Cationic MOFs (metal organic frameworks) material as well as preparation method and application thereof
By preparing cationic MOFs material UiO-66-2,5-2NH2·HCl in aqueous solution, the problems of high toxicity, instability and low separation efficiency of perrhenate adsorption removal method are solved, and efficient and environmentally friendly adsorption effect is achieved , the adsorption capacity and stability are significantly improved.
Patent Information
- Application Number
- CN202411429888.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-14
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing perrhenate adsorption and removal methods have problems of high toxicity, instability and low separation efficiency. The traditional method uses organic solvents, which are complex in operation and high in cost.
Using water as a solvent, 2,5-diaminoterephthalic acid and octahydro zirconium chloride were reacted in aqueous solution to prepare the cationic MOFs material UiO-66-2,5-2NH2·HCl, which was added by protonation treatment. Amino active sites and positive electrical properties improve adsorption capacity.
It has achieved efficient adsorption of perrhenate, with excellent chemical stability, thermal stability and anti-ion interference capability, with an adsorption capacity of up to 580-620mg/g, and the equilibrium time can be reached within 200 minutes. Kinetic adsorption complies with the secondary kinetics Model and preparation process is environmentally friendly and economical.
Smart Images

Figure CN119016038A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nanoporous materials, and in particular to a cationic MOFs material and a preparation method and application thereof, and in particular to the use of the material for adsorption and removal of perrhenate. Background Art
[0002] technetium -99 ( 99 Tc) is a major radioactive isotope in nuclear waste, which poses a great threat to human health and the natural environment. Excessive exposure to 99 Tc environment can cause cancer, ulcers and other diseases. In oxygenated aqueous solution, 99 Tc is mainly present in the form of pertechnetate, i.e. 99 TcO4 - The oxidized form exists stably. 99 TcO4 - It has the characteristics of high water solubility and high volatility, and migrates quickly in the environment and easily enters the food chain, thus causing serious harm to the survival of humans and animals. 99 TcO4 - It is of great significance. 99 TcO4 - The radioactivity of ReO4 limits its use in laboratory research. - Thermodynamic parameters, charge density, stereochemical structure and other properties of 99 TcO4 - Very similar, so usually use non-radioactive perrhenate (ReO4 - )replace 99 TcO4 - , and conduct laboratory adsorption and removal research. - The removal methods include ion exchange, bioreduction, supramolecular recognition, chemical reduction, solvent extraction and bioreduction, etc. However, these methods have the disadvantages of using a large amount of toxic organic matter, long operation time, chemical and thermal instability of materials and low separation efficiency. Therefore, it is urgent to develop advanced technologies and functional materials to capture ReO4 from polluted water. - Among them, the adsorption method has been widely used in sewage treatment due to its convenience and simplicity. The key lies in the design and construction of adsorption materials with high adsorption capacity and good selective separation performance.
[0003] At present, many adsorbents have been studied and developed in liquid phase adsorption, including layered double hydroxide (LDH), activated carbon (AC), biomaterials, resins, metal-organic framework materials (MOFs), etc. Among these adsorbents, MOFs have high chemical stability, thermal stability and water stability, and thus show great potential. Based on this, according to the characteristics of perrhenate anions, the internal structure of MOF materials is regulated to increase their active sites, which can improve the removal rate of perrhenate. Summary of the invention
[0004] The present invention provides a cationic MOFs material, which is a high-density amino-functionalized MOFs material, has a high adsorption capacity for perrhenate, and can solve the shortcomings of traditional adsorption methods such as high toxicity, instability and low separation efficiency; the preparation method provided by the present invention uses water as a solvent, which solves the problem of using organic solvents in traditional methods, and has the advantages of simple operation, economic savings, etc.
[0005] To achieve the above objectives, the technical solution of the present invention is as follows:
[0006] A method for preparing a cationic MOFs material comprises the following steps:
[0007] S1. Dissolve 2,5-diaminoterephthalic acid and zirconium oxychloride octahydrate in H2O solvent, add a regulator, reflux at 95-115°C for 24-30h, cool to room temperature, wash with deionized water and ethanol for multiple times, collect solids by centrifugation, and dry at 95-105°C to obtain UiO-66-2,5-2NH2;
[0008] S2. After activating the UiO-66-2,5-2NH2 prepared in step S1, soak it in a hydrochloric acid solution for 4 to 5 hours for reaction, collect the solid by centrifugation, and dry it at 98 to 102° C. to obtain UiO-66-2,5-2NH2·HCl, which is the cationic MOFs material.
[0009] Wherein, the molar ratio of 2,5-diaminoterephthalic acid to zirconium oxychloride octahydrate in step S1 is 1:(0.85-1.27), preferably 1:1.04;
[0010] The concentration of the 2,5-diaminoterephthalic acid in the H2O solvent is 0.205-0.306 mmol / mL, preferably 0.25 mmol / mL;
[0011] The regulator is one of acetic acid, formic acid or propionic acid, preferably acetic acid;
[0012] The volume ratio of the H2O solvent to the regulator is 1:(1.64-2.44), preferably 1:2;
[0013] Wherein, the concentration of HCl in the hydrochloric acid solution in step S2 is 1.8-2.2M, preferably 2M;
[0014] The concentration of UiO-66-2,5-2NH2 in the hydrochloric acid solution is 4.1-6.1 mg / mL, preferably 5 mg / mL.
[0015] 2,5-Diaminoterephthalic acid has low solubility in H2O solvent. The traditional method is to use DMF as a solvent to dissolve 2,5-diaminoterephthalic acid. The preparation method provided by the present invention uses a small amount of water as a solvent, and the organic ligand reacts with the metal salt in a semi-liquid and semi-solid state to assemble and generate a diamino MOF. The high concentration of organic ligand 2,5-diaminoterephthalic acid in the reaction system can fully coordinate with the metal salt Zr, so that the MOF material successfully introduces amino active functional groups and increases amino active sites; after using HCl for protonation engineering treatment, the -NH2 functional group is converted into -NH3 + In addition, acid treatment can convert μ-OH groups into [μ-OH2] + To improve the stability of the μ-OH group, the acid protonation engineering can finally make the MOF surface extremely positively charged.
[0016] Another object of the present invention is to provide a cationic MOFs material prepared by the above preparation method, namely, UiO-66-2,5-2NH2·HCl material, which has a specific surface area of 215 to 260 m 2 / g, and the average pore size is 4.7 to 5.8 angstroms.
[0017] The third object of the present invention is to provide an application of the cationic MOFs material, especially its use in adsorbing and removing perrhenate, and its adsorption capacity for perrhenate is 580-620 mg / g.
[0018] Compared with the prior art, the present invention has the following advantages:
[0019] 1. A high-density amino functional group was constructed in the UiO-66-2,5-2NH2 material. From the perspective of functional group functionalized materials, a high-density protonated amino functionalized UiO-66-2,5-2NH2·HCl material was prepared through protonation engineering. A large number of adsorption sites were introduced into the material. After protonation engineering treatment, the surface of the material has a strong positive charge, which can realize the adsorption of anion ReO4 - The adsorption process can be well described by the Langmuir isotherm model. The adsorption can reach equilibrium in about 200 minutes. The kinetic adsorption process can be well described by the second-order kinetic model.
[0020] 2. The adsorbent has excellent chemical stability and thermal stability, good resistance to ion interference and adsorption-desorption regeneration and recycling capabilities.
[0021] 3. A small amount of water is used as solvent in the preparation process, replacing traditional organic solvents, which is economical and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is the structural diagram of UiO-66-2,5-2NH2·HCl;
[0023] Figure 2 (a) is the scanning electron microscopy image of UiO-66-2,5-2NH2; Figure 2 (b) is the SEM image of UiO-66-2,5-2NH2·HCl;
[0024] Figure 3 (a) is a high-magnification transmission electron microscopy image of UiO-66-2,5-2NH2; Figure 3 (b) is a high-magnification transmission electron microscopy image of UiO-66-2,5-2NH2·HCl;
[0025] Figure 4 (a) is the PXRD spectrum of UiO-66-2,5-2NH2·HCl; Figure 4 (b) is the infrared spectrum of UiO-66-2,5-2NH2·HCl;
[0026] Figure 5 (a) is the BET specific surface area spectrum of UiO-66-2,5-2NH2·HCl; Figure 5 (b) is the pore size distribution diagram of UiO-66-2,5-2NH2·HCl;
[0027] Figure 6 is the zeta potential diagram of UiO-66-2,5-2NH2·HCl;
[0028] Figure 7 (a) is the TGA curve of UiO-66-2,5-2NH2·HCl; Figure 7 (b) is the XRD pattern of UiO-66-2,5-2 after immersion in NH2·HCl solutions with different pH values;
[0029] Figure 8 (a) is the adsorption isotherm of UiO-66-2,5-2NH2·HCl; Figure 8 (b) is the fitting diagram of nonlinear Langmuir and Freundlich isotherm models;
[0030] Fig. 9It is the adsorption kinetics curve of UiO-66-2,5-2NH2·HCl;
[0031] Fig.10 (a) is the first-order adsorption kinetics fitting curve of UiO-66-2,5-2NH2·HCl; Fig.10 (b) is the second-order kinetic fitting curve of UiO-66-2,5-2NH2·HCl;
[0032] Fig.11 The reaction of UiO-66-2,5-2NH2·HCl with ReO4 under the condition of coexisting ions - Adsorption capacity diagram of
[0033] Fig.12 It is the adsorption-desorption cycle performance diagram of UiO-66-2,5-2NH2·HCl;
[0034] Fig.13 UiO-66-2,5-2NH2·HCl to ReO4 - Theoretical calculation diagram of adsorption DTF. DETAILED DESCRIPTION
[0035] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solution of the invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] Example 1
[0037] A method for preparing a cationic MOFs material comprises the following steps:
[0038] S1. Add 2.5 mmol of 2,5-diaminoterephthalic acid and 2.6 mmol of zirconium chloride octahydrate into 10 mL of H2O solvent, add 20 mL of acetic acid, reflux at 105°C for 24 h, cool to room temperature after the reaction, wash with deionized water and ethanol several times, collect the solid by centrifugation, and dry in a vacuum blower drying oven at 100°C to prepare UiO-66-2,5-2NH2, which is characterized by Figure 2 (a) and Figure 3 (a);
[0039] S2, after activating 50 mg of UiO-66-2,5-2NH2 prepared in step S1, soak it in 10 mL of hydrochloric acid solution for 4 h for reaction, wherein the concentration of HCl is 2 M, collect the solid by centrifugation, and dry it in a vacuum blower drying oven at 100 ° C to obtain UiO-66-2,5-2NH2·HCl, which is a cationic MOFs material. The specific surface area of the prepared cationic MOFs material is 238 m 2 / g, with an average pore size of 5.2 angstroms. Its structure is shown in Figure 1 , see Figure 2 (b) Figure 3 (b) Figure 4 , Figure 5 , Figure 6 and Figure 7 .
[0040] Example 2
[0041] A method for preparing a cationic MOFs material comprises the following steps:
[0042] S1. Add 2.25 mmol of 2,5-diaminoterephthalic acid and 2.34 mmol of zirconium oxychloride octahydrate to 11 mL of H2O solvent, add 18 mL of acetic acid, reflux at 95°C for 26 h, cool to room temperature after the reaction, wash with deionized water and ethanol several times, collect the solid by centrifugation, and dry in a vacuum blower drying oven at 95°C to prepare UiO-66-2,5-2NH2;
[0043] S2, after activating 45 mg of UiO-66-2,5-2NH2 prepared in step S1, soak it in 11 mL of hydrochloric acid solution for 5 h for reaction, wherein the HCl concentration is 1.8 M, collect the solid by centrifugation, and dry it in a vacuum blower drying oven at 98 ° C to obtain UiO-66-2,5-2NH2·HCl, which is a cationic MOFs material. The specific surface area of the obtained cationic MOFs material is 215 m 2 / g, and the average pore size is 4.7 angstroms.
[0044] Example 3
[0045] A method for preparing a cationic MOFs material comprises the following steps:
[0046] S1. Add 2.75 mmol of 2,5-diaminoterephthalic acid and 2.86 mmol of zirconium oxychloride octahydrate into 9 mL of H2O solvent, add 22 mL of acetic acid, reflux at 115°C for 30 h, cool to room temperature after the reaction, wash with deionized water and ethanol several times, collect the solid by centrifugation, and dry in a vacuum blower drying oven at 105°C to prepare UiO-66-2,5-2NH2;
[0047] S2, after activating 55 mg of UiO-66-2,5-2NH2 prepared in step S1, soak it in 9 mL of hydrochloric acid solution for 4.5 h for reaction, wherein the HCl concentration is 2.2 M, collect the solid by centrifugation, and dry it in a vacuum blower drying oven at 102 ° C to obtain UiO-66-2,5-2NH2·HCl, which is a cationic MOFs material. The specific surface area of the obtained cationic MOFs material is 260 m 2 / g, and the average pore size is 5.8 angstroms.
[0048] Example 4
[0049] A method for preparing a cationic MOFs material comprises the following steps:
[0050] S1. Add 2.3 mmol of 2,5-diaminoterephthalic acid and 2.72 mmol of zirconium oxychloride octahydrate into 10 mL of H2O solvent, add 19 mL of formic acid, reflux at 105°C for 28 h, cool to room temperature after the reaction, wash with deionized water and ethanol several times, collect the solid by centrifugation, and dry in a vacuum blower drying oven at 102°C to prepare UiO-66-2,5-2NH2;
[0051] S2, after activating 52 mg of UiO-66-2,5-2NH2 prepared in step S1, soak it in 10 mL of hydrochloric acid solution for 4 h for reaction, wherein the HCl concentration is 2.1 M, collect the solid by centrifugation, and dry it in a vacuum blower drying oven at 100 ° C to obtain UiO-66-2,5-2NH2·HCl, which is a cationic MOFs material. The specific surface area of the obtained cationic MOFs material is 246 m 2 / g, and the average pore size is 5.2 angstroms.
[0052] Example 5
[0053] A method for preparing a cationic MOFs material comprises the following steps:
[0054] S1. Add 2.63 mmol of 2,5-diaminoterephthalic acid and 2.5 mmol of zirconium oxychloride octahydrate into 10 mL of H2O solvent, add 21 mL of propionic acid, reflux at 95°C for 24 h, cool to room temperature after the reaction, wash with deionized water and ethanol several times, collect the solid by centrifugation, and dry in a vacuum blower drying oven at 98°C to prepare UiO-66-2,5-2NH2;
[0055] S2, after activating 48 mg of UiO-66-2,5-2NH2 prepared in step S1, soak it in 10 mL of hydrochloric acid solution for 5 h for reaction, wherein the HCl concentration is 1.9 M, collect the solid by centrifugation, and dry it in a vacuum blast drying oven at 100 ° C to obtain UiO-66-2,5-2NH2·HCl, which is a cationic MOFs material. The specific surface area of the obtained cationic MOFs material is 224 m 2 / g, and the average pore size is 5.1 angstroms.
[0056] Test Example 1
[0057] Testing the removal of ReO4 by adsorption of UiO-66-2,5-2NH2·HCl - : Take 5 mg of UiO-66-2,5-2NH2·HCl prepared in Example 1, add it to 10 mL of sodium perrhenate solution with an initial mass concentration of 0-1500 mg / L and a certain pH condition, oscillate and adsorb under certain temperature conditions, take samples, and conduct inductively coupled plasma (Inductively Coupled Plasma) to the ReO4 in the solution. - The concentration of UiO-66-2,5-2NH2·HCl to ReO4 - The adsorption amount.
[0058] UiO-66-2,5-2NH2·HCl to ReO4 - The adsorption isotherm of Figure 8 (a), it can be seen from the figure that UiO-66-2,5-2NH2·HCl in ReO4 - Concentration range of 100-1500mg / L for ReO4 - The maximum adsorption capacity of UiO-66-2,5-2NH2·HCl on ReO4 - The adsorption isotherm model is shown in Figure 8 (b), The fitting results show that the adsorption process is more consistent with the Langmuir isotherm model.
[0059] UiO-66-2,5-2NH2·HCl adsorption of ReO4 - The kinetic curve of Fig. 9 As can be seen from the figure, when ReO4 - When the initial concentration of UiO-66-2,5-2NH2·HCl was low (50 mg / L), the effect of UiO-66-2,5-2NH2·HCl on ReO4 - The adsorption of ReO4 can reach equilibrium in a short time, and the equilibrium time is about 30 minutes. -When the initial concentration of ReO4 was high (500 mg / L), the adsorption reached equilibrium at about 240 mins. - It has a faster adsorption and removal rate. Its kinetic adsorption fitting data can be found in Fig.10 The fitting results show that ReO4 - The kinetic adsorption of ReO4 on UiO-66-2,5-2NH2·HCl is more consistent with the second-order kinetic model. - Theoretical calculation of adsorption DTF is shown in Fig.13 .
[0060] Test Example 2
[0061] Test the different interfering ions in water for ReO4 - Effect of adsorption amount: 5 mg of UiO-66-2,5-2NH2·HCl prepared in Example 1 was added to ReO4 - The mass concentration is 100mg / L and contains NO3 - 、ClO4 - , Cl - Br - ,I - In the interfering ion solution, the concentration of interfering ions was 100 mg / L, and adsorption was performed at 30 °C for 24 h. The calculated results showed that UiO-66-2,5-2NH2·HCl had a strong affinity for ReO4. - The adsorption amount.
[0062] Effect of UiO-66-2,5-2NH2·HCl on ReO4 in the presence of different interfering ions - The adsorption amount is shown in Fig.11 As can be seen from the figure, the order of influence of interfering ions is NO3 - >ClO4 - >Cl - >Br - >I - The adsorption amounts were 88.9%, 89.7%, 92.1%, 92.9% and 94.2% of those without interfering ions. - The main reason for the impact may be NO3 - It is triangular, and the N atom can easily obtain electrons; ClO4 - It is a regular tetrahedron with good symmetry, and its electron-acquisition ability is weaker than that of NO3. - ; For I - Br - and Cl - , the order of acquiring electron ability is Cl - >Br - >I- , the order of ionic radius is Cl - <Br - - , therefore, Cl - It is easier to diffuse into the pores of the adsorbent and compete for the adsorption sites. However, even in the presence of interfering ions, UiO-66-2,5-2NH2·HCl has a strong affinity for ReO4 - The adsorption amount is still higher than that of most reported adsorbents, indicating that UiO-66-2,5-2NH2·HCl can be used as a potential perrhenate adsorbent.
[0063] Test Example 3
[0064] Elution experiment: HNO3 solution was selected as the eluent to adsorb ReO4 - The UiO-66-2,5-2NH2·HCl was immersed in 0.01M HNO3 solution for 24h, and then the solid was collected, washed with methanol, and dried at 80℃ for 24h. After four cycles, UiO-66-2,5-2NH2·HCl had a significant effect on the performance of ReO4 - The adsorption amount is shown in Fig.12 After four cycles, UiO-66-2,5-2NH2·HCl reacts with ReO4 - The adsorption capacity can still reach 106.4 mg / g, indicating that UiO-66-2,5-2NH2·HCl has good cyclic desorption of ReO4 - potential.
[0065] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present invention and to form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present invention and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.
Claims
1. A method for preparing a cationic MOFs material, characterized in that: The following steps are involved: S1. Dissolve 2,5-diaminoterephthalic acid and zirconium oxychloride octahydrate in H2O solvent, add a regulator, reflux reaction, cool to room temperature, wash, centrifuge to collect solids, and dry to obtain UiO-66-2,5-2NH2; S2. After activating UiO-66-2,5-2NH2, immersing it in a hydrochloric acid solution for reaction, collecting the solid by centrifugation and drying it, so as to obtain UiO-66-2,5-2NH2·HCl, which is the cationic MOFs material.
2. The preparation method according to claim 1, characterized in that: The molar ratio of 2,5-diaminoterephthalic acid to zirconium oxychloride octahydrate in step S1 is 1:(0.85-1.27); the concentration of 2,5-diaminoterephthalic acid in H2O solvent is 0.205-0.306 mmol / mL; the regulator is one of acetic acid, formic acid or propionic acid; The volume ratio of the H2O solvent to the regulator is 1:(1.64-2.44).
3. The preparation method according to claim 1, characterized in that: In step S1, the reflux reaction temperature is 95-115°C, and the reflux reaction time is 24-30h; the washing is performed by using deionized water and ethanol for multiple washings; and the drying temperature is 95-105°C.
4. The preparation method according to claim 1, characterized in that: The concentration of HCl in the hydrochloric acid solution in step S2 is 1.8-2.2 M; the concentration of UiO-66-2,5-2NH2 in the hydrochloric acid solution is 4.1-6.1 mg / mL.
5. The preparation method according to claim 1, characterized in that: The soaking reaction time in step S2 is 4 to 5 hours; the drying temperature is 98 to 102°C.
6. A cationic MOFs material obtained by the preparation method according to any one of claims 1 to 5.
7. The cationic MOFs material according to claim 6, characterized in that: The specific surface area of the cationic MOFs material is 215 to 260 m 2 / g, and the average pore size is 4.7 to 5.8 angstroms.
8. Use of the cationic MOFs material according to claim 6 in the adsorption and removal of perrhenate.
9. The use according to claim 8, characterized in that: The cationic MOFs material has an adsorption capacity of 580 to 620 mg / g for perrhenate.
Citation Information
Patent Citations
Preparation method for synthesizing metal organic framework UiO-66 adsorbents by aid of mixed ligands
CN109395698A
Normal-pressure preparation method of zirconium metal-organic framework material UIO-66
CN111333851A
MOFs material capable of efficiently adsorbing precious metal palladium and preparation method of MOFs material
CN113731368A
Cited By
Preparation method and application of NH2-UiO-66 encapsulated sulfamic acid
CN119976950A