Silicon carbide doped calcium-based CO2 adsorbent and preparation method thereof
By introducing silicon carbide and microwave heating technology into calcium-based CO2 adsorbent, the problem of insufficient structural stability and wear resistance of calcium-based adsorbent during circulation is solved, and the efficient long-term recycling of adsorbent and CO2 adsorption performance of adsorbent is achieved. promote.
Patent Information
- Application Number
- CN202310605027.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-05-26
AI Technical Summary
The adsorption capacity of the calcium-based CO2 adsorbent decreases due to sintering and structural stability during the circulation process, and its wear resistance and strength under high temperature conditions are insufficient, making it difficult to meet the requirements of gasification or hydrogen production processes.
The preparation method of silicon carbide-doped calcium-based CO2 adsorbent is adopted. Silicon carbide is introduced as a support framework through in-situ reaction, combined with microwave heating and specific additive treatment, to improve the mechanical strength and structural stability of the adsorbent, and form a developed pore structure. To buffer volume changes.
It significantly improves the mechanical strength, chemical stability and thermal stability of the adsorbent, extends its circulation life, and improves the CO2 adsorption performance, and is suitable for high-temperature regeneration.
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of adsorption separation, and in particular relates to an adsorption material for adsorption separation of carbon dioxide and a preparation method thereof. Background Art
[0002] Calcium-based CO2 adsorbents, known for their fast adsorption rate, high capacity, low price, and ease of use, have attracted considerable attention as high-temperature adsorbents. They are not only the most promising adsorbent for industrial CO2 capture, but can also be applied to a variety of chemical processes involving or involving CO2, leveraging CO2 absorption or release to influence reaction equilibrium and alter reaction pathways. For example, in biomass gasification, methane hydrogen production, and ethanol reforming hydrogen production processes, the use of calcium-based CO2 adsorbents can increase hydrogen concentration, improve gas quality, and reduce costs and energy consumption.
[0003] The calcium-based CO2 adsorbent completes the CO2 adsorption and desorption cycle through the carbonation / calcination regeneration process. Since the Tamman temperature of CaCO3 is lower than the regeneration temperature of the calcium-based adsorbent, after multiple cycles, the adsorbent particles begin to sinter and fuse, resulting in a significant decrease in specific surface area and a rapid decrease in adsorption capacity. At the same time, the molar volume of CaCO3 is 36.9 cm 3 / mol, while CaO is 16.7cm 3 / mol, so during the cycle, the pores of the calcium-based adsorbent are easily collapsed due to local volume changes, and the structural stability is destroyed. For the above reasons, the carbonation conversion rate of the calcium-based adsorbent decays rapidly with the increase of the number of cycles. To address this problem, researchers often modify the adsorbent by doping with high-Taman temperature inert components such as Zr to provide a supporting skeleton for the adsorbent and alleviate its sintering. At the same time, they use hollow structures and other methods to control its morphology and maintain its structural characteristics. After the above modifications, the adsorption stability and structural stability of the calcium-based adsorbent are improved, but its strength improvement is limited, far from meeting the requirements for application in gasification or hydrogen production processes, especially in moving beds and fluidized beds.
[0004] CN109012008A discloses a method for preparing a calcium-based adsorbent by uniformly mixing a pretreated rare earth dopant powder with a calcined calcium-based precursor and grinding the mixture. This method produces a calcium-based CO2 adsorbent doped with rare earth waste. CN108499515A discloses a method for preparing a calcium-based adsorbent by pre-calcining a mixture of Li4SiO4, prepared using a high-temperature solid-phase method with Li2CO3 and fly ash or SiO2, and a calcium-based precursor derived from waste. This method produces a Li4SiO4-doped and modified calcium-based adsorbent. The above patents utilize direct mixing and doping methods to prepare calcium-based adsorbents, resulting in relatively weak mechanical strength, particularly high-temperature wear resistance. Summary of the Invention
[0005] To address the shortcomings of the prior art, the present invention provides a silicon carbide-doped calcium-based CO2 adsorbent and a method for preparing the same. The adsorbent exhibits wear resistance, high adsorption capacity, high microwave absorptivity, resistance to sintering and carbon deposition, and long-term cyclical use.
[0006] The present invention provides a method for preparing a silicon carbide-doped calcium-based CO2 adsorbent, the preparation method comprising the following steps:
[0007] (1) mixing the carbon source and the first auxiliary agent solution under contact conditions, then introducing the silicon source, and further drying and calcining to obtain the first material;
[0008] (2) mixing the calcium source, the solvent, and the first material obtained in step (1) under contact conditions, then introducing the second auxiliary agent, and drying to obtain the second material;
[0009] (3) Processing the second material obtained in step (2) under microwave conditions to obtain a silicon carbide-doped calcium-based CO2 adsorbent.
[0010] Furthermore, in the preparation method of the above-mentioned silicon carbide-doped calcium-based CO2 adsorbent, as a specific embodiment, the first auxiliary agent in step (1) is one or more of the nitrate, carbonate, phosphate, organic acid salt, and chloride of the first metal, wherein the first metal can be selected from one or more of aluminum, iron, magnesium, copper, silver, nickel, zirconium, cerium, lanthanum, yttrium, manganese, titanium, ytterbium, and neodymium; the first auxiliary agent is further preferably selected from one or more of aluminum nitrate, iron nitrate, magnesium nitrate, copper nitrate, silver nitrate, nickel nitrate, zirconium nitrate, cerium nitrate, lanthanum nitrate, yttrium nitrate, manganese nitrate, titanium tetrachloride, ytterbium nitrate, neodymium nitrate, basic aluminum acetate, magnesium acetate, magnesium oxalate, zirconium acetate, etc., and is further preferably one or more of aluminum nitrate, iron nitrate, magnesium nitrate, copper nitrate, silver nitrate, nickel nitrate, and zirconium nitrate.
[0011] Furthermore, in the preparation method of the above-mentioned silicon carbide-doped calcium-based CO2 adsorbent, as a specific embodiment, the solvent of the first auxiliary solution in step (1) is water and / or an organic solvent; the organic solvent is preferably an alcohol solvent, which can be specifically selected from one or more of ethanol, methanol, propanol, butanol, ethylene glycol, propylene glycol, glycerol, and butanediol, and is further preferably ethanol; when the solvent is a mixed solvent of water and an organic solvent, the concentration of the organic solvent is 1wt% to 80wt%.
[0012] Furthermore, in the preparation method of the above-mentioned silicon carbide-doped calcium-based CO2 adsorbent, as a specific embodiment, in step (1), before introducing the silicon source, the pH value of the material after mixing the carbon source and the first auxiliary agent solution can be preferably adjusted to 1 to 10. For example, the pH value can be adjusted by adding acid or ammonia water. The acid can be one or more of nitric acid, hydrochloric acid, phosphoric acid, oxalic acid, and citric acid.
[0013] Furthermore, in the preparation method of the above-mentioned silicon carbide-doped calcium-based CO2 adsorbent, as a specific embodiment, the carbon source in step (1) is one or more of monosaccharides, disaccharides, water-soluble polysaccharides, phenolic resins, water-soluble starches, dextrins, glycerol, furfural, and furfuryl alcohol, preferably sucrose and / or phenolic resin.
[0014] Furthermore, in the preparation method of the above-mentioned silicon carbide-doped calcium-based CO2 adsorbent, as a specific embodiment, the silicon source in step (1) is one or more of diatomaceous earth, white carbon black, mesoporous silica, nano-silica, and silica fume.
[0015] Furthermore, in the preparation method of the above-mentioned silicon carbide-doped calcium-based CO2 adsorbent, as a specific embodiment, based on the mass of the silicon source, the dry basis content of the first auxiliary agent is 0.01wt% to 10.0wt%, and the mass ratio of the carbon source to the silicon source is 0.3:1 to 10:1.
[0016] Furthermore, in the preparation method of the silicon carbide-doped calcium-based CO2 adsorbent, as a specific embodiment, the drying temperature in step (1) is 100-150°C.
[0017] Furthermore, in the preparation method of the above-mentioned silicon carbide-doped calcium-based CO2 adsorbent, as a specific embodiment, the calcination temperature in step (1) is 350-900°C, and the calcination time is 0.2-10 hours.
[0018] Furthermore, in the preparation method of the above-mentioned silicon carbide-doped calcium-based CO2 adsorbent, as a specific embodiment, the calcination in step (1) is carried out under an inert atmosphere and / or a reducing atmosphere, preferably under a reducing atmosphere; the inert atmosphere is nitrogen and / or an inert gas, and the inert gas is one or more of helium, neon, argon, krypton, and xenon. The reducing atmosphere is any one of a reducing gas and a mixed gas of a reducing gas and an inert atmosphere; the reducing gas is one or more of hydrogen, carbon monoxide, methane, and C2-C4 gas, preferably hydrogen and / or methane; the volume content of the reducing gas in the mixed gas is 0.5 to 100%. The inert atmosphere is nitrogen and / or an inert gas, and the inert gas is one or more of helium, neon, argon, krypton, and xenon.
[0019] Furthermore, in the preparation method of the silicon carbide-doped calcium-based CO2 adsorbent, as a specific embodiment, in step (1), solid-liquid separation is preferably performed before drying, and the separated solid phase material is dried.
[0020] Furthermore, in the preparation method of the above-mentioned silicon carbide-doped calcium-based CO2 adsorbent, as a specific embodiment, the calcium source in step (2) is one or more of calcium oxide, calcium hydroxide, and calcium salt, preferably one or more of calcium oxalate, calcium gluconate, calcium hydroxide, calcium oxide, calcium carbonate, calcium acetate, calcium propionate, calcium acetylacetonate, calcium lactate, calcium formate, calcium citrate, and calcium nitrate, and further preferably one or more of calcium oxalate, calcium oxide, and calcium nitrate.
[0021] Furthermore, in the preparation method of the above-mentioned silicon carbide-doped calcium-based CO2 adsorbent, as a specific embodiment, the solvent in step (2) is water and / or an organic solvent; the organic solvent is preferably an alcohol solvent, specifically one or more of ethanol, methanol, propanol, butanol, ethylene glycol, propylene glycol, glycerol, and butanediol, and ethanol is further preferred; when the solvent is a mixed solvent of water and an organic solvent, the concentration of the organic solvent is 1wt% to 80wt%.
[0022] Furthermore, in the preparation method of the above-mentioned silicon carbide-doped calcium-based CO2 adsorbent, as a specific embodiment, the second auxiliary agent in step (2) can be selected from one or more of carboxymethyl cellulose, hydroxyethyl cellulose, microcrystalline cellulose, chitosan, sesbania powder, hydroxypropyl methylcellulose, polyvinyl alcohol (molecular weight 0.5 to 150,000), silica sol, aluminum dihydrogen phosphate and their solutions, preferably one or more of carboxymethyl cellulose, sesbania powder, polyvinyl alcohol (molecular weight 0.5 to 150,000), silica sol and their solutions.
[0023] Furthermore, in the preparation method of the above-mentioned silicon carbide-doped calcium-based CO2 adsorbent, as a specific embodiment, in step (2), based on the mass of the calcium source, the mass ratio of the solvent to the calcium source is 0.2:1 to 20:1, the weight ratio of the first material to the calcium source is 0.01:1 to 2:1, and the dry basis content of the second auxiliary agent is 0.5wt% to 10wt%.
[0024] Furthermore, in the preparation method of the silicon carbide-doped calcium-based CO2 adsorbent, as a specific embodiment, in step (2), a molding process is preferably performed before drying. The molding technology is an existing technology well known to those skilled in the art. The specific molding operation can be selected by those skilled in the art according to actual needs. The shape can be any shape such as cylindrical strip, clover, four-leaf clover, sphere, etc., preferably spherical. The ball molding method can be one or more of extrusion ball molding, rolling molding, and spray drying molding.
[0025] Furthermore, in the preparation method of the above silicon carbide-doped calcium-based CO2 adsorbent, as a specific embodiment, the drying temperature in step (2) is 100-150°C.
[0026] Furthermore, in the preparation method of the above-mentioned silicon carbide-doped calcium-based CO2 adsorbent, as a specific embodiment, calcination treatment can also be carried out after drying in step (2), the calcination temperature is 350-900°C, the calcination time is 1-10 hours, and the calcination is carried out in the presence of an inert atmosphere, wherein the inert atmosphere is nitrogen and / or an inert gas, and the inert gas is one or more of helium, neon, argon, krypton, and xenon.
