Cobalt oxyhydroxide catalyst, preparation method thereof and CoOOH / PTFE catalytic membrane

A three-dimensional porous flower-shaped cobalt hydroxyoxide catalyst was prepared by hydrothermal method and loaded onto a PTFE membrane, which solved the problems of difficult conversion and poor pH adaptability of transition metal-based catalysts in activated persulfate technology in the prior art, and achieved the effect of efficient removal of recalcitrant organic pollutant EE2.

CN119016049AActive Publication Date: 2024-11-26YUNNAN UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411101665.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-26
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

Existing transition metal-based catalysts have problems such as difficult conversion in activated persulfate technology, low recycling rate of powdered catalysts, and secondary pollution caused by dispersion in water bodies. They are difficult to efficiently remove recalcitrant organic pollutants such as 17α-ethynylestradiol (EE2) and have poor pH adaptability.

Method used

A three-dimensional porous flower-shaped cobalt hydroxyoxide catalyst was prepared by hydrothermal method and loaded onto a polytetrafluoroethylene (PTFE) membrane to form a CoOOH/PTFE catalytic membrane, which was used to activate persulfate (PMS) to remove EE2.

Benefits of technology

It achieves a high removal rate of EE2 (over 95%), has wide pH adaptability, low cobalt ion leaching concentration and good anti-interference ability. It can continuously treat water in actual water bodies for 24 hours and maintain a removal rate of 92.48%, showing the potential of green and efficient water treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016049A_ABST
    Figure CN119016049A_ABST
Patent Text Reader

Abstract

The invention discloses a cobalt oxyhydroxide catalyst, a preparation method thereof and a CoOOH / PTFE catalytic membrane, and belongs to the technical field of advanced oxidation water treatment. CoSO4. 7H2O, (NH4) 2S2O8 and K2SO4 are used as raw materials, the three-dimensional porous ball-flower-shaped hydroxyl cobalt oxide catalyst is prepared by adopting a hydrothermal method, and due to the special morphology of the material, the material can excite PMS to catalyze EE2, the removal rate reaches up to 95% or above, the removal rate is 2.39 times that of CoOOH prepared by a conventional precipitation method and 5.96 times that of commercial Co3O4, and the removal rate is up to 95% or above. In addition, the CoOOH material activated PMS catalysis EE2 also has relatively wide pH adaptability (the pH is 3.0 to 10.0), cycling stability and low cobalt ion leaching concentration (0.0019 mg / L). Besides, the CoOOH material is loaded on the PTFE membrane through a vacuum filtration technology, a CoOOH / PTFE membrane-PMS system is built, the CoOOH / PTFE membrane-PMS system is applied to continuous degradation of EE2 in actual water, continuous treatment can be conducted for 24 h, the removal rate of 92.48% can be kept, and potential actual application value is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of advanced oxidation water treatment, and specifically relates to a cobalt oxyhydroxide catalyst and a preparation method thereof, and a CoOOH / PTFE catalytic membrane. Background Art

[0002] Water pollution caused by refractory organic pollutants poses a huge threat to the ecological environment and human health. Among them, 17α-ethynyl estradiol (EE2) is a synthetic estrogen widely used in human oral contraceptives and drugs for the treatment of prostate cancer and osteoporosis, as well as in livestock and aquaculture activities. Due to its long half-life, high toxicity and resistance to biodegradation, EE2 has been widely found in aquatic environments and interferes with the endocrine system of exposed organisms through environmental enrichment, thereby causing reproductive disorders and sex reversal. At present, EE2 has become a common problem in environmental pollution, and it is difficult for sewage treatment plants and other traditional treatment processes to achieve continuous, green and complete removal of EE2. Therefore, it is urgent to explore an efficient, harmless and widely applicable water treatment technology. In recent years, Sulfate Radical Based advanced oxidation processes (S-AOPs) have gradually become one of the popular methods for treating organic pollutants in wastewater due to their advantages such as low cost and high reaction activity. Among them, the persulfate activation technology with transition metal-based catalysts is simple to operate, has a quick effect and low operating cost. However, it also has defects such as the difficulty in converting transition metal ions from a high-valent state to a low-valent state, low recovery rate of powdered catalysts, and secondary pollution caused by dispersion in water bodies, which limits its widespread application in the field of organic wastewater treatment.

[0003] Cobalt-based transition metals have high standard reduction potentials. 3+ / Co 2+ (E0 = 1.92V), which makes it easier to activate PMS efficiently. Among them, cobalt oxyhydroxide (CoOOH), as an environmentally friendly mineral, has the advantages of fast electron transfer, relative stability and low cost, and has also received widespread attention in the field of environmental remediation by activating PMS to remove organic matter. The abundant hydroxyl groups and active sites on the surface of CoOOH are conducive to the adsorption and activation of PMS, and its good electron transfer rate can promote electron transfer to quickly activate PMS, but CoOOH catalysts still have problems such as low pollutant removal rate and poor pH adaptability. Summary of the invention

[0004] In view of the above-mentioned shortcomings of the prior art, the present invention provides a cobalt oxyhydroxide catalyst and a preparation method thereof and a CoOOH / PTFE catalyst membrane.

[0005] To achieve the above object, the technical solution adopted by the present invention is:

[0006] A method for preparing a cobalt oxyhydroxide catalyst comprises the following steps: dissolving CoSO4·7H2O, (NH4)2S2O8 and K2SO4 in water, washing the precipitate obtained by hydrothermal reaction by centrifugation with ethanol and pure water, and then drying to obtain a CoOOH catalyst.

[0007] As a preferred embodiment of the present invention, the molar ratio of CoSO4·7H2O, (NH4)2S2O8 and K2SO4 is 1:1:3.

[0008] As a preferred embodiment of the present invention, the temperature of the hydrothermal reaction is 100-160° C. and the time is 8-20 h.

[0009] As a preferred embodiment of the present invention, the volume of the reaction kettle in the hydrothermal reaction is 30%-60%.

[0010] The present invention also claims a method for preparing the cobalt oxyhydroxide catalyst to prepare a three-dimensional porous flower-spherical cobalt oxyhydroxide catalyst.

[0011] As a preferred embodiment of the present invention, the surface of the three-dimensional porous flower-ball-shaped cobalt oxyhydroxide catalyst is rich in oxygen vacancies, and the abundant oxygen vacancy defects are conducive to accelerating electron transport and improving the catalyst activation PMS efficiency.

[0012] A CoOOH / PTFE catalytic membrane comprises a PTFE membrane microporous filter and a three-dimensional porous flower ball-shaped cobalt oxyhydroxyl catalyst loaded on the PTFE membrane microporous filter.

[0013] As a preferred embodiment of the present invention, the three-dimensional porous flower-spherical cobalt oxyhydroxide catalyst suspension on the CoOOH / PTFE catalyst membrane is loaded on the PTFE membrane microporous filter membrane by vacuum filtration.

[0014] As a preferred embodiment of the present invention, the pore size of the PTFE membrane microporous filter is 45 um.

[0015] As a preferred embodiment of the present invention, the loading amount of the three-dimensional porous flower-shaped cobalt oxyhydroxide catalyst on the CoOOH / PTFE catalyst membrane is 0.004-0.024 g / cm 2 .

[0016] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention uses CoSO4·7H2O, (NH4)2S2O8 and K2SO4 as raw materials, and adopts a hydrothermal method to prepare a three-dimensional porous flower-ball-shaped cobalt hydroxide oxide catalyst. Due to the special morphology of the material, it can stimulate PMS to remove EE2 with a removal rate of more than 95%, which is 2.39 times that of CoOOH prepared by conventional precipitation method and 5.96 times that of commercial Co3O4. In addition, the CoOOH material activates PMS to catalyze EE2 with a wide pH adaptability (pH: 3.0-10.0), cyclic stability, low cobalt ion leaching concentration (0.0019 mg / L) and good anti-interference ability, showing excellent activation PMS performance, good chemical stability and safety. In addition, the present invention loads CoOOH material on a polytetrafluoroethylene (PTFE) membrane with strong mechanical strength and acid, alkali and high temperature resistance through vacuum filtration technology, and builds a CoOOH / PTFE membrane-PMS system, which is applied to the continuous degradation of EE2 in actual water bodies. It can continuously treat for 24 hours and degrade 1.25L of Dianchi Lake water (Kunming, Yunnan) containing 3mg / L EE2, and can maintain a removal rate of 92.48%, which has potential practical application value. The CoOOH / PTFE membrane-PMS system proposed in this article is expected to achieve green, efficient and continuous treatment of organic pollutants in wastewater. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 The invention discloses a preparation process of cobalt oxyhydroxide catalyst and CoOOH / PTFE catalytic membrane.

[0018] Figure 2 A catalytic membrane system for degrading organic pollutants using CoOOH / PTFE catalytic membrane.

[0019] Figure 3Figure 1 is a graph showing the removal performance of the catalysts prepared in Example 1 and Comparative Example 1 for EE2; (a) is a graph showing the removal activity of the PMS catalytic system, the CoOOH catalytic system prepared in Example 1, the p-CoOOH catalytic system prepared in Comparative Example 1, the PMS+CoOOH catalytic system, the PMS+p-CoOOH catalytic system, and the PMS+Co3O4 catalytic system for EE2; (b) is a graph showing the reaction kinetics of the PMS catalytic system, the CoOOH catalytic system prepared in Example 1, the p-CoOOH catalytic system prepared in Comparative Example 1, the PMS+CoOOH catalytic system, the PMS+p-CoOOH catalytic system, and the PMS+Co3O4 catalytic system for EE2; (c) is a graph showing the removal activity of the PMS catalytic system by activating the PMS in (d) is a diagram showing the removal effect of EE2 in the initial organic pollutant solution with different pH values; (d) is a diagram showing the removal effect of EE2 in the organic pollutant solution with different water configurations by activating PMS in the PMS+CoOOH catalytic system, in which: PMS means that only PMS is added to the catalytic system; CoOOH means that only CoOOH prepared in Example 1 is added to the catalytic system; p-CoOOH means that only p-CoOOH prepared in Comparative Example 1 is added to the catalytic system; PMS+CoOOH means that PMS and CoOOH prepared in Example 1 are added to the catalytic system; PMS+p-CoOOH means that PMS and p-CoOOH prepared in Comparative Example 1 are added to the catalytic system; PMS+Co3O4 means that PMS and Co3O4 are added to the catalytic system.

[0020] Figure 4 Figure 2 is a graph showing the EE2 removal performance of CoOOH / PTFE catalytic membranes and PTFE membranes with different CoOOH / loading amounts; (a) is a graph showing the EE2 removal performance of CoOOH / PTFE catalytic membranes and PTFE membranes with different CoOOH / loading amounts; (b) is a graph showing the membrane flux comparison of CoOOH / PTFE catalytic membranes and PTFE membranes with different CoOOH / loading amounts; (c) is a graph showing the actual water treatment effect of the CoOOH / PTFE catalytic membrane prepared in Example 2, in which: PTFE membrane is the only PTFE membrane added to the catalytic system; PTFE membrane + PMS is the catalytic system PTFE membrane and PMS were added to the system; CoOOH / PTFE catalytic membrane-0.05+PMS was a catalytic system in which 0.05g of CoOOH prepared in Example 1 was added to the CoOOH / PTFE catalytic membrane and PMS; CoOOH / PTFE catalytic membrane-0.1+PMS was a catalytic system in which 0.3g of CoOOH prepared in Example 1 was added to the CoOOH / PTFE catalytic membrane and PMS.

[0021] Figure 5 (a) is a graph showing the stability of EE2 removal by the CoOOH-activated PMS prepared in Example 1; (b) is a graph showing the Co leaching concentration comparison of EE2 removal by the CoOOH-activated PMS prepared in Example 1 in EE2 solutions of different pH values.

[0022] Figure 6 This is a comparison diagram of XRD of CoOOH prepared in Example 1 before and after activating PMS to remove EE2.

[0023] Figure 7 XRD and FTIR patterns of CoOOH prepared in Example 1 and p-CoOOH prepared in Comparative Example 1, (a) is the XRD pattern, (b) is the FTIR pattern, in which CoOOH is CoOOH prepared in Example 1, and p-CoOOH is p-CoOOH prepared in Comparative Example 1.

[0024] Figure 8 The morphology images and N2 adsorption-desorption isotherms of the materials prepared in Example 1 and Comparative Example 1; (a) is the SEM image of CoOOH prepared in Example 1; (b) is the SEM image of p-CoOOH prepared in Comparative Example 1; (c) is the N2 adsorption-desorption isotherms of the materials prepared in Example 1 and Comparative Example 1; (d) is the low-magnification TEM image of CoOOH prepared in Example 1; (e) is the HRTEM image of CoOOH prepared in Example 1; (f) is the high-magnification TEM image of CoOOH prepared in Example 1; (g) is the EDS energy spectrum of the O element on the surface of CoOOH prepared in Example 1; (h) is the EDS energy spectrum of the Co element on the surface of CoOOH prepared in Example 1. DETAILED DESCRIPTION

[0025] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0026] Example 1

[0027] A preparation method of a cobalt oxyhydroxide catalyst comprises the following steps: dissolving 0.02 mol of CoSO4·7H2O, 0.02 mol of (NH4)2S2O8 and 0.06 mol of K2SO4 in 70 mL of deionized water, stirring for 2 h, transferring to a 200 mL polytetrafluoroethylene reactor, placing in a constant temperature drying oven to maintain 140 DEG C for reaction for 14 h, taking out a precipitate obtained after the reaction, washing it by centrifugation for three times with ethanol and pure water, and drying it at 60 DEG C overnight to obtain a CoOOH catalyst, which is recorded as CoOOH.

[0028] Example 2

[0029] like Figure 1 As shown, a method for preparing a CoOOH / PTFE catalytic membrane comprises the following steps: taking a PTFE membrane microporous filter membrane (pore size 45um) with a diameter of 47mm, soaking it in ethanol and deionized water for 1h respectively to remove surface impurities, and then drying it at 60°C overnight. Weighing 0.1g of the CoOOH catalyst material prepared in Example 1, dissolving it in 100mL of deionized water, ultrasonically dispersing it until uniform, vacuum filtering the CoOOH material onto the PTFE filter membrane, and drying it at 60°C overnight to prepare a cobalt oxyhydroxide catalyst with a loading of 0.018g / cm 2 CoOOH / PTFE membrane.

[0030] Example 3

[0031] A preparation method of a cobalt oxyhydroxide catalyst comprises the following steps: dissolving 0.02 mol of CoSO4·7H2O, 0.02 mol of (NH4)2S2O8 and 0.06 mol of K2SO4 in 70 mL of deionized water, stirring for 2 h, transferring to a 200 mL polytetrafluoroethylene reactor, placing in a constant temperature drying oven to maintain 160 DEG C for reaction for 20 h, taking out a precipitate obtained after the reaction, washing it by centrifugation for three times with ethanol and pure water, and drying it at 60 DEG C overnight to obtain a CoOOH catalyst, which is recorded as CoOOH.

[0032] Example 4

[0033] A method for preparing a CoOOH / PTFE catalytic membrane comprises the following steps: taking a PTFE membrane microporous filter membrane (pore size 45um) with a diameter of 47mm, soaking it in ethanol and deionized water for 1h respectively to remove surface impurities, and then drying it at 60°C overnight. Weighing 0.025g of the CoOOH catalyst material prepared in Example 3, dissolving it in 100mL of deionized water, ultrasonically dispersing it until uniform, vacuum filtering the CoOOH material onto the PTFE filter membrane, and drying it at 60°C overnight to prepare a cobalt oxyhydroxide catalyst with a loading of 0.004g / cm 2 CoOOH / PTFE membrane.

[0034] Example 5

[0035] A preparation method of a cobalt oxyhydroxide catalyst comprises the following steps: dissolving 0.02 mol of CoSO4·7H2O, 0.02 mol of (NH4)2S2O8 and 0.06 mol of K2SO4 in 70 mL of deionized water, stirring for 2 h, transferring to a 200 mL polytetrafluoroethylene reactor, placing in a constant temperature drying oven and maintaining at 100 DEG C for reaction for 8 h, taking out a precipitate obtained after the reaction, washing it by centrifugation for three times with ethanol and pure water, and drying it at 60 DEG C overnight to obtain a CoOOH catalyst, which is recorded as CoOOH.

[0036] Example 6

[0037] A method for preparing a CoOOH / PTFE catalytic membrane comprises the following steps: taking a PTFE membrane microporous filter with a diameter of 47 mm (pore size of 45 μm), soaking it in ethanol and deionized water for 1 hour to remove surface impurities, and then drying it at 60° C. overnight. Weighing 0.25 g of the CoOOH catalyst material prepared in Example 4, dissolving it in 100 mL of deionized water, ultrasonically dispersing it until uniform, vacuum filtering the CoOOH material onto a PTFE filter membrane, and drying it at 60° C. overnight to prepare a cobalt oxyhydroxide catalyst with a loading of 0.024 g / cm 2 CoOOH / PTFE membrane.

[0038] Comparative Example 1

[0039] A method for preparing a cobalt oxyhydroxide catalyst comprises the following steps: taking 50 mL of 10 mM CoCl2·H2O and placing it in a 100 mL beaker, dropping 12.5 mL of 1 M NaOH solution, and ultrasonicating for 10 min until uniform dispersion. Then, 2.5 mL of 0.9 M NaClO solution is added dropwise, ultrasonicating for 30 min, centrifugally washing and collecting the material, and drying at 60° C. overnight, and the obtained material is recorded as p-CoOOH.

[0040] Figure 7 (a) is the XRD spectrum of CoOOH prepared in Example 1 and p-CoOOH prepared in Comparative Example 1. The diffraction peaks of both are in good agreement with the hexagonal CoOOH (PDF#73-1213). Among them, 2θ=20.24°, 37.01°, 38.93°, 50.67°, 65.41° and 69.25° can perfectly match the (003), (101), (012), (015), (110) and (113) crystal planes of the structure, and combined with Figure 7From the FTIR graph of (b), it can be seen that both Example 1 of the present invention and Comparative Example 1 successfully synthesized CoOOH materials. Comparing the materials synthesized by the two methods of Example 1 and Comparative Example 1, it can be seen from the XRD graph that the CoOOH prepared in Example 1 has a stronger diffraction peak on the (003) crystal plane, which indicates that the cobalt oxyhydroxide catalyst prepared in Example 1 of the present invention has a preferential orientation structure along the (003) plane. Figure 7 As shown, the surface of the three-dimensional porous flower-shaped cobalt oxyhydroxide catalyst prepared in Example 1 is rich in oxygen vacancies. The abundant oxygen vacancy defects are conducive to accelerating electron transport and improving the efficiency of catalyst activation PMS. Figure 8 From (a)-(b) and (d)-(h), it can be seen that the CoOOH material prepared in Example 1 of the present invention is a three-dimensional porous flower ball morphology of a hollow structure assembled from thin nanosheets, with more pores inside, which can expose more active sites, and the Co and O elements are evenly distributed; the p-CoOOH material prepared in Comparative Example 1 has a morphology of nanoparticles agglomerated into blocks. Figure 8 (c) It can be seen that both the CoOOH prepared in Example 1 and the p-CoOOH prepared in Comparative Example 1 have a mesoporous structure, and CoOOH has a larger specific surface area of ​​67.28 m 2 / g, and the average pore size is 35.65nm. In summary, compared with p-CoOOH, the unique morphology and structure of CoOOH is more conducive to the diffusion, adsorption and desorption of pollutants on the catalyst surface, thereby improving the catalytic efficiency.

[0041] Comparative Example 2

[0042] The only difference between the preparation method of the CoOOH / PTFE catalyst membrane described in this comparative example and that of Example 2 is that the CoOOH catalyst material prepared in Example 2 is replaced by p-CoOOH prepared in Comparative Example 1.

[0043] Comparative Example 3

[0044] A preparation method of a cobalt oxyhydroxide catalyst comprises the following steps: dissolving 0.02 mol of CoSO4·7H2O, 0.02 mol of (NH4)2S2O8 and 0.06 mol of NaOH in 70 mL of deionized water, stirring for 2 h, transferring to a 200 mL polytetrafluoroethylene reaction kettle, placing in a constant temperature drying oven to maintain 140 DEG C for reaction for 14 h, taking out a precipitate obtained after the reaction, washing it three times by centrifugation with ethanol and pure water, and drying it at 60 DEG C overnight to obtain a CoOOH catalyst.

[0045] Comparative Example 4

[0046] The only difference between the preparation method of the CoOOH / PTFE catalyst membrane described in this comparative example and that of Example 2 is that the CoOOH catalyst material prepared in Example 2 is replaced by the CoOOH catalyst prepared in Comparative Example 3.

[0047] Comparative Example 5

[0048] A preparation method of a cobalt oxyhydroxide catalyst comprises the following steps: dissolving 0.02 mol of CoCl2·6H2O, 0.02 mol of (NH4)2S2O8 and 0.06 mol of K2SO4 in 70 mL of deionized water, stirring for 2 h, transferring to a 200 mL polytetrafluoroethylene reactor, placing in a constant temperature drying oven to maintain 140 DEG C for reaction for 14 h, taking out a precipitate obtained after the reaction, washing it three times by centrifugation with ethanol and pure water, and drying it at 60 DEG C overnight to obtain a CoOOH catalyst.

[0049] Comparative Example 6

[0050] The only difference between the preparation method of the CoOOH / PTFE catalytic membrane described in this comparative example and that of Example 2 is that the CoOOH catalyst material prepared in Example 2 is replaced by the CoOOH catalyst prepared in Comparative Example 5.

[0051] Effect Example 1

[0052] Powder catalysts prepared in Examples 1, 3, 5 and Comparative Examples 1, 3 and 5 for degradation of organic pollutants: This study used 3 mg / L EE2 as the target pollutant, and the performance test of the catalyst was carried out at room temperature (25±2°C). The specific method is as follows: Add 50 mL of 3 mg / L EE2 solution and 0.2 g / L catalyst material to a 150 mL conical flask, then transfer to a constant temperature oscillator and oscillate for 20 minutes. After reaching adsorption-desorption equilibrium, add 0.03 g / L PMS to the conical flask and continue to oscillate evenly. After a certain reaction time, use a syringe to transfer 3 mL of the solution and filter through a glass fiber filter. Then, use an ultra-high performance liquid chromatograph to measure the EE2 concentration in the solution after the reaction. The performance data is shown in Figure 3 and Figure 4 .

[0053] The catalytic membranes prepared in Examples 2, 4, 6 and Comparative Examples 2, 4 and 6 degrade organic pollutants: Figure 2As shown, the catalytic membrane system consists of a peristaltic pump, a feed liquid, a filtrate, a catalytic membrane and a fixed mold reactor. 200 mL, 3 mg / L EE2 solution is placed in a 500 mL beaker, 0.03 g / L PMS is added, and the feed liquid is stirred evenly. The prepared CoOOH / PTFE catalytic membrane is placed in the reactor, and the feed liquid passes through the catalytic membrane through the peristaltic pump to obtain the filtrate after the reaction, and the filtrate is no longer returned to the feed liquid. The filtrate is collected at certain time intervals and the EE2 concentration therein is measured using an ultra-high performance liquid chromatograph. The performance data is shown in Figure 3 and Figure 4 .

[0054] The removal efficiency of the catalyst for EE2 is calculated using the following formula:

[0055] R = C / C0 x 100%;

[0056] Wherein, R is the EE2 content (%) in the solution after a certain period of time, C0 and C are the initial concentration of EE2 and the concentration after a certain period of reaction, respectively.

[0057] The data of the catalyst activation PMS degradation EE2 experiment were fitted by the pseudo-first-order kinetic reaction rate equation as shown below:

[0058] ln(C / C0)=kt

[0059] Where k is the catalytic reaction rate constant and t is the reaction time.

[0060] The water flux calculation formula of the catalytic membrane is:

[0061] J = Vw / (Sxt);

[0062] J is the water flux, Vw is the volume of solution passing through the membrane (L), S is the effective area of ​​the catalytic membrane (m 2 ), t is the filtering time (h).

[0063] like Figure 3 As shown in (a) and (b), when only PMS, CoOOH prepared in Example 1 or p-CoOOH prepared in Comparative Example 1 are added to the catalytic system, the removal rate of EE2 is less than 10%, indicating that the unactivated PMS, CoOOH prepared in Example 1 or p-CoOOH prepared in Comparative Example 1 have limited ability to oxidatively remove EE2. After the CoOOH prepared in Example 1 or p-CoOOH prepared in Comparative Example 1 activates PMS in the catalytic system, the CoOOH / PMS system achieves an EE2 removal rate of 95.62% within 9 minutes, and the reaction rate constant is 0.36557 min -1, which is 2.39 times that of the p-CoOOH / PMS system (p-CoOOH is a flake material) prepared in Example 1, and 5.96 times that of the commercial Co3O4-PMS system, indicating that the three-dimensional porous flower-shaped CoOOH material prepared by the one-step hydrothermal method has great potential in activating PMS to degrade pollutants. The CoOOH / PMS system prepared in Examples 3 and 5 achieved a removal rate of more than 94% for EE2 within 9 minutes.

[0064] like Figure 4 As shown in (a), the PTFE membrane has almost no retention of EE2 (the removal rate of EE2 is only 10.45%). When only PMS is added to the catalytic system, the removal rate of EE2 within 40 minutes is 9.15%, indicating that the oxidation capacity of PMS is limited when it is not activated. Loading CoOOH material on the PTFE membrane can significantly improve the catalytic performance. When the material loading amount is 0.05g, 0.1g (Example 2), and 0.2g, the removal rate of EE2 by the catalytic membrane system is 71.03%, 95.23%, and 57.45%, respectively. When only 0.05g of CoOOH material is loaded, only a small number of active sites can be provided for activating PMS, resulting in unsatisfactory removal effect. When the CoOOH material loaded on the membrane is 0.3g, a large amount of catalyst agglomerates during vacuum filtration and cannot fully expose the active sites. The CoOOH / PMS system prepared in Examples 4 and 6 has a removal rate of more than 94% for EE2 within 40 minutes.

[0065] The materials prepared in Comparative Examples 3 and 5 are flaky in morphology, and their effects of activating PMS to catalyze EE2 are not ideal.

[0066] The CoOOH / PTFE catalytic membranes prepared in Comparative Examples 2, 4 and 6 have poor degradation performance due to the limited ability of the CoOOH material to activate PMS to degrade PMS.

[0067] Effect Example 2

[0068] The powder catalysts prepared in Example 1 and Comparative Examples 1, 3 and 5 degraded organic pollutants in initial organic pollutant solutions with different pH values: the pH of the initial solution (3 mg / L EE2 solution) was adjusted to 3, 4, 6.5, 8 and 10 respectively by 0.1 M NaOH or 0.1 M HCl (the original pH value of the solution was 6.5), and then the powder catalysts activated PMS at room temperature (25±2°C) to remove (adsorb and degrade) EE2 in initial organic pollutant solutions with different pH values.

[0069] like Figure 3(c) It can be seen that when the solution pH is 3.0, 4.0, 6.5, 8.0 and 10.0, the system has a large difference in the adsorption efficiency of EE2 within 20 minutes, which are 48.74%, 20.12%, 9.69%, 11.24% and 9.38% respectively. This shows that pH has a great influence on the catalyst adsorption of target pollutants, mainly because the surface isoelectric point of the CoOOH material prepared in Example 1 is 6.8. When the pH is less than 6.8, the surface of the catalyst material has a positive potential, and the electrostatic adsorption effect with EE2 is enhanced. When the pH is greater than 6.8, the surface of the material has a negative potential, and the attraction between it and the acidic PMS gradually decreases with the increase of the solution pH value, which will inhibit degradation. However, in the subsequent degradation catalytic stage, the system shows extremely high removal rate (greater than 95.95%) for EE2 at different pH values. This means that there is a non-free radical pathway that is insensitive to pH during the degradation process, which fully demonstrates that the CoOOH / PMS reaction system can achieve rapid degradation of EE2 through surface adsorption-catalytic synergy within a wide pH range (pH = 3.0-10.0).

[0070] The CoOOH material prepared by the present invention has a three-dimensional porous flower ball shape, so its mechanism of activating PMS to degrade EE2 does not depend on the pH value of the solution. However, since the morphology of the materials prepared in Comparative Examples 1, 3 and 5 is a flake morphology, it affects the way in which it activates PMS to degrade EE2, and it is more dependent on the pH of the solution.

[0071] Effect Example 3

[0072] In order to explore the influence of various inorganic ions and organic matter in organic pollutant solution on the activation of PMS catalyzed by CoOOH catalyst, this effect example uses pure water, tap water or Dianchi Lake water to prepare EE2 solution, and then the powder catalyst activates PMS at room temperature (25±2℃) to remove (adsorb and degrade) EE2 in organic pollutant solution prepared by different water bodies.

[0073] like Figure 3 As shown in d, the EE2 removal rates of the CoOOH / PMS system prepared in Example 1 in the three water bodies were 96.52%, 95.38% and 95.69% respectively. Tap water contains a large amount of anions (Cl - 、H2PO4 - 、CO3 2- 、NO 3- and SO4 2- ), the water of Dianchi Lake contains a large amount of anions (Cl-, H2PO4 - 、CO3 2- 、NO 3- and SO4 2-), metal ions and organic matter (HA). The experimental results show that the CoOOH / PMS system can achieve the degradation of pollutants in complex water bodies and has excellent practical application prospects.

[0074] Effect Example 4

[0075] The catalytic stability of Examples 1-2 and Comparative Examples 1-6 was explored.

[0076] (1) The catalyst material after the catalytic reaction in Example 1 was collected by centrifugation, and the residual substances on the catalyst surface were washed away with ethanol, and then used to activate PMS to degrade EE2. The cycle was repeated 5 times, with each adsorption-catalysis time of 30 minutes.

[0077] from Figure 5 It can be seen that after five cycles, the EE2 removal rate of the CoOOH material prepared in Example 1 decreased from 96.34% to 92.54%. Figure 6 The XRD diagram of the CoOOH material prepared in Example 1 before and after the reaction, its physical phase remains unchanged, indicating that the material can be reused. In addition, the amount of metal ion leaching after the CoOOH-PMS system prepared in Example 1 degraded EE2 in different pH solutions was tested by ICP (the CoOOH concentration in the CoOOH-PMS system was 0.20 g / L; the PMS concentration was 0.03 g / L). The experimental results are shown in Figure 1. Figure 5 As shown in (b), the ion leaching concentration of the CoOOH catalyst prepared in Example 1 in the pH range of 4-10 is lower than the Chinese standard (GB 25467-2010: 0.01 mg / L), and under strong alkaline conditions, almost no cobalt ions are dissolved in the solution, indicating that the material has high catalytic performance and also has green and safe practical application potential.

[0078] Compared with comparative examples 1-6, the materials prepared in Examples 1-2 of the present invention have better stability and lower Co leaching rate.

