Photo-assisted metal organic framework interlayer forward osmosis membrane, preparation method and application

By using the intermediate layer of the light-assisted metal organic frame in the lithium concentrated film, the interface polymerization process is regulated and the dense separation layer is formed, which solves the problem of low recovery efficiency of traditional films and improves high water flux and lithium ion recovery rate.

CN119015901APending Publication Date: 2024-11-26XI'AN UNIVERSITY OF ARCHITECTURE AND TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411343381.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Traditional positive permeability membranes have low recovery efficiency in lithium concentration applications, mainly due to the fast diffusion rate of amine monomers and the low roughness of the separation layer, resulting in insufficient water flux and the presence of defective holes.

Method used

By using the preparation method of the photo-assisted metal organic frame intermediate layer positive permeation membrane, PCN-134-2D nanosheets and 5,10,15,20-tetrakis(4-carboxyphenyl)porphyrin are uniformly dispersed on the surface of the nylon support layer. Combined with ultraviolet light, the interface polymerization process is regulated to form a dense separation layer, slow down the diffusion of amine monomers and improve the roughness of the separation layer.

Benefits of technology

It significantly improves water flux and lithium ion recovery, reduces reverse solute flux, optimizes membrane structure, and improves the efficiency of lithium concentration applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119015901A_ABST
    Figure CN119015901A_ABST
Patent Text Reader

Abstract

The invention discloses a photo-assisted metal organic framework interlayer forward osmosis membrane, a preparation method and application, and belongs to the technical field of preparation of osmosis membranes. According to the preparation method provided by the invention, PCN-134-2D nanosheets and 5, 10, 15, 20-tetra (4-carboxyphenyl) porphyrin are selected as interlayer materials of the forward osmosis membrane, and light irradiation is assisted, so that the purposes of regulating and controlling the interfacial polymerization process and optimizing the structure of the forward osmosis membrane are achieved. The middle layer material has a large number of carboxyl groups, and the diffusion rate of amine monomers in interfacial polymerization can be slowed down based on strong interaction of the middle layer material and the amine monomers; furthermore, the material of the middle layer has a unique photo-thermal characteristic, can generate heat through ultraviolet radiation, and can promote rapid self-polymerization of an interface, so that a thin and compact separation layer structure is obtained; and meanwhile, a large amount of soluble gas in a water-phase solution escapes due to the photothermal effect, so that more nanometer bubble structures are formed on the separation layer, the roughness of the separation layer is improved, and the method has an excellent lithium concentration application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of osmotic membrane preparation, and in particular to a light-assisted metal organic framework intermediate layer forward osmosis membrane, a preparation method and an application thereof. Background Art

[0002] With the rapid growth of global energy demand, lithium, as a key strategic resource, has become increasingly important. Especially in the fields of new energy vehicles and energy storage systems, the demand for lithium continues to rise. Whether lithium is extracted from brine or ore, the lithium solution needs to be highly concentrated before precipitation to obtain lithium products. Lithium concentration currently relies on traditional processes such as evaporation crystallization and reverse osmosis. These methods are not only extremely energy-intensive, but also have high requirements for equipment.

[0003] In recent years, forward osmosis technology, as a new type of membrane separation technology, has gradually attracted attention and attention due to its advantages such as high efficiency, energy saving and environmental protection, and has gradually been used in fields such as lithium concentration and recovery. However, traditional thin-layer composite forward osmosis membranes often have thicker polyamide separation layers, which is due to the excessively fast rate of aqueous phase monomers (usually amine monomers) during interfacial polymerization. The thicker separation layer increases the distance and resistance of the solvent (usually water) through the membrane, and reduces the amount of solvent passing through the membrane per unit time, that is, the water flux. Secondly, a thicker polyamide layer may cause more serious concentration polarization and membrane fouling, further reducing the permeability of the membrane. In addition, due to the large pore size of the support layer of the traditional forward osmosis membrane, it is difficult for amine monomers to be retained during interfacial polymerization, which makes it difficult to form a uniform and dense polyamide separation layer on the surface of the support layer, and it is easy to produce non-selective defective holes. The presence of these defective holes greatly reduces the recovery performance of the membrane for lithium ions, thereby affecting the lithium concentration effect.

[0004] In addition, these defective holes may also allow reverse solutes to enter the permeate side, thereby reducing the osmotic pressure difference between the two phases and reducing the system processing capacity. Constructing a metal organic framework nanosheet intermediate layer can prevent the loss of amine monomers and slow down the diffusion rate of amine monomers during interfacial polymerization, which reduces the thickness of the separation layer and avoids the formation of defective holes in the separation layer, thereby effectively improving the membrane structure and enhancing its lithium concentration performance.

[0005] However, although the metal organic framework nanosheet intermediate layer forward osmosis membrane has improved the lithium recovery effect to a certain extent, the roughness of the separation layer has been significantly reduced due to the construction of the uniform metal organic framework nanosheet intermediate layer. This change has led to a lower water flux of the forward osmosis membrane and limited improvement in water permeability, which has affected the recovery efficiency of the forward osmosis membrane in lithium concentration applications.

[0006] Therefore, how to slow down the diffusion rate of amine monomers in interfacial polymerization, increase the roughness of the separation layer, and thereby improve the recovery efficiency of forward osmosis membranes in lithium concentration applications has become a technical problem that technicians in this field urgently need to overcome. Summary of the invention

[0007] The purpose of the present invention is to provide a light-assisted metal organic framework intermediate layer forward osmosis membrane, a preparation method and an application thereof, so as to overcome the problem in the prior art that the recovery efficiency of the forward osmosis membrane in lithium concentration applications is low due to the fast diffusion rate of the amine monomer and the low roughness of the separation layer.

[0008] The present invention solves the above technical problems through the following technical solutions: A method for preparing a light-assisted metal organic framework intermediate layer forward osmosis membrane comprises the following steps: The PCN-134-2D nanosheets were uniformly dispersed in deionized water, and 5,10,15,20-tetrakis(4-carboxyphenyl)porphyrin was added to obtain a mixed solution A; The mixed solution A is loaded on the surface of the nylon support layer by vacuum filtration to obtain an intermediate layer; The intermediate layer is irradiated under ultraviolet light conditions; and under ultraviolet light conditions, an aqueous monomer solution of m-phenylenediamine and an organic solution of trimesoyl chloride are added to the surface of the irradiated intermediate layer, respectively, so that the m-phenylenediamine and trimesoyl chloride undergo an interfacial polymerization reaction and form a separation layer, thereby obtaining a light-assisted metal organic framework intermediate layer forward osmosis membrane.

[0009] Furthermore, the mass ratio of PCN-134-2D nanosheets to 5,10,15,20-tetrakis(4-carboxyphenyl)porphyrin is (1~4):1.

[0010] Furthermore, the interfacial polymerization reaction specifically includes: An aqueous solution of meta-phenylenediamine monomer is added to the surface of the intermediate layer for soaking, and excess solution is removed after soaking to obtain a dried film; then an organic solution of trimesoyl chloride is added to the surface of the dried film for reaction, and excess solution is removed after the reaction, and thermal curing is performed at 40 ºC to 80 ℃ for 2 to 5 minutes to complete the interfacial polymerization reaction.

[0011] Furthermore, the steps of obtaining PCN-134-2D nanosheets include: Step 1: Preparation of PCN-134-2D precursor: The benzoic acid was dissolved in N,N-dimethylformamide, and after ultrasonication, zirconium tetrachloride, 1,3,5-tri(4-carboxyphenyl)benzene and ultrapure water were added, and after ultrasonication again, a mixed solution B was obtained; the mixed solution B was heated at 85°C to 175°C for 14 h to 52 h, and the supernatant was obtained by centrifugation and filtered, and then washed with N,N-dimethylformamide and methanol respectively to obtain a PCN-134-2D precursor; Step 2: Preparation of PCN-134-2D nanosheets: The PCN-134-2D precursor and 5,10,15,20-tetrakis(4-carboxyphenyl)porphyrin are uniformly dispersed in N,N-dimethylformamide to obtain a mixed solution C; the mixed solution C is continuously reacted at 80 ºC to 120 ºC for 8 to 12 h; the solid product is collected after centrifugation, and after alternately washing with N,N-dimethylformamide and acetone washing solution for 3 to 5 times, it is vacuum dried at 40 ºC to 80 ºC to obtain PCN-134-2D powder; after ultrasonic centrifugation, the supernatant is taken to obtain a PCN-134-2D dispersion; and then vacuum dried to obtain PCN-134-2D nanosheets.

[0012] Furthermore, in the mixed solution B, every (40-80) g of benzoic acid corresponds to (20-40) mL of N,N-dimethylformamide, (1-3) g of zirconium tetrachloride, (1-3) g of 1,3,5-tris(4-carboxyphenyl)benzene and (40-60) mL of ultrapure water; In mixed solution C, every (10 ~ 20) mg of PCN-134-2D precursor corresponds to (2 ~ 3) mmol of 5,10,15,20-tetrakis(4-carboxyphenyl)porphyrin and (3 ~ 5) mL of N,N-dimethylformamide.

[0013] Furthermore, the pressure of the vacuum filtration is 0.01 Mpa to 0.06 Mpa; the ultraviolet light condition is provided by a xenon lamp, the irradiation intensity is 0 to 20 A, and the irradiation time is 1 min to 8 min, wherein the irradiation time of the middle layer is 25 to 35 seconds.

[0014] Furthermore, the step of obtaining the aqueous phase monomer solution of m-phenylenediamine comprises: Dissolve m-phenylenediamine in deionized water to obtain an aqueous phase monomer solution of m-phenylenediamine, wherein the mass fraction of the aqueous phase monomer solution of m-phenylenediamine is 1.5 wt% to 3 wt%.