[0027] Furthermore, in the preparation method of the above-mentioned silicon carbide-doped calcium-based CO2 adsorbent, as a specific embodiment, the microwave heating treatment power in step (3) is 10-1000W / (g material), preferably 100-500W / (g material); the treatment time is 0.1 to 10 hours, preferably 0.1 to 1 hour; the microwave treatment is further preferably carried out in the presence of an inert gas, and the inert gas is one or more of helium, neon, argon, krypton, and xenon.
[0028] Furthermore, in the preparation method of the above-mentioned silicon carbide-doped calcium-based CO2 adsorbent, as a specific embodiment, the preparation method also includes step (4), wherein the material obtained in step (3) is subjected to heat treatment under oxygen-containing atmosphere conditions. The oxygen-containing atmosphere can be any one of air, oxygen, and a mixture of oxygen and an inert atmosphere, wherein the volume content of oxygen in the mixture is 5 to 99.99%; the inert atmosphere is nitrogen and / or an inert gas, wherein the inert gas is one or more of helium, neon, argon, krypton, and xenon. The heat treatment temperature is 500 to 1300°C, preferably 500 to 800°C, and the heat treatment time is 0.5 to 8 hours.
[0029] A second aspect of the present invention provides a silicon carbide-doped calcium-based CO2 adsorbent, wherein the silicon carbide-doped calcium-based CO2 adsorbent is obtained by the preparation method provided above.
[0030] Furthermore, in the above-mentioned silicon carbide-doped calcium-based CO2 adsorbent, as a specific embodiment, the silicon carbide-doped calcium-based CO2 adsorbent includes calcium oxide, silicon carbide, a compound of a first metal, and silicon dioxide. Based on the weight of the adsorbent, the silicon carbide content is 0.1 to 45 wt%, the first metal compound content is 0.01 to 5 wt%, and the silicon dioxide content is 0.01 to 5 wt%.
[0031] Compared with the prior art, the silicon carbide-doped calcium-based CO2 adsorbent and its preparation method provided by the present invention have the following advantages:
[0032] 1. The present invention provides a method for preparing a silicon carbide-doped calcium-based CO2 adsorbent. Silicon carbide, a high-Temperature inert component with excellent mechanical strength, chemical stability, and thermal stability, is introduced via an in-situ reaction. By doping and modifying CaO with silicon carbide, the silicon carbide acts as a supporting framework during subsequent high-temperature regeneration, effectively mitigating and preventing CaO sintering. This allows the CaO to maintain its optimal structural properties, enhance strength and wear resistance, and improve CO2 adsorption performance, facilitating the long-term recycling of the adsorbent.
[0033] 2. In the method for preparing the silicon carbide-doped calcium-based CO2 adsorbent provided by the present invention, the silicon source acts as a template to a certain extent, guiding the formation of the adsorbent's surface morphology while inhibiting the growth of active CaO particles. The carbon source also acts as a pore-forming agent to a certain extent, promoting the formation of a well-developed pore structure in the adsorbent. This buffers local volume changes during the adsorption and desorption cycles, ensuring the adsorbent's structural stability, and also helps increase the specific surface area and CO2 diffusion, thereby promoting CO2 adsorption.
[0034] 3. In the preparation method of silicon carbide-doped calcium-based CO2 adsorbent provided by the present invention, the first auxiliary agent part forms metal particles on the surface of the silicon source. First, the metal particles can interact strongly with microwaves, and the electromagnetic field can cause electron movement to generate induced eddy currents. The eddy currents are confined inside the medium, which will produce Joule heating effect and even trigger microwave discharge, which will cause the metal particles to heat up sharply and enhance the microwave selective heating effect; secondly, the metal particles can also be oxidized to generate inert components with high Tamman temperature, further alleviating and preventing the sintering of CaO particles; and at the same time, the introduction of metal active components (such as nickel, iron, cobalt, etc.) can catalyze the reaction between the carbon source and the silicon source, reduce the difficulty of silicon carbide synthesis, and regulate the structure and morphology of silicon carbide.
[0035] 4. In the method for preparing the silicon carbide-doped calcium-based CO2 adsorbent provided by the present invention, the material is heated under microwave conditions, and the hotspot effect, selective heating effect, and other non-thermal effects of microwaves are used to resolve the contradiction between the high temperature, difficult processing, and difficult forming of silicon carbide and the maintenance of the activity of CaO particles, thereby generating silicon carbide in situ. During the preparation process, carbon, metal particles, and newly generated silicon carbide form hotspots, which lower the reaction temperature and promote the rapid generation of silicon carbide and the formation of a supporting skeleton. The dielectric properties of carbon, metal particles, silicon carbide, and calcium oxide are very different. Carbon, metal particles, and silicon carbide are wave-absorbing materials, while calcium oxide is a wave-transmitting material. In a microwave field, the heating rates of the former three are much greater than those of the latter. This selective heating helps to overcome the problem of the growth of active CaO particles caused by the higher generation temperature of silicon carbide. DETAILED DESCRIPTION
[0036] The specific content and effects of the method of the present invention are further described below by way of specific examples, but the scope of the present invention is not limited thereby. In the present invention, the molecular weight of the polyvinyl alcohol is the viscosity average molecular weight.
[0037] The specific embodiments of the present invention are described in detail below. However, it should be noted that the protection scope of the present invention is not limited by these specific embodiments, but is determined by the claims in the appendix.
[0038] All publications, patent applications, patents, and other references mentioned in this specification are incorporated herein by reference. Unless otherwise defined, all technical and scientific terms used in this specification have the meanings commonly understood by those skilled in the art. In the event of conflict, the definitions in this specification will prevail.
[0039] When this specification uses the prefix "well known to those skilled in the art", "prior art" or similar terms to introduce materials, substances, methods, steps, devices or components, the objects introduced by the prefix include those commonly used in the art when this application is filed, but also include those that are not commonly used at present but will become generally recognized in the art to be suitable for similar purposes.
[0040] Unless otherwise expressly indicated, throughout the specification and claims, the term "comprise" or variations thereof such as "comprises" or "comprising" will be understood to include the elements or components stated without excluding other elements or other components. In this document, all numerical values of parameters (e.g., quantities or conditions) are to be understood as being modified in all instances by the term "about", regardless of whether "about" actually appears before the numerical value.
[0041] Unless otherwise specified, all percentages, parts, ratios, etc. mentioned in this specification are based on weight and pressure is gauge pressure.
[0042] In the context of this specification, any two or more embodiments of the present invention may be arbitrarily combined, and the technical solutions thus formed belong to part of the original disclosure of this specification and also fall within the scope of protection of the present invention.
[0043] In the following examples and comparative examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or those recommended by the manufacturer. All reagents and instruments used, if no manufacturer is specified, are commercially available conventional products.
[0044] Example 1
[0045] Sucrose and aluminum nitrate were slowly added to deionized water containing 5% ethanol, with rapid stirring. The pH was adjusted to 1 with nitric acid, and then nano-silica was slowly added. The aluminum nitrate content was 10%, and the mass ratio of sucrose to nano-silica was 6:1, based on the mass of the nano-silica. The mixture was dried at 120°C and then kept constant at 600°C in a hydrogen atmosphere for 2 hours to obtain a first material.
[0046] Calcium oxalate is slowly added to deionized water containing 1% ethanol, stirred rapidly, and then the first material is slowly added, followed by the sesbania powder and silica sol. The mass ratio of the solvent to calcium oxalate is 10:1, the weight ratio of the first material to calcium oxalate is 0.25:1, the dry basis content of the sesbania powder is 5%, and the dry basis content of the silica sol is 0.5%. The above materials are prepared into microspheres, dried at 120°C, and then kept at a constant temperature of 600°C in a nitrogen atmosphere for 3 hours. The above materials are sent to a microwave roasting furnace and treated at a power of 500W / (g material) in an argon atmosphere for 1 hour. The above materials are kept at a constant temperature of 600°C in an air atmosphere for 2 hours to obtain a calcium-based CO2 adsorbent.
[0047] Example 2
[0048] Starch and ferric nitrate were slowly added to deionized water containing 20% methanol, with rapid stirring. The pH was adjusted to 3 with phosphoric acid, and then mesoporous silica was slowly added. The ferric nitrate content was 1%, based on the mass of the mesoporous silica, and the starch to mesoporous silica mass ratio was 2:1. The mixture was separated into solid and liquid, dried at 150°C, and then heated at 900°C in an ethane atmosphere for 1 hour to obtain the first material.
[0049] Calcium acetylacetonate is slowly added to deionized water containing 80% methanol, stirred rapidly, and then the first material is slowly added, followed by the slow addition of aluminum dihydrogen phosphate. The mass ratio of the solvent to calcium acetylacetonate is 20:1, the weight ratio of the first material to calcium acetylacetonate is 0.1:1, and the dry basis content of aluminum dihydrogen phosphate is 0.5%. The above materials are prepared into microspheres, dried at 150°C, and then kept at a constant temperature of 350°C in a nitrogen atmosphere for 10 hours. The above materials are sent to a microwave roasting furnace and treated at a power of 1000W / (g material) for 0.5 hours in an argon atmosphere. The above materials are kept at a constant temperature of 650°C in a nitrogen atmosphere containing 50% oxygen for 1 hour to obtain a calcium-based CO2 adsorbent.
[0050] Example 3
[0051] Fructose and magnesium nitrate were slowly added to deionized water with rapid stirring, followed by the slow addition of silica. The magnesium nitrate content was 3% based on the mass of silica, and the mass ratio of fructose to silica was 10:1. The mixture was dried at 100°C and then held at 600°C in a methane atmosphere for 4 hours to obtain a first material.
[0052] Calcium nitrate is slowly added to deionized water, stirred rapidly, and then the first material is slowly added, followed by the sesbania powder and polyvinyl alcohol (average molecular weight of 22,000). The mass ratio of the solvent to calcium nitrate is 5:1, the weight ratio of the first material to calcium nitrate is 0.5:1, the dry basis content of the sesbania powder is 2%, and the dry basis content of the polyvinyl alcohol (average molecular weight of 22,000) is 2%. The above materials are prepared into microspheres, dried at 120°C, and then kept at a constant temperature of 700°C in a nitrogen atmosphere for 1 hour. The above materials are sent to a microwave roasting furnace and treated at a power of 800W / (g material) for 0.5 hour in an argon atmosphere. The above materials are kept at a constant temperature of 800°C in an air atmosphere for 1 hour to obtain a calcium-based CO2 adsorbent.
[0053] Example 4
[0054] Phenolic resin and zirconium nitrate were slowly added to deionized water containing 65% ethanol, with rapid stirring. The pH was adjusted to 5 with oxalic acid, and diatomaceous earth was then slowly added. The zirconium nitrate content was 5%, based on the mass of the diatomaceous earth, and the mass ratio of phenolic resin to diatomaceous earth was 6:1. The mixture was dried at 120°C and then held at 600°C in a hydrogen atmosphere for 8 hours to obtain a first material.
[0055] Calcium oxide is slowly added to deionized water containing 15% ethanol, stirred rapidly, and then the first material is slowly added, followed by the carboxymethyl cellulose and silica sol. Wherein, based on the mass of calcium oxide, the mass ratio of the solvent to calcium oxide is 15:1, the weight ratio of the first material to calcium oxide is 1.8:1, the dry basis content of carboxymethyl cellulose is 5%, and the dry basis content of silica sol is 0.5%. The above materials are prepared into microspheres, dried at 120°C, and then kept at a constant temperature of 800°C in a nitrogen atmosphere for 1 hour. The above materials are sent to a microwave roasting furnace and treated at a power of 100W / (g material) for 3 hours in an argon atmosphere. The above materials are kept at a constant temperature of 350°C in an oxygen atmosphere for 8 hours to obtain a calcium-based CO2 adsorbent.
[0056] Comparative Example 1
[0057] Sucrose was slowly added to deionized water containing 5% ethanol, with rapid stirring. The pH was adjusted to 1 with nitric acid, and then nano-silica was slowly added. The mass ratio of sucrose to nano-silica was 6:1 based on the mass of the nano-silica. The mixture was dried at 120°C and then kept at 600°C in a hydrogen atmosphere for 2 hours to obtain a first material.
[0058] Calcium oxalate is slowly added to deionized water containing 1% ethanol, stirred rapidly, and then the first material is slowly added, followed by the sesbania powder and silica sol. The mass ratio of the solvent to calcium oxalate is 10:1, the weight ratio of the first material to calcium oxalate is 0.25:1, the dry basis content of the sesbania powder is 5%, and the dry basis content of the silica sol is 0.5%. The above materials are prepared into microspheres, dried at 120°C, and then kept at a constant temperature of 600°C in a nitrogen atmosphere for 3 hours. The above materials are sent to a microwave roasting furnace and treated at a power of 500W / (g material) in an argon atmosphere for 1 hour. The above materials are kept at a constant temperature of 600°C in an air atmosphere for 2 hours to obtain a calcium-based CO2 adsorbent.
[0059] Comparative Example 2
[0060] SiC micropowder, aluminum oxide, yttrium oxide, and carbon black are mixed and ground to obtain a first material, wherein the aluminum oxide accounts for 5%, the yttrium oxide accounts for 2%, and the carbon black accounts for 10%, based on the mass of the SiC micropowder.
[0061] Calcium oxalate is slowly added to deionized water containing 1% ethanol, stirred rapidly, and then the first material is slowly added, followed by the sesbania powder and silica sol. The mass ratio of the solvent to calcium oxalate is 5:1, the weight ratio of the first material to calcium oxalate is 0.15:1, the dry basis content of the sesbania powder is 5%, and the dry basis content of the silica sol is 0.5%. The above materials are prepared into microspheres, dried at 120°C, and then kept at a constant temperature of 600°C in a nitrogen atmosphere for 3 hours. The above materials are sent to a microwave roasting furnace and treated at a power of 500W / (g material) in an argon atmosphere for 3 hours. The above materials are kept at a constant temperature of 600°C in an air atmosphere for 2 hours to obtain a calcium-based CO2 adsorbent.
[0062] Comparative Example 3
[0063] Sucrose and aluminum nitrate were slowly added to deionized water containing 5% ethanol, with rapid stirring. The pH was adjusted to 1 with nitric acid, and then nano-silica was slowly added. The aluminum nitrate content was 10%, and the mass ratio of sucrose to nano-silica was 6:1, based on the mass of the nano-silica. The mixture was dried at 120°C and then kept constant at 600°C in a hydrogen atmosphere for 2 hours to obtain a first material.
[0064] Calcium oxalate was slowly added to deionized water containing 1% ethanol with rapid stirring. The first material was then slowly added, followed by the sesbania powder and silica sol. The mass ratio of the solvent to calcium oxalate was 10:1, the weight ratio of the first material to calcium oxalate was 0.25:1, the dry basis content of the sesbania powder was 5%, and the dry basis content of the silica sol was 0.5%. The above materials were prepared into microspheres, dried at 120°C, and then heated at 1700°C in an argon atmosphere for 7 hours. The above materials were then heated at 600°C in an air atmosphere for 2 hours to obtain a calcium-based CO2 adsorbent.
[0065] Adsorbent performance evaluation:
[0066] The mass wear rate of the calcium-based CO2 adsorbents prepared in Examples 1-4 and Comparative Examples 1-3 was measured using a KM-5A particle wear tester at a speed of 25 r / min and a test time of 10 h. The results are shown in Table 1:
[0067] Table 1 Mass wear rate of adsorbent
[0068] catalyst Mass wear rate / % Example 1 0.62 Example 2 0.51 Example 3 0.43 Example 4 0.39 Comparative Example 1 2.35 Comparative Example 2 0.49 Comparative Example 3 0.57
[0069] The CO2 adsorption capacity of the calcium-based CO2 adsorbents prepared in Examples 1-4 and Comparative Examples 1-3 was measured using a thermogravimetric analyzer (TGA). The measurement conditions were: adsorption temperature of 650°C, desorption temperature of 800°C, 100 cycles, and the average value was taken. The results are shown in Table 2:
[0070] Table 2 CO2 adsorption capacity of adsorbents
[0071] catalyst <