[0079] (2) The value of the catalytic membrane system in practical applications: a 3 mg / L EE2 solution was prepared using an actual water sample (taken from Dianchi Lake, Kunming on January 17, 2024) to explore the catalytic effect of the catalytic membrane on the actual water body in a continuous flow. Figure 4 As shown in (c), the catalytic membrane system prepared in Example 1 can continuously treat the Dianchi Lake water sample containing EE2 for 24 hours, the wastewater treatment volume reaches 1.25L, and the EE2 removal rate can still be maintained at 92.48%, indicating that the CoOOH / PTFE catalytic membrane system has broad application prospects and excellent practical application potential.

[0080] (3) Catalytic membrane flux plays an important role in the stable operation of the catalytic membrane system. The catalytic membranes prepared in Example 2, Comparative Examples 2, 4 and 6 degraded organic pollutants for 40 minutes, and the catalytic membrane flux was detected and calculated. Figure 4 (b) It can be seen that after 40 min of reaction, the flux of the PTFE membrane is 45.62 L / (m -2 h -1 ), while the flux of the catalytic membrane loaded with 0.05, 0.1, and 0.3 g of material can still be maintained at 48.38, 47.68, and 46.81 L / (m -2 h -1 ). The wettability of the catalytic membrane was studied by contact angle test. The water contact angle of the PTFE membrane was 118°. The water contact angle of the CoOOH / PTFE catalytic membrane prepared in Example 1 was 60°, showing good hydrophilicity. This is because the loading of the CoOOH material increases the surface hydrophilic hydroxyl groups of the catalytic membrane, thereby improving the hydrophilicity of the catalytic membrane, not only increasing the membrane flux, but also making the catalytic membrane have a certain anti-pollution ability, which is beneficial to wastewater treatment. However, when too much catalyst is loaded, the pores on the membrane will be blocked due to catalyst agglomeration, so that the membrane flux is reduced. Therefore, the most suitable catalyst loading is selected to be 0.1g.

[0081] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing a cobalt oxyhydroxide catalyst, characterized in that: The method comprises the following steps: dissolving CoSO4·7H2O, (NH4)2S2O8 and K2SO4 in water, washing the precipitate obtained by hydrothermal reaction by centrifugation with ethanol and pure water, and then drying to obtain a CoOOH catalyst.

2. The method for preparing the cobalt oxyhydroxide catalyst according to claim 1, characterized in that: The molar ratio of CoSO4·7H2O, (NH4)2S2O8 and K2SO4 is 1:1:

3.

3. The method for preparing the cobalt oxyhydroxide catalyst according to claim 1, characterized in that: The temperature of the hydrothermal reaction is 100-160° C. and the time is 8-20 hours.

4. The method for preparing the cobalt oxyhydroxide catalyst according to claim 1, characterized in that: The volume of the reaction kettle in the hydrothermal reaction is 30%-60%.

5. The method for preparing the cobalt oxyhydroxide catalyst according to any one of claims 1 to 4, wherein the cobalt oxyhydroxide catalyst having a three-dimensional porous flower ball shape is prepared.

6. The cobalt oxyhydroxide catalyst according to claim 5, characterized in that The surface of the three-dimensional porous flower-spherical cobalt oxyhydroxide catalyst is rich in oxygen vacancies.

7. A CoOOH / PTFE catalyst membrane, characterized in that: The invention comprises a PTFE membrane microporous filter and the three-dimensional porous flower-spherical cobalt hydroxide oxycatalyst as claimed in claim 6 loaded on the PTFE membrane microporous filter.

8. The CoOOH / PTFE catalyst membrane according to claim 7, characterized in that: The three-dimensional porous flower-spherical cobalt oxyhydroxide catalyst suspension on the CoOOH / PTFE catalyst membrane is loaded on the PTFE membrane microporous filter membrane by vacuum filtration.

9. The CoOOH / PTFE catalyst membrane according to claim 7, characterized in that: The pore size of the PTFE membrane microporous filter is 45um.

10. The CoOOH / PTFE catalyst membrane according to claim 7, characterized in that: The loading amount of the three-dimensional porous flower-shaped cobalt oxyhydroxide catalyst on the CoOOH / PTFE catalyst membrane is 0.004-0.024 g / cm 2 .

Citation Information

Patent Citations

  • Composite nanofiltration membrane with catalytic degradation function, preparation method and application thereof

    CN105597558A

  • Biochar-loaded nano CoOOH catalyst capable of efficiently activating persulfate and preparation method of biochar-loaded nano CoOOH catalyst

    CN115888717A

  • Cobalt oxyhydroxide particle and method for producing the same

    JP2005104771A

  • Electrocatalytic materials and methods for manufacturing same

    US20140213441A1

  • Material for oxygen evolution (OER) electrode catalyst, and use thereof

    WO2020096022A1