, the layers other than the uppermost layer are sometimes affected by more than 2 exposures. That is, in the layer close to the substrate, a tendency is obtained in which the reaction rate becomes higher, and the laminated cured body has a good photocured state as a whole. It has a good photocured state as a whole of the laminated cured body, and therefore, the laminated cured body of the present invention has excellent heat resistance. In addition, the laminated cured body of the present invention can also be laminated on both sides of the substrate.
[0098] Examples of the components of the photocurable resin composition used in the present invention are shown below.
[0099] [Photocurable resin composition]
[0100] In the present invention, as the photocurable resin composition, a composition generally used in the manufacture of a solder mask and cured by exposure can be used without particular limitation. As one embodiment thereof, a composition comprising (A) a carboxyl group-containing resin, (B) a photopolymerization initiator, (C) an epoxy resin, (D) a colorant, and (E) a photopolymerizable compound can be cited.
[0101] [(A) Carboxyl-containing resin]
[0102] The photocurable resin composition of the present invention may include (A) a carboxyl-containing resin. The (A) carboxyl-containing resin may be formed into a photosensitive resin composition that can be alkali developed by including a carboxyl group. As the (A) carboxyl-containing resin, a photosensitive carboxyl-containing resin having one or more photosensitivity unsaturated double bonds may be used, and the resin is not limited to a specific substance. The (A) carboxyl-containing resin may be any of an oligomer or a polymer.
[0103] As examples of (A) carboxyl group-containing resins, the following can be suitably used.
[0104] (1) Carboxyl-containing resins obtained by copolymerization of unsaturated carboxylic acids and compounds having unsaturated double bonds;
[0105] (2) a photosensitive carboxyl-containing resin obtained by reacting a carboxyl-containing (meth) acrylic copolymer resin with a compound having an oxirane ring and an ethylenically unsaturated group in one molecule;
[0106] (3) a photosensitive carboxyl-containing resin obtained by reacting a copolymer of a compound having one epoxy group and one unsaturated double bond in one molecule and a compound having an unsaturated double bond with an unsaturated monocarboxylic acid, and reacting the resulting secondary hydroxyl group with a saturated or unsaturated polyacid anhydride;
[0107] (4) A photosensitive resin containing hydroxyl and carboxyl groups obtained by reacting a hydroxyl-containing polymer with a saturated or unsaturated polybasic acid anhydride and then reacting the resulting carboxylic acid with a compound having one epoxy group and one unsaturated double bond per molecule.
[0108] Among these, preferred are the photosensitive carboxyl group-containing resins of (2) above, which are copolymer resins having a carboxyl group obtained by reacting (a) a carboxyl group-containing (meth) acrylic copolymer resin with (b) a compound having an ethylene oxide ring and an ethylenically unsaturated group in one molecule.
[0109] The carboxyl group-containing (meth)acrylic copolymer resin (a) is obtained by copolymerizing a (meth)acrylic acid ester with a compound having one unsaturated group and at least one carboxyl group in one molecule. Examples of the (meth)acrylate constituting the copolymer resin (a) include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, and hexyl (meth)acrylate, hydroxyl-containing (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, and caprolactone-modified 2-hydroxyethyl (meth)acrylate, and glycol-modified (meth)acrylates such as methoxydiethylene glycol (meth)acrylate, ethoxydiethylene glycol (meth)acrylate, isooctyloxydiethylene glycol (meth)acrylate, phenoxytriethylene glycol (meth)acrylate, methoxytriethylene glycol (meth)acrylate, and methoxypolyethylene glycol (meth)acrylate. These may be used alone or in combination of two or more. It should be noted that, in the present specification, (meth)acrylate is a term that collectively refers to acrylate and methacrylate, and the same applies to other similar expressions.
[0110] In addition, examples of compounds having one unsaturated group and at least one carboxyl group in one molecule include acrylic acid, methacrylic acid, modified unsaturated monocarboxylic acids formed by chain extension between unsaturated groups and carboxylic acids, such as β-carboxyethyl (meth)acrylate, 2-acryloyloxyethyl succinate, 2-acryloyloxyethyl hexahydrophthalate, unsaturated monocarboxylic acids having ester bonds by lactone modification, modified unsaturated monocarboxylic acids having ether bonds, and compounds containing two or more carboxyl groups in the molecule such as maleic acid, etc. These compounds may be used alone or in combination of two or more.
[0111] As (b) a compound having an ethylene oxide ring and an ethylenically unsaturated group in one molecule, any compound having an ethylene oxide ring in one molecule may be used, for example, glycidyl (meth)acrylate, α-methyl glycidyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, 3,4-epoxycyclohexylethyl (meth)acrylate, 3,4-epoxycyclohexylbutyl (meth)acrylate, 3,4-epoxycyclohexylmethylamino acrylate, etc. Among them, 3,4-epoxycyclohexyl methyl (meth)acrylate is preferred. These (b) compounds having an ethylene oxide ring and an ethylenically unsaturated group in one molecule may be used alone or in combination of two or more.
[0112] The content of the carboxyl group-containing resin (A) in the present invention is preferably 10 to 60% by mass, more preferably 15 to 55% by mass, based on the solid content of the photocurable resin composition of the present invention.
[0113] [(B) Photopolymerization initiator]
[0114] In the photocurable resin composition of the present invention, any known photopolymerization initiator can be used as long as it is a photopolymerization initiator or a photoradical generator. Examples of the photopolymerization initiator (B) used in the present invention include benzoins and benzoin alkyl ethers such as benzoin, benzoin methyl ether, benzoin ethyl ether, and benzoin isopropyl ether; acetophenones such as acetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, and 1,1-dichloroacetophenone; aminoalkyl phenones such as 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropane-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone, and 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholino)phenyl]-1-butanone; and 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, and 1-chloroanthraquinone. Anthraquinones; thioxanthones such as 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, and 2,4-diisopropylthioxanthone; ketals such as acetophenone dimethyl ketal and benzil dimethyl ketal; benzophenones such as benzophenone; or xanthone; phosphine oxides such as (2,6-dimethoxybenzoyl)-2,4,4-pentylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, and ethyl 2,4,6-trimethylbenzoylphenylphosphonate; various peroxides, titanocene-based initiators, etc., which can be used in combination with photosensitizers such as tertiary amines such as N,N-dimethylaminobenzoic acid ethyl ester, N,N-dimethylaminobenzoic acid isopentyl ester, 4-dimethylaminobenzoic acid pentyl ester, triethylamine, and triethanolamine. These photopolymerization initiators can be used alone or in combination of two or more.
[0115] The amount of the photopolymerization initiator (B) in the present invention is preferably in the range of 0.01 to 30 parts by mass, more preferably 0.5 to 15 parts by mass, based on 100 parts by mass of the carboxyl group-containing resin (A).
[0116] [(C) Epoxy resin]
[0117] The photocurable resin composition of the present invention may contain (C) an epoxy resin in order to impart heat resistance.
[0118] Examples of the epoxy resin (C) include various commonly used epoxy resins, such as bisphenol S epoxy resins, diglycidyl phthalate resins, triglycidyl isocyanurate (e.g., TEPIC-H manufactured by Nissan Chemical Co., Ltd. (a β-form having a structure in which three epoxy groups are bonded in the same direction to the s-triazine ring skeleton surface), TEPIC (a mixture of a β-form and an α-form having a structure in which one epoxy group and two other epoxy groups are bonded in different directions to the s-triazine ring skeleton surface)), heterocyclic epoxy resins, bixylenol epoxy resins, biphenol epoxy resins, tetraglycidyl isocyanurate (e.g., TEPIC-H manufactured by Nissan Chemical Co., Ltd. (a β-form having a structure in which three epoxy groups are bonded in the same direction to the s-triazine ring skeleton surface), TEPIC (a mixture of a β-form and an α-form having a structure in which one epoxy group and two other epoxy groups are bonded in different directions to the s-triazine ring skeleton surface)), etc., bixylenol epoxy resins, biphenol epoxy resins, tetraglycidyl isocyanurate (e.g., TEPIC-H manufactured by Nissan Chemical Co., Ltd. (a β-form having a structure in which three epoxy groups are bonded in the same direction to the s-triazine ring skeleton surface)), etc., Epoxy resins that are poorly soluble in diluents, such as tetraglycidylxylenoylethane resins, bisphenol A epoxy resins, hydrogenated bisphenol A epoxy resins, bisphenol F resins, brominated bisphenol A epoxy resins, phenol novolac or cresol novolac epoxy resins, alicyclic epoxy resins, bisphenol A novolac epoxy resins, chelate epoxy resins, glyoxal epoxy resins, amino-containing epoxy resins, rubber-modified epoxy resins, dicyclopentadiene phenol epoxy resins, silicone-modified epoxy resins, ε-caprolactone-modified epoxy resins, etc. These epoxy resins can be used alone or in combination of two or more.
[0119] The amount of the epoxy resin (C) in the present invention is preferably in the range of 0.3 to 3.0 equivalents, more preferably 0.5 to 2.0 equivalents, relative to 1 equivalent of the carboxyl group of the carboxyl group-containing resin (A).
[0120] [(D) Colorant]
[0121] The photocurable resin composition of the present invention may contain (D) a colorant to form a laminated cured body reflecting the color of the colorant itself.
[0122] As the colorant (D) used in the photocurable resin composition of the present invention, conventionally known pigments or dyes such as white, black, green, blue, yellow, red, and purple can be used alone or in combination of two or more depending on the desired application.
[0123] As a white colorant, a white pigment is preferred, and specific examples thereof include titanium oxide, zinc oxide, potassium titanate, zirconium oxide, antimony oxide, white lead, zinc sulfide, lead titanate, and the like. Among white pigments, titanium oxide is preferably used from the perspective of the high inhibitory effect of heat-induced discoloration. Rutile titanium oxide is particularly preferably used as titanium oxide. Anatase titanium oxide has a higher whiteness than rutile titanium oxide, and is therefore often used. However, anatase titanium oxide has photocatalytic activity, and therefore sometimes causes discoloration of the resin in the solder mask composition. In contrast, the whiteness of rutile titanium oxide is slightly worse than that of anatase titanium oxide, but it is basically not photoactive, and therefore a stable solder mask film can be obtained. As rutile titanium oxide, a known rutile titanium oxide can be used. Specifically, TR-600, TR-700, TR-750, TR-840 manufactured by Fuji Titanium Industry Co., Ltd., R-550, R-580, R-630, R-820, CR-50, CR-60, CR-90 manufactured by Ishihara Industry Co., Ltd., KR-270, KR-310, KR-380 manufactured by Titanium Industry Co., Ltd., etc. can be used. The white pigment can be used alone or in the form of a mixture of two or more.
[0124] In order to make the photocurable resin composition white after curing, a pigment other than white, such as a blue pigment, may be added to the white pigment.
[0125] In addition, as the black colorant, a black pigment is preferred, and specific examples thereof include carbon black, lamp black, bone black, black lead, iron black, copper-chromium black, copper-iron-manganese black, cobalt-iron-chromium black, cobalt oxide such as cobalt tetraoxide, and ruthenium oxide.
[0126] Specific examples of violet pigments include cobalt violet, manganese violet, quinacridone violet, and dioxazine violet.
[0127] Specific examples of green pigments include chrome green, cobalt green, chromium oxide, phthalocyanine green, bromide green, cobalt chrome green, titanium / nickel / cobalt / zinc green, etc. Specific examples of blue pigments include ultramarine, phthalocyanine blue, metal-free / phthalocyanine / blue, indanthrene blue, cobalt blue, etc.
[0128] Specific examples of yellow pigments include yellow lead, yellow iron oxide, titanium yellow, yellow earth, antimony yellow, barium yellow, monoazo pigments, disazo pigments, polyazo pigments, isoindolinone pigments, anthracene pigments, metal complex pigments, and quinophthalone pigments.
[0129] Specific examples of red pigments include chrome vermilion, molybdenum red, Indian red, lake red 4R, carmine FB, dinitroaniline orange, pyrazolone orange, pyrazolone red, peronone orange, permanent red 2B, lake red R, maroon L (Bon Maroon Light), jujube red 10B, maroon M (Bon Maroon Medium), thioindigo jujube red, maroon L, perylene vermilion, perylene red, perylene chestnut red, and benzimidazolone orange.
[0130] When the photocurable resin composition of the present invention contains a white pigment as the colorant (D), the yellowing tendency after reflow is reduced by using the laminated cured body produced by the production method of the present invention. The reason for this is as follows.
[0131] Generally, a laminated cured body of a photocurable resin composition used as a solder mask layer or the like is exposed to a high temperature of, for example, 260° C. or higher when mounting components, thereby showing a tendency to yellow. However, according to the manufacturing method of the present invention, each uncured film is exposed independently and sequentially through the above-mentioned steps (2) and (4), so that ultraviolet light fully reaches each layer, thereby having a good photocured state, and thus having excellent heat resistance. When the components are mounted in this state, the unreacted photocurable components in each cured film, especially in the lower layer, decrease, thereby reducing the degree of yellowing. Such yellowing suppression is a very meaningful characteristic, especially for a white laminated cured body that is easily affected by yellowing. That is, if a laminated cured body manufactured from a white or light-colored photocurable resin composition turns yellow, the effect on the characteristics is greater than that of a black or dark-colored laminated cured body. When manufactured according to the method of the present invention, the tendency to yellowing is reduced, and therefore, the yellowing that is obviously produced in white or light colors, especially in white, is extremely well suppressed.
[0132] When the photocurable resin composition of the present invention contains a white pigment or a black pigment as the colorant (D), the resolution and adhesion are also improved by using the laminated cured body produced by the production method of the present invention. The reasons are as follows.
[0133] Generally, a black resist layer containing a black pigment has the property that the irradiated light during exposure is easily absorbed by the resist layer and is not easy to penetrate. In addition, a white resist layer containing a white pigment has the property that the irradiated light during exposure is easily reflected by the resist layer and is not easy to penetrate. That is, the light irradiated from the upper part of the black resist layer or the white resist layer is absorbed or reflected in the layer before reaching the depth of the resist layer. At the depth of the resist layer, etc., where the irradiated light does not fully reach, the photoreaction of the photocurable resin composition does not fully proceed, sometimes affecting the occurrence ratio and resolution of undercuts. However, according to the manufacturing method of the present invention, the above-mentioned steps (2) and (4) are provided for exposure more than 2 times, so compared with the case of 1 exposure, the photoreaction is reliably carried out throughout the entire photocurable resin composition. As a result, the resolution is improved and the occurrence of undercuts is suppressed. That is, the black resist layer or the white resist layer manufactured by the 2 exposures of the present invention has improved adhesion to the circuit substrate and becomes difficult to peel off.
[0134] In the case of a white colorant, the amount of the colorant (D) of the present invention to be added is preferably 50 to 500 parts by mass, more preferably 100 to 450 parts by mass, based on 100 parts by mass of the carboxyl group-containing resin (A).
[0135] In the case of a black colorant, the amount of the colorant (D) of the present invention to be added is preferably 1 to 50 parts by mass relative to 100 parts by mass of the carboxyl group-containing resin (A).
[0136] [(E) Photopolymerizable compound]
[0137] The photocurable resin composition of the present invention may contain the following (E) photopolymerizable compound: it has an ethylenically unsaturated group, and is photocured by irradiation with active energy rays, so that the irradiated part of the photocurable resin composition is insoluble in an alkaline aqueous solution, or helps to be insoluble. Examples of the (E) photopolymerizable compound used in the present invention include: hydroxyalkyl acrylates such as 2-hydroxyethyl acrylate and 2-hydroxybutyl acrylate; mono- or diacrylates of diols such as ethylene glycol, methoxytetraethylene glycol, polyethylene glycol, and propylene glycol; acrylamides such as N,N-dimethylacrylamide and N-hydroxymethylacrylamide; aminoalkyl acrylates such as N,N-dimethylaminoethyl acrylate; hexanediol, trimethylolpropane, pentaerythritol, dipentaerythritol, dipentaerythritol hexaacrylate ( Polyacrylates of polyols such as DHPA), trihydroxyethyl isocyanurate or their ethylene oxide or propylene oxide adducts; acrylates such as phenoxy acrylate, bisphenol A diacrylate and their phenolic ethylene oxide or propylene oxide adducts; acrylates of glycidyl ethers such as glycerol diglycidyl ether and trimethylolpropane triglycidyl ether; melamine acrylate; and / or methacrylates corresponding to the above-mentioned acrylates, etc., but are not limited to these, and well-known and commonly used photopolymerizable compounds can be used.
[0138] The amount of the photopolymerizable compound (E) in the present invention is preferably 0.01 to 40 parts by mass, more preferably 0.5 to 30 parts by mass, based on 100 parts by mass of the carboxyl group-containing resin (A).
[0139] [Organic solvents]
[0140] In order to prepare the composition or to adjust the viscosity for coating on the substrate or carrier film, the photocurable resin composition of the present invention can use an organic solvent. As the organic solvent, a known substance can be used. In addition, the organic solvent can be used alone or in combination of two or more. As such an organic solvent, ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as methyl cellosolve, ethyl cellosolve, butyl cellosolve, methyl carbitol, butyl carbitol, carbitol acetate, propylene glycol monomethyl ether, diethylene glycol monoethyl ether, dipropylene glycol monoethyl ether, and triethylene glycol monoethyl ether; esters such as ethyl acetate, butyl acetate, cellosolve acetate, diethylene glycol monoethyl ether acetate, and esters of the above glycol ethers; alcohols such as ethanol, propanol, ethylene glycol, and propylene glycol; aliphatic hydrocarbons such as octane and decane; petroleum solvents such as petroleum ether, petroleum naphtha, hydrogenated petroleum naphtha, and solvent naphtha, etc.
[0141] Furthermore, a curing catalyst, a curing accelerator, a thermal polymerization inhibitor, a thickener, a defoaming agent, a leveling agent, a coupling agent, a flame retardant auxiliary agent, etc. may be used as necessary.
[0142] The photocurable resin composition of the present invention can be applied on a substrate in a liquid or paste form and dried to be laminated.
[0143] Example
[0144] Hereinafter, the present invention will be described based on Examples, but the present invention is not limited thereto. All "parts" and "%" described below are based on mass unless otherwise specified.
[0145] [Production Example of Photocurable Resin Composition]
[0146] [Manufacturing of Composition 1 and Composition 2]
[0147] The components described in Table 1 below were blended in the amounts described in the same table, stirred, and dispersed using a three-roll mill to prepare a photocurable resin composition. The numbers in Table 1 represent parts by mass in terms of varnish including a solvent.
[0148] [Table 1]
[0149] Table 1
[0150]
[0151] The details of the components in Table 1 are as follows.
[0152] (A) Carboxyl group-containing resin Cyclomer P (ACA) Z250: an acrylic oligomer manufactured by Daicel Corporation (average molecular weight (Mw): 22,000) solid content concentration 53% by mass (solvent: dipropylene glycol monomethyl ether)
[0153] (B) Photopolymerization initiator Omnirad 819: manufactured by IGM Resins, bis(2,4,6-methylbenzoyl)phenylphosphine oxide
[0154] (B) Photopolymerization initiator 2,4,6-trimethylbenzoyldiphenylphosphine oxide
[0155] (C) Epoxy resin jER-828: manufactured by Mitsubishi Chemical Corporation, epoxy equivalent: 184 to 194, liquid at room temperature (25°C), molecular weight (Mw): about 370
[0156] (D) Colorant CR-90: manufactured by Ishihara Sangyo Co., Ltd., rutile titanium oxide
[0157] (D) Colorant MA-100: manufactured by Mitsubishi Chemical Corporation, carbon black
[0158] (E) Photopolymerizable compound DPHA: dipentaerythritol hexaacrylate, DAICEL-ALLNEX Co., Ltd.
[0159] Curing catalyst DICY: dicyandiamide
[0160] Curing catalyst melamine
[0161] [Examples 1 to 4, Comparative Examples 1 to 4]
[0162] Using the composition 1 and the composition 2 produced as described above, a laminated cured body consisting of one, two or three layers of cured films was produced.
[0163] The following describes the method for producing a laminated cured product of the present invention and the evaluation of the obtained laminated cured product. In Table 2, "-" in the treatment process indicates that the corresponding treatment was not performed, and "-" in the evaluation item indicates that the composition 2 containing no white colorant was used and the function as a reflective material was not required, so the corresponding evaluation was not performed.
[0164] <Production of Evaluation Substrate>
[0165] <1. Formation of the lower layer>
[0166] As shown in Table 2, in Example 1, the composition 1 was printed on the entire surface of the circuit substrate pre-treated by pickling and polishing (two series of Scotch brite SF (equivalent to #600) and UEF (equivalent to #1000)) by screen printing with #100 so that the film thickness after drying was 25 μm. The uncured film of the composition 1 thus obtained was dried for 15 minutes (pre-cured) at 80°C using a hot air circulation drying oven (DF610 manufactured by Yamato Scientific Co., Ltd.). Then, for the dried uncured film, a direct exposure machine (DiIMPACT Mms60 manufactured by ORCMANUFACTURING CO., LTD.) using a metal halide as a light source was used to form a line pattern of 30 to 300 μm width (30 μm scale) at a cumulative exposure amount of 600 mJ / cm 2 Exposure was performed. The same treatment was performed in Examples 2 to 4 and Comparative Examples 1 to 3, but Composition 2 was used in Example 4 and Comparative Example 3. In addition, exposure was not performed in Comparative Examples 1 to 3. Thereafter, in Example 2, development was performed for 70 seconds using a 1 mass % sodium carbonate aqueous solution at a liquid temperature of 30°C and a spraying pressure of 0.2 MPa. In Comparative Example 4, printing, drying, and exposure were performed using the same apparatus and steps as in Example 1, but full-surface printing was performed based on #60 screen printing in such a way that the film thickness after drying became 50 μm, the drying time at 80°C was 30 minutes, and the cumulative exposure amount was 1200 mJ / cm 2 .
[0167] It should be noted that in Table 2, those that have undergone corresponding processing steps are represented by symbols 0 or ●.
[0168] <2. Formation of the upper layer (middle layer)>
[0169] As described in Table 2, pickling and polishing were not performed on the lower layer of Example 3. In addition, the upper layer (middle layer) was formed according to the same operation as that of Example 1 described in relation to the formation of the lower layer. It should be noted that in the examples and comparative examples other than Example 3, the upper layer (middle layer) was not provided, and a laminated solid body having the upper layer (uppermost layer) in Table 2 directly on the lower layer was formed.
[0170] <3. Formation of the upper layer (top layer)>
[0171] Furthermore, as described in Table 2, an upper layer (uppermost layer) was formed on the upper surface of the lower layer of Examples 1, 2, 4 and Comparative Examples 1 to 3 and the upper surface of the upper layer (middle layer) of Example 3. In each Example and Comparative Example, the same composition as the composition was used to form the lower layer, and the entire surface was printed using a #100 screen printing machine in such a manner that the film thickness after drying became 25 μm, and dried at 80°C for 30 minutes (pre-curing) using a hot air circulation drying furnace (DF610 manufactured by Yamato Scientific Co., Ltd.). For the dried uncured film, a direct exposure machine using a metal halide as a light source (DiIMPACT Mms60 manufactured by ORCMANUFACTURING CO., LTD.) was used to form a line pattern of 30 to 300 μm width (30 μm scale). In Examples 1 to 4 and Comparative Examples 1 and 3, the cumulative exposure amount was 600 mJ / cm 2 Exposure was performed. In Comparative Example 2, the cumulative exposure amount was 1200 mJ / cm 2 Then, a 1 mass % sodium carbonate aqueous solution at a liquid temperature of 30° C. was used for development for 210 seconds in Example 3 and for 140 seconds in other Examples and Comparative Examples under the condition of a spray pressure of 0.2 MPa. It should be noted that in Comparative Example 4, no upper layer was provided on the lower layer, and a cured body consisting of only one lower layer was prepared.
[0172] <4. Post-curing>
[0173] The laminated cured body subjected to the above treatment was heated and post-cured in a heat cycle box furnace at 150° C. for 60 minutes. Thus, evaluation substrates of laminated cured bodies of Examples 1 to 4 of the present invention and laminated cured bodies of Comparative Examples 1 to 4 were obtained. It should be noted that the film thickness did not change during the period from exposure to post-curing, and therefore, the film thickness of the laminated cured body after post-curing was the same as that after drying (dry state).
[0174] <Evaluation>
[0175] The following evaluation tests were performed using the above-mentioned evaluation substrates. The results are shown in Table 2.
[0176] <1. Evaluation of resolution>
[0177] The minimum line width remaining in each evaluation substrate before post-curing in the above-mentioned <Preparation of Evaluation Substrate> was evaluated.
[0178] <2. Peeling of evaluation substrate after gold plating>
[0179] The surface of the evaluation substrate was subjected to acid degreasing, soft etching, and sulfuric acid treatment as pretreatment, and gold plating was performed using an electroless nickel plating bath and an electroless gold plating bath under conditions such that nickel was plated to a thickness of 3 μm and gold was plated to a thickness of 0.03 μm.
[0180] Thereafter, a tape peeling test was performed on the gold-plated evaluation substrate in accordance with JIS K 5600-5-6 to evaluate the minimum line width remaining on the evaluation substrate.
[0181] <3. Evaluation of discoloration resistance>
[0182] A substrate for evaluating discoloration resistance was prepared according to the same procedure except that the entire surface of the dried uncured film was exposed to light instead of the step of exposing the film so as to form a line pattern in the above <Preparation of Evaluation Substrate>.
[0183] The substrate for evaluating discoloration resistance was subjected to reflow treatment five times with a maximum temperature of 285° C. using a reflow apparatus (NIS-20-82C manufactured by EIGHTECH TECTRON Co., Ltd.).
[0184] Before and after the reflow treatment, the L* value, a* value, and b* value of the cured film surface on the substrate for evaluating discoloration resistance were measured in accordance with JIS Z 8781 using a spectrophotometer CM-2600d manufactured by Konica Minolta, Inc. in the L*a*b* colorimetric system, and ΔE calculated using formula (1) based on the changes in the L* value, a* value, and b* value (ΔL, Δa, Δb) obtained by comparing the values before and after the reflow treatment was evaluated using the following criteria.
[0185] ΔE={(ΔL) 2 +(Δa) 2 +(Δb) 2} 1 / 2 Formula (1)
[0186] ◎: 1.5 or less
[0187] ○: More than 1.5 and less than 2.0
[0188] △: More than 2.0 and less than 2.5
[0189] ×: more than 2.5
[0190] <Evaluation of solder ball bonding>
[0191] A substrate for bonding evaluation in which a copper circuit was exposed in the through-hole opening was produced by the same process except that exposure was performed so that the through-hole opening diameter became 500 μm instead of the exposure step in the above <Production of Evaluation Substrate> to form a line pattern.
[0192] Solder balls were formed at the through-hole openings of each bonding evaluation substrate by using a eutectic solder of Sn / Pb=63 / 37 and performing a reflow process in a reflow furnace at 150°C (90 seconds) + 220°C (10 seconds).
[0193] Next, a heated bump pull test was performed using a universal bond tester (bond tester "Series 4000") manufactured by Dazzy Co., Ltd. in the following manner.
[0194] First, the tensile probe of the bonding strength tester is heated with a heater, and when the tip temperature of the tensile probe reaches 270°C, the tip of the tensile probe is vertically inserted into the center of the solder ball. After that, the tensile probe is naturally cooled in the inserted state until the tip temperature of the tensile probe reaches 40°C, thereby fixing the solder ball and the tensile probe. Next, the tensile probe is vertically pulled up at a speed of 300μm / second, and the strength (bonding strength (N)) required for the solder ball to peel off from the bonding surface (interface peeling) is measured as the bonding strength.
[0195] The measured bonding strength was evaluated based on the following criteria.
[0196] ◎: Bonding strength is 8.5N or more
[0197] ○: Bonding strength is 7.5N or more and less than 8.5N
[0198] △: Bonding strength is 6.0N or more and less than 7.5N
[0199] ×: Bonding strength is less than 6.0N [Table 2]
[0200]
[0201] Figure 7 A cross-sectional view of the laminate obtained in Comparative Example 1 is shown in FIG.
[0202] In Comparative Example 1, the lower layer was printed and dried, and then the upper layer was provided on the dried lower layer without exposure. As a result, significant undercutting was observed in the obtained laminate. Figure 7 A schematic cross-sectional view of the laminated cured body of Comparative Example 1 is shown in FIG.
[0203] As mentioned above, the invention made by the present inventors has been specifically described based on the embodiment, but the present invention is not limited to the above-mentioned embodiment, and various modifications can be made without departing from the scope of the invention.
[0204] Description of Reference Numerals
[0205] 1 Circuit board
[0206] 3-layer solidified body
[0207] 3A lower layer curing film
[0208] 3Aa The end surface of the lower cured film
[0209] 3B upper curing film
[0210] 3Ba The end surface of the upper cured film
[0211] Concave part of 3C laminated solid body
[0212] 5. Conductor part
[0213] 10. Printed Circuit Board.
Claims
1. A laminated solidified body, characterized in that: It is used as an anti-corrosion layer of a printed circuit board. The laminated cured body comprises: a lower cured film which is laminated on any one of the surfaces of the printed circuit board and is formed of a photocurable resin composition which is photocured; and, one or more upper cured films, which are laminated on the lower cured film and are formed from a photocurable resin composition which is separately photocured, The end surface of each of the stacked and cured films has one or more recessed portions extending in the peripheral direction along the bonding surface between the lower layer cured film and the upper layer cured film or along the bonding surfaces of the plurality of upper layer cured films.
2. The laminated solidified body according to claim 1, characterized in that: The laminate is stacked so as to surround the conductor portion provided on the printed circuit board, and the recess is formed along the inner peripheral surface of the laminated solid body.
3. The laminated solidified body according to claim 1, characterized in that: The conductors are stacked on both sides of a conductor portion provided on a printed circuit board so as to face each other, and the recesses are formed on the end surfaces facing each other.
4. A printed circuit board, characterized in that: A laminated cured body according to any one of claims 1 to 3.
5. A method for producing a laminated solidified body according to any one of claims 1 to 3, characterized in that: The invention relates to a method for producing a laminated solid body used as an anti-corrosion layer of a printed circuit board, the method comprising the following steps: (1) a step of forming an uncured film of a lower layer, wherein a photocurable resin composition is applied to any one of the surfaces of a printed circuit board and dried to form an uncured film of a lower layer; (2) a lower layer cured film forming step of exposing and curing the lower layer uncured film; (3) forming an upper uncured film, coating the upper surface of the lower cured film with a photocurable resin composition which is the same as or different from the photocurable resin composition and drying the composition to form an upper uncured film; and, (4) An upper cured film forming step of exposing and curing the upper uncured film.
6. The method for producing a laminated solidified body according to claim 5, characterized in that: The following step is further included after the one or more steps of forming the uncured film of the upper layer and forming the cured film of the upper layer: (5) a development step of applying a development treatment to the laminated lower cured film and upper cured film; and, (6) A thermal curing step of thermally curing the laminated lower layer cured film and upper layer cured film after development.
7. The method for producing a laminated solidified body according to claim 5, wherein: The photocurable resin composition comprises: (A) a carboxyl group-containing resin, (B) a photopolymerization initiator, (C) an epoxy resin, (D) a colorant, and (E) a photopolymerizable compound.
8. The method for producing a laminated solid body according to claim 5, wherein: The colorant (D) includes a white colorant, and the amount of the colorant blended is 50 to 500 parts by mass relative to 100 parts by mass of the carboxyl group-containing resin (A).
9. The method for producing a laminated solidified body according to claim 5, wherein: The (D) colorant includes a black colorant, and the amount of the colorant blended is 1 to 50 parts by mass based on 100 parts by mass of the (A) carboxyl group-containing resin.
Citation Information