[0015] Further, the step of obtaining the trimesoyl chloride organic phase solution comprises: The trimesoyl chloride is dissolved in n-hexane to obtain a trimesoyl chloride organic phase solution, wherein the mass fraction of the trimesoyl chloride organic phase solution is 0.2 wt% to 1 wt%.

[0016] A light-assisted metal organic framework intermediate layer forward osmosis membrane is prepared by adopting the above-mentioned preparation method.

[0017] An application of the above-mentioned light-assisted metal organic framework intermediate layer forward osmosis membrane in lithium concentration.

[0018] Compared with the prior art, the positive and progressive effects of the present invention are: The preparation method of the light-assisted metal organic framework intermediate layer forward osmosis membrane provided by the present invention achieves the purpose of regulating the interfacial polymerization process and optimizing the structure of the forward osmosis membrane by selecting PCN-134-2D nanosheets and 5,10,15,20-tetrakis(4-carboxyphenyl)porphyrin as the intermediate layer materials of the forward osmosis membrane and assisting light irradiation. The intermediate layer material as an intermediate layer can prevent the loss of aqueous phase monomers and avoid the formation of defective pores; and it has a large number of carboxyl groups, which can slow down the diffusion rate of amine monomers in interfacial polymerization based on its strong interaction with amine monomers; furthermore, the intermediate layer material has unique photothermal properties, generates heat through ultraviolet irradiation, and can promote rapid self-polymerization of the interface, thereby obtaining a thin and dense separation layer structure; at the same time, the photothermal effect will cause a large amount of dissolved gas in the aqueous phase solution to escape, so that the separation layer forms more nanobubble structures, and the roughness of the separation layer is improved. Based on the optimization of the separation layer structure, the obtained forward osmosis membrane exhibits good water flux, reverse solute interception performance and lithium ion recovery, and has excellent application prospects for lithium concentration. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The drawings in the specification are used to provide further understanding of the present invention and constitute a part of the present invention. The schematic embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0020] Figure 1 It is a schematic diagram of the preparation process of the present invention; Figure 2 It is a schematic diagram of the temperature of the intermediate layer of the present invention under different light intensities. DETAILED DESCRIPTION

[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art; obviously, the drawings described below are some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0022] The present invention is further described in detail below in conjunction with the accompanying drawings, which are intended to explain the present invention rather than to limit it.

[0023] See also Figure 1 The present invention provides a method for preparing a light-assisted metal organic framework intermediate layer forward osmosis membrane, comprising the following steps: The PCN-134-2D nanosheets were uniformly dispersed in deionized water, and 5,10,15,20-tetrakis(4-carboxyphenyl)porphyrin was added to obtain a mixed solution A; The mixed solution A is loaded on the surface of the nylon support layer by vacuum filtration to obtain an intermediate layer; Under ultraviolet light conditions, the intermediate layer is irradiated; under ultraviolet light conditions, the aqueous phase monomer solution of m-phenylenediamine and the organic phase solution of trimesoyl chloride are added to the surface of the irradiated intermediate layer respectively, so that the m-phenylenediamine and trimesoyl chloride undergo interfacial polymerization reaction and form a separation layer, thereby obtaining a light-assisted metal organic framework intermediate layer forward osmosis membrane. Specifically, the mass ratio of PCN-134-2D nanosheets to 5,10,15,20-tetrakis(4-carboxyphenyl)porphyrin is (1~4):1.

[0024] Specifically, the interfacial polymerization reaction includes: An aqueous solution of meta-phenylenediamine monomer is added to the surface of the intermediate layer for soaking, and excess solution is removed after soaking to obtain a dried film; then an organic solution of trimesoyl chloride is added to the surface of the dried film for reaction, and excess solution is removed after the reaction, and thermal curing is performed at 40 ºC to 80 ℃ for 2 to 5 minutes to complete the interfacial polymerization reaction.

[0025] Specifically, the pressure of the vacuum filtration is 0.01 Mpa to 0.06 Mpa; the ultraviolet light condition is provided by a xenon lamp, the irradiation intensity is 0 to 20 A, and the irradiation time is 1 min to 8 min, wherein the irradiation time of the middle layer is 25 to 35 seconds.

[0026] Wherein, the step of obtaining the aqueous phase monomer solution of m-phenylenediamine comprises: Dissolve m-phenylenediamine in deionized water to obtain an aqueous phase monomer solution of m-phenylenediamine, wherein the mass fraction of the aqueous phase monomer solution of m-phenylenediamine is 1.5 wt% to 3 wt%; the step of obtaining an organic phase solution of trimesoyl chloride comprises: dissolving trimesoyl chloride in n-hexane to obtain an organic phase solution of trimesoyl chloride, wherein the mass fraction of the organic phase solution of trimesoyl chloride is 0.2 wt% to 1 wt%.

[0027] The preparation method of PCN-134-2D nanosheets is as follows: Step 1: Preparation of PCN-134-2D precursor: The benzoic acid was dissolved in N,N-dimethylformamide, and after ultrasonication, zirconium tetrachloride, 1,3,5-tri(4-carboxyphenyl)benzene and ultrapure water were added, and after ultrasonication again, a mixed solution B was obtained; the mixed solution B was heated at 85°C to 175°C for 14 h to 52 h, and the supernatant was obtained by centrifugation and filtered, and then washed with N,N-dimethylformamide and methanol respectively to obtain a PCN-134-2D precursor; Step 2: Preparation of PCN-134-2D nanosheets: The PCN-134-2D precursor and 5,10,15,20-tetrakis(4-carboxyphenyl)porphyrin are uniformly dispersed in N,N-dimethylformamide to obtain a mixed solution C; the mixed solution C is continuously reacted at 80 ºC to 120 ºC for 8 to 12 h; the solid product is collected after centrifugation, and after alternately washing with N,N-dimethylformamide and acetone washing solution for 3 to 5 times, it is vacuum dried at 40 ºC to 80 ºC to obtain PCN-134-2D powder; after ultrasonic centrifugation, the supernatant is taken to obtain a PCN-134-2D dispersion; and then vacuum dried to obtain PCN-134-2D nanosheets.

[0028] In the mixed solution B, every (40-80) g of benzoic acid corresponds to (20-40) mL of N,N-dimethylformamide, (1-3) g of zirconium tetrachloride, (1-3) g of 1,3,5-tris(4-carboxyphenyl)benzene and (40-60) mL of ultrapure water; In mixed solution C, every (10 ~ 20) mg of PCN-134-2D precursor corresponds to (2 ~ 3) mmol of 5,10,15,20-tetrakis(4-carboxyphenyl)porphyrin and (3 ~ 5) mL of N,N-dimethylformamide.

[0029] In this preparation method, on the surface of the nylon support layer, the PCN-134-2D material is used as an intermediate layer, and then interfacial polymerization is performed on the intermediate layer to obtain a separation layer. Compared with the nanomaterial intermediate layer membrane, the PCN-intermediate layer composite forward osmosis membrane constructed in this paper uses the photothermal effect to regulate the roughness of the separation layer, which not only improves the hydrophilicity of the membrane but also uses the light intensity to regulate the roughness of the membrane surface.

[0030] The test method of the membrane prepared by the present invention adopts the following method: deionized water is used as the raw material liquid, 1 mol / L NaCl is used as the draw liquid, and the performance of the prepared forward osmosis membrane is tested under the condition of a membrane surface flow rate of 12.5 cm / s at room temperature. V and reverse solute flux J S , calculated according to the following formulas:

[0031]

[0032] Where △V represents the permeation volume (L), A eff Indicates the effective area of ​​the membrane (㎡), C t Indicates the salt concentration of the raw water at time t (g / L), V t It represents the volume of the raw water side at time t (L), and △t represents the penetration time (h).

[0033] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not used to limit the scope of protection of the present invention.

[0034] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0035] It should be noted that the process equipment or devices not specifically specified in the following embodiments are all conventional equipment or devices in the art.

[0036] In addition, it should be understood that one or more method steps mentioned in the present invention do not exclude the existence of other method steps before or after the combination step or the insertion of other method steps between these explicitly mentioned steps, unless otherwise specified; it should also be understood that the combination connection relationship between one or more devices / apparatuses mentioned in the present invention does not exclude the existence of other devices / apparatuses before or after the combination device / apparatus or the insertion of other devices / apparatuses between these explicitly mentioned two devices / apparatuses, unless otherwise specified. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or the scope of the present invention. Changes or adjustments in their relative relationships should also be regarded as the scope of the present invention without substantially changing the technical content.

[0037] Unless otherwise specified in the following examples, all raw materials are commercially available or prepared by conventional methods in the art.

[0038] Among the following, m-phenylenediamine: purity is 99.5%, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; zirconium tetrachloride: purity is 99.9%, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; trimesoyl chloride: purity is 98%, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; n-hexane: purity is analytical grade, purchased from Guangdong Guanghua Technology Co., Ltd.; N,N-dimethylformamide: purity is analytical grade, purchased from Guangdong Guanghua Technology Co., Ltd.; methanol: purity is analytical grade, purchased from Tianjin Tianli Chemical Reagent Co., Ltd.; 5,10,15,20-tetrakis(4-carboxyphenyl)porphyrin: purity 99%, purchased from Jiangsu Aikang Biopharmaceutical Research and Development Co., Ltd.; acetone: CAS number 67-64-1, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; benzoic acid: CAS number 65-85-0, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; 1,3,5-tris(4-carboxyphenyl)benzene: CAS number: 50446-44-1, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.

[0039] Comparative Example 1: The support layer is a nylon microfiltration membrane with a pore size of 0.2 μm. At a constant temperature of 25°C, the support layer is immersed in a 2.5% by mass aqueous solution of m-phenylenediamine for 5 minutes. After drying, a 0.5% by mass organic solution of trimesoyl chloride is poured on the surface of the support layer. After 1 minute, the excess organic solution is poured off, and finally the support layer is placed in an oven at 60°C for thermal curing for 2 minutes.

[0040] The prepared forward osmosis membrane was evaluated. The flow rate on both sides of the membrane was 12.5 cm / s. The raw liquid was deionized water, and the draw liquid was 1 mol / L sodium chloride solution. The test was carried out at room temperature. The water flux of the prepared forward osmosis membrane was 15.91 L▪m -2 ▪h (LMH), the reverse solute flux is 2.15 g▪ m -2 ▪h (gMH), the lithium ion recovery rate was 85.7%.

[0041] Embodiment 1: Preparation of PCN-134-2D precursor: dissolve benzoic acid in N,N-dimethylformamide, perform ultrasound for 1 h, add zirconium tetrachloride, 1,3,5-tris(4-carboxyphenyl)benzene (H3BTB) and ultrapure water, perform ultrasound for 1 h twice, and obtain mixed solution B; place the obtained mixed solution in an oven at 85℃~175℃, react for 14h~52h, and place the obtained material and solution in a centrifuge for centrifugation at a speed of 3500r / min~8000r / min. Take the supernatant and filter it, wash it with N,N-dimethylformamide and methanol to obtain PCN-134-2D precursor. Preparation of PCN-134-2D nanosheets: The obtained PCN-134-2D precursor (50-100 mg) and 5,10,15,20-tetrakis(4-carboxyphenyl)porphyrin (H4TCPP) (10-15 mmol) were dispersed in 20 mL of N,N-dimethylformamide to obtain a mixed solution C; the obtained mixed solution C was continuously reacted at 100°C for 8-12 hours; the solid was collected by centrifugation, and was alternately washed with N,N-dimethylformamide and acetone washing solution for 3-5 times, and the product was vacuum dried at 40-80°C for 12 hours to obtain PCN-134-2D powder, and an appropriate amount of the powder was taken for ultrasonic centrifugation, and the supernatant, i.e., the PCN-134-2D dispersion, was taken; and then vacuum dried to obtain PCN-134-2D nanosheets.

[0042] Step 1, 5-20 mg of PCN-134-2D nanosheets are dispersed evenly in 120 mL of deionized water, and 0.05 mg of 5,10,15,20-tetrakis(4-carboxyphenyl)porphyrin (H4TCPP) is added to obtain a mixed solution A; Step 2, dissolving 10 g of m-phenylenediamine (MPD) in 390 g of deionized water, stirring for 30 min to obtain an aqueous phase monomer solution of m-phenylenediamine; dissolving 0.5 g of trimesoyl chloride (TMC) in 95 g of n-hexane, and ultrasonicating for 30 min to obtain an organic solution of trimesoyl chloride; Step 3, the mixed solution A prepared in step 1 is loaded on the surface of the nylon support layer by vacuum filtration to form an intermediate layer; 10 mL of the aqueous phase monomer solution of m-phenylenediamine in step 2 is added to the surface of the formed intermediate layer and soaked for 5 minutes, and the excess solution is removed after soaking; the prepared treated trimesoyl chloride organic solution is poured onto the membrane surface and illuminated under light sources of different intensities for 1 to 8 minutes to remove the excess solution, and then placed in an oven at 60°C for thermal curing for 2 to 5 minutes to form a separation layer, thereby obtaining a light-assisted metal organic framework intermediate layer forward osmosis membrane.

[0043] Based on the forward osmosis membrane preparation method in Comparative Example 1, the difference is that PCN-134-2D nanosheets and 5,10,15,20-tetrakis(4-carboxyphenyl)porphyrin are selected as the intermediate layer materials of the forward osmosis membrane, and the mixed solution A is filtered to the surface of the support layer by 0.04MPa pressure, and then treated with ultraviolet light. Among them, the irradiation intensity is 16A, and the ultraviolet irradiation time is 5min. The mass of nanomaterials in the dispersion is 5mg. Similarly, the prepared forward osmosis membrane is tested, and the average water flux of the forward osmosis membrane is 18.73 LMH, and the reverse solute flux is 0.88 gMH.

[0044] Embodiment 2 of the present invention: Based on the forward osmosis membrane preparation method in Comparative Example 1, the difference is that PCN-134-2D nanosheets and 5,10,15,20-tetrakis(4-carboxyphenyl)porphyrin are selected as the intermediate layer materials of the forward osmosis membrane, and the mixed solution A is filtered to the surface of the support layer by 0.04MPa pressure, and then treated with ultraviolet light. Among them, the irradiation intensity is 16A and the irradiation time is 5min. The mass of nanomaterials in the dispersion is 10mg. Similarly, the prepared forward osmosis membrane is tested, and the average water flux of the forward osmosis membrane is 29.41 LMH, and the reverse solute flux is 0.34 gMH.

[0045] Embodiment 3 of the present invention: Based on the forward osmosis membrane preparation method in Comparative Example 1, the difference is that PCN-134-2D nanosheets and 5,10,15,20-tetrakis(4-carboxyphenyl)porphyrin are selected as the intermediate layer materials of the forward osmosis membrane, and the mixed solution A is filtered to the surface of the support layer by 0.04MPa pressure, and then treated with ultraviolet light. Among them, the irradiation intensity is 16A and the irradiation time is 5min. The mass of nanomaterials in the dispersion is 15mg. Similarly, the prepared forward osmosis membrane is tested, and the average water flux of the forward osmosis membrane is 37.20 LMH, the reverse solute flux is 0.18 gMH, and the lithium ion recovery rate is 96.38%.

[0046] Embodiment 4 of the present invention: Based on the forward osmosis membrane preparation method in Comparative Example 1, the difference is that PCN-134-2D nanosheets and 5,10,15,20-tetrakis(4-carboxyphenyl)porphyrin are selected as the intermediate layer materials of the forward osmosis membrane, and the mixed solution A is filtered to the surface of the support layer by 0.04MPa pressure, and then treated with ultraviolet light. Among them, the irradiation intensity is 16A and the irradiation time is 5min. The mass of nanomaterials in the dispersion is 20mg. Similarly, the prepared forward osmosis membrane is tested, and the average water flux of the forward osmosis membrane is 27.67 LMH, and the reverse solute flux is 0.96 gMH.

[0047] Embodiment 5 of the present invention: Based on the forward osmosis membrane preparation method in Comparative Example 1, the difference is that PCN-134-2D nanosheets and 5,10,15,20-tetrakis(4-carboxyphenyl)porphyrin are selected as the intermediate layer materials of the forward osmosis membrane, and the mixed solution A is filtered to the surface of the support layer by 0.01MPa pressure, and then treated with ultraviolet light. Among them, the irradiation intensity is 16A and the irradiation time is 5min. The mass of nanomaterials in the dispersion is 15mg. Similarly, the prepared forward osmosis membrane is tested, and the average water flux of the forward osmosis membrane is 17.60 LMH, and the reverse solute flux is 1.03 gMH.

[0048] Embodiment 6 of the present invention: Based on the forward osmosis membrane preparation method in Comparative Example 1, the difference is that PCN-134-2D nanosheets and 5,10,15,20-tetrakis(4-carboxyphenyl)porphyrin are selected as the intermediate layer materials of the forward osmosis membrane, and the mixed solution A is filtered to the surface of the support layer by 0.06MPa pressure, and then treated with ultraviolet light. Among them, the irradiation intensity is 16A and the irradiation time is 5min. The mass of nanomaterials in the dispersion is 15mg. Similarly, the prepared forward osmosis membrane is tested, and the average water flux of the forward osmosis membrane is 28.56 LMH, and the reverse solute flux is 0.65 gMH.

[0049] Embodiment 7 of the present invention: Based on the forward osmosis membrane preparation method in Comparative Example 1, the difference is that PCN-134-2D nanosheets and 5,10,15,20-tetrakis(4-carboxyphenyl)porphyrin are selected as the intermediate layer materials of the forward osmosis membrane, and the mixed solution A is filtered to the surface of the support layer by using a 0.04MPa pressure. Among them, the mass of the nanomaterial in the dispersion is 15mg, and no ultraviolet light irradiation is added. Similarly, the prepared forward osmosis membrane was tested, and the average water flux of the forward osmosis membrane was 20.91 LMH, the reverse solute flux was 0.25 gMH, and the lithium ion recovery rate was 87.51%.

[0050] Embodiment 8 of the present invention: Based on the forward osmosis membrane preparation method in Comparative Example 1, the difference is that PCN-134-2D nanosheets and 5,10,15,20-tetrakis(4-carboxyphenyl)porphyrin are selected as the intermediate layer materials of the forward osmosis membrane, and the mixed solution A is filtered to the surface of the support layer by 0.04MPa pressure, and then treated with ultraviolet light. Among them, the irradiation intensity is 12A and the irradiation time is 5min. The mass of nanomaterials in the dispersion is 15mg. Similarly, the prepared forward osmosis membrane is tested, and the average water flux of the forward osmosis membrane is 22.46LMH, the reverse solute flux is 0.20 gMH, and the lithium ion recovery rate is 88.97%.

[0051] Embodiment 9 of the present invention: Based on the forward osmosis membrane preparation method in Comparative Example 1, the difference is that PCN-134-2D nanosheets and 5,10,15,20-tetrakis(4-carboxyphenyl)porphyrin are selected as the intermediate layer materials of the forward osmosis membrane, and the mixed solution A is filtered to the surface of the support layer by 0.04MPa pressure, and then treated with ultraviolet light. Among them, the irradiation intensity is 20A and the irradiation time is 5min. The mass of nanomaterials in the dispersion is 15mg. Similarly, the prepared forward osmosis membrane is tested, and the average water flux of the forward osmosis membrane is 26.23LMH, the reverse solute flux is 0.38 gMH, and the lithium ion recovery rate is 87.23%.

[0052] Embodiment 10 of the present invention: Based on the forward osmosis membrane preparation method in Comparative Example 1, the difference is that PCN-134-2D nanosheets and 5,10,15,20-tetrakis (4-carboxyphenyl) porphyrin are selected as the intermediate layer materials of the forward osmosis membrane, and the mixed solution A is filtered to the surface of the support layer by 0.04MPa pressure, and then treated with ultraviolet light. Among them, the irradiation intensity is 16A and the irradiation time is 1min. The mass of nanomaterials in the dispersion is 15mg. Similarly, the prepared forward osmosis membrane is tested, and the average water flux of the forward osmosis membrane is 25.36LMH, and the reverse solute flux is 0.26 gMH.

[0053] Embodiment 11 of the present invention: Based on the forward osmosis membrane preparation method in Comparative Example 1, the difference is that PCN-134-2D nanosheets and 5,10,15,20-tetrakis(4-carboxyphenyl)porphyrin are selected as the intermediate layer materials of the forward osmosis membrane, and the mixed solution A is filtered to the surface of the support layer by 0.04MPa pressure, and then treated with ultraviolet light. Among them, the irradiation intensity is 16A and the irradiation time is 8min. The mass of nanomaterials in the dispersion is 15mg. Similarly, the prepared forward osmosis membrane is tested, and the average water flux of the forward osmosis membrane is 29.89LMH, and the reverse solute flux is 1.87 gMH.

[0054] The detailed comparison of the test data of the forward osmosis membranes of Examples 1-11 is shown in Table 1.

[0055] type Mass of nanomaterials (g) Light intensity Lighting time Filtration pressure (Mpa) Water flux (LMH) Reverse solute flux (gMH) Lithium ion recovery rate (%) Comparative Example 1 - - - - 15.91 2.15 85.7 Example 1 5 16A 5min 0.04 18.73 0.88 - Example 2 10 16A 5min 0.04 29.41 0.34 - Example 3 15 16A 5min 0.04 37.20 0.18 96.38 Example 4 20 16A 5min 0.04 27.67 0.96 - Example 5 15 16A 5min 0.01 17.60 1.03 - Example 6 15 16A 5min 0.06 28.56 0.65 - Example 7 15 0A 0min 0.04 20.91 0.25 87.51 Example 8 15 12A 5min 0.04 22.46 0.20 88.97 Example 9 15 20A 5min 0.04 26.23 0.38 87.23 Example 10 15 16A 1min 0.04 25.36 0.26 - Embodiment 11 15 16A 8min 0.04 29.89 1.87 - See also Figure 2, the initial temperature of the membrane surface containing the intermediate layer material is only 25.4 degrees Celsius. Under different intensities of irradiation, the temperature of the membrane surface increases with the increase of current intensity, showing that the temperature change is the largest under the condition of current intensity of 20A. And according to the comparison between PCN-16A and Nylon-M0, it can be seen that the temperature change of the load material under illumination is 20.8℃ higher than that of Nylon-M0. This is mainly because the surface is doped with PCN-134-2D material and H4TCPP. Due to its own unique porphyrin structure, it has a wide range of light absorption capacity in the visible light region and has the ability to convert more light energy into heat energy. This feature also echoes the changes in the membrane surface structure caused by different light intensities. The increase in the membrane surface temperature is conducive to the formation of more ring structures on the membrane surface.

[0056] In summary, the present invention provides a light-assisted metal organic framework intermediate layer forward osmosis membrane, a preparation method and an application. An intermediate layer is constructed during the preparation process. The prepared forward osmosis membrane significantly improves the water flux, reduces the reverse solute flux, and improves the lithium ion recovery rate. On the surface of the nylon support layer, PCN-134-2D nanosheets and 5,10,15,20-tetrakis(4-carboxyphenyl)porphyrin are selected as the intermediate layer materials of the forward osmosis membrane, and interfacial polymerization is performed on the intermediate layer in light assistance to obtain a separation layer. Compared with traditional nanomaterial membranes, this intermediate layer can regulate the structure of the separation layer by changing the MPD retention and diffusion rate; in addition, by introducing the light-assisted method to prepare the forward osmosis membrane, the roughness of the separation layer and the degree of cross-linking of the polyamide can be further regulated by increasing the temperature of the intermediate layer to achieve better water permeability and selectivity. The comprehensive application of this multiple means provides new ideas and methods for further improvement and enhancement of forward osmosis membrane technology, and provides valuable references for the use of forward osmosis for lithium concentration and other precious and rare metal resource enrichment and recovery.

[0057] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a light-assisted metal organic framework intermediate layer forward osmosis membrane, characterized in that: The following steps are involved: The PCN-134-2D nanosheets were uniformly dispersed in deionized water, and 5,10,15,20-tetrakis(4-carboxyphenyl)porphyrin was added to obtain a mixed solution A; The mixed solution A is loaded on the surface of the nylon support layer by vacuum filtration to obtain an intermediate layer; The intermediate layer is irradiated under ultraviolet light conditions; and under ultraviolet light conditions, an aqueous monomer solution of m-phenylenediamine and an organic solution of trimesoyl chloride are added to the surface of the irradiated intermediate layer, respectively, so that the m-phenylenediamine and trimesoyl chloride undergo an interfacial polymerization reaction and form a separation layer, thereby obtaining a light-assisted metal organic framework intermediate layer forward osmosis membrane.

2. The method for preparing a light-assisted metal organic framework intermediate layer forward osmosis membrane according to claim 1, characterized in that: The mass ratio of PCN-134-2D nanosheets to 5,10,15,20-tetrakis(4-carboxyphenyl)porphyrin is (1~4):

1.

3. The method for preparing a light-assisted metal organic framework intermediate layer forward osmosis membrane according to claim 1, characterized in that: Interfacial polymerization reactions specifically include: An aqueous solution of meta-phenylenediamine monomer is added to the surface of the intermediate layer for soaking, and excess solution is removed after soaking to obtain a dried film; then an organic solution of trimesoyl chloride is added to the surface of the dried film for reaction, and excess solution is removed after the reaction, and thermal curing is performed at 40 ºC to 80 ℃ for 2 to 5 minutes to complete the interfacial polymerization reaction.

4. The method for preparing a light-assisted metal organic framework intermediate layer forward osmosis membrane according to claim 1, characterized in that: The steps for obtaining PCN-134-2D nanosheets include: Step 1: Preparation of PCN-134-2D precursor: The benzoic acid was dissolved in N,N-dimethylformamide, and after ultrasonication, zirconium tetrachloride, 1,3,5-tri(4-carboxyphenyl)benzene and ultrapure water were added, and after ultrasonication again, a mixed solution B was obtained; the mixed solution B was heated at 85°C to 175°C for 14 h to 52 h, and the supernatant was obtained by centrifugation and filtered, and then washed with N,N-dimethylformamide and methanol respectively to obtain a PCN-134-2D precursor; Step 2: Preparation of PCN-134-2D nanosheets: The PCN-134-2D precursor and 5,10,15,20-tetrakis(4-carboxyphenyl)porphyrin are uniformly dispersed in N,N-dimethylformamide to obtain a mixed solution C; the mixed solution C is continuously reacted at 80 ºC to 120 ºC for 8 to 12 h; the solid product is collected after centrifugation, and after alternately washing with N,N-dimethylformamide and acetone washing solution for 3 to 5 times, it is vacuum dried at 40 ºC to 80 ºC to obtain PCN-134-2D powder; after ultrasonic centrifugation, the supernatant is taken to obtain a PCN-134-2D dispersion; and then vacuum dried to obtain PCN-134-2D nanosheets.

5. The method for preparing a light-assisted metal organic framework intermediate layer forward osmosis membrane according to claim 4, characterized in that: In the mixed solution B, every (40-80) g of benzoic acid corresponds to (20-40) mL of N,N-dimethylformamide, (1-3) g of zirconium tetrachloride, (1-3) g of 1,3,5-tris(4-carboxyphenyl)benzene and (40-60) mL of ultrapure water; In mixed solution C, every (10 ~ 20) mg of PCN-134-2D precursor corresponds to (2 ~ 3) mmol of 5,10,15,20-tetrakis(4-carboxyphenyl)porphyrin and (3 ~ 5) mL of N,N-dimethylformamide.

6. The method for preparing a light-assisted metal organic framework intermediate layer forward osmosis membrane according to claim 1, characterized in that: The pressure of vacuum filtration is 0.01 Mpa ~ 0.06 Mpa; the ultraviolet light condition is provided by a xenon lamp, the irradiation intensity is 0 ~ 20 A, and the irradiation time is 1 min ~ 8 min, wherein the irradiation time of the middle layer is 25 ~ 35 seconds.

7. The method for preparing a light-assisted metal organic framework intermediate layer forward osmosis membrane according to claim 1, characterized in that: The steps of obtaining the aqueous phase monomer solution of m-phenylenediamine include: Dissolve m-phenylenediamine in deionized water to obtain an aqueous phase monomer solution of m-phenylenediamine, wherein the mass fraction of the aqueous phase monomer solution of m-phenylenediamine is 1.5 wt% to 3 wt%.

8. The method for preparing a light-assisted metal organic framework intermediate layer forward osmosis membrane according to claim 1, characterized in that: The steps of obtaining the organic phase solution of trimesoyl chloride include: The trimesoyl chloride is dissolved in n-hexane to obtain a trimesoyl chloride organic phase solution, wherein the mass fraction of the trimesoyl chloride organic phase solution is 0.2 wt% to 1 wt%.

9. A light-assisted metal organic framework intermediate layer forward osmosis membrane, characterized in that: The method is prepared according to any one of claims 1 to 8.