Method for improving photocatalytic oxygen production performance of bismuth oxyhalide

By loading cerium oxide promoter on the surface of bismuth oxyhalide, cerium oxide/bismuth oxyhalide composite material is formed, the problem of poor photocatalytic performance of bismuth oxyhalide is solved, and the effect of improving photocatalytic oxygen production performance and photocorrosion resistance is achieved. .

CN119016070AActive Publication Date: 2024-11-26FUZHOU UNIV +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411323509.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2024-11-26
Estimated Expiration
2044-09-23

AI Technical Summary

Technical Problem

Bismuth oxyhalide BiOX has low visible light utilization rate, high photogenerated carrier recombination rate, and is susceptible to light decomposition, resulting in poor photocatalytic effect, limiting its application in oxygen production and environmental treatment.

Method used

The cerium oxide CeO2 cocatalyst is supported on the surface of BiOX of BiOX, and the cerium oxide/bis oxide oxyhalide composite material is formed by in-situ photodeposition method to improve its photocatalytic oxygen production performance.

Benefits of technology

By loading CeO2, the photogenerated carrier migration distance is shortened, the carrier separation efficiency is improved, the photocorrosion resistance and photocatalytic performance are enhanced, and the photocatalytic oxygen production performance of bismuth oxyhalide is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016070A_ABST
    Figure CN119016070A_ABST
Patent Text Reader

Abstract

The invention belongs to a semiconductor photocatalytic material. The cerium oxide / bismuth oxyhalide composite material is synthesized by loading cerium oxide on bismuth oxyhalide by adopting an in-situ photodeposition method. The cocatalyst is loaded on the bismuth oxyhalide, and photodecomposition of the bismuth oxyhalide is greatly reduced while the photocatalytic oxygen production performance of the bismuth oxyhalide is effectively improved by shortening the migration distance of photon-generated carriers, promoting separation of electron hole pairs of the bismuth oxyhalide, improving the photocurrent performance and reducing impedance; and the photocorrosion resistance of the bismuth oxyhalide is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of photocatalytic materials, and in particular to a method for improving the photocatalytic oxygen production performance of bismuth oxyhalide. Background Art

[0002] As a new and effective green technology, photocatalysis can use sunlight to effectively remove toxic and harmful organic pollutants in the environment (Colloids Surf., A, 2019, 573, 137-45). In addition, photocatalysis is also often used to produce hydrogen and reduce carbon dioxide to fuel (J. Photochem. Photobiol., C, 2019,38, 1-26). Therefore, semiconductor photocatalysis is considered to be an effective way to solve energy and environmental problems.

[0003] Bismuth oxyhalide BiOX is an indirect bandgap semiconductor with a medium bandgap and good visible light absorption performance (Water Resour. Ind., 2023, 29, 100211). At the same time, BiOX has the advantages of open layered structure, high oxidation ability and high visible light response ability, which makes it widely concerned by researchers (Appl. Surf. Sci., 2019,487, 743-54).

[0004] However, due to the low visible light utilization rate of bismuth oxyhalide BiOX, the high recombination rate of photogenerated carriers, and the easy decomposition of bismuth oxyhalide under light, its poor photocatalytic effect limits its further application. It is of great significance to improve the photocatalytic performance and anti-photocorrosion ability of bismuth oxyhalide by ion doping, metal loading, and heterojunction construction (Korean J. Chem. Eng., 2018, 35, 1955-68). Summary of the invention

[0005] The object of the present invention is to provide a method for improving the photocatalytic oxygen production performance of bismuth oxyhalide.

[0006] To achieve the above object, the present invention adopts the following technical solution: A method for improving the photocatalytic oxygen production performance of bismuth oxyhalide, wherein a co-catalyst cerium oxide CeO2 is loaded on the surface of the bismuth oxyhalide BiOX to improve the photocatalytic oxygen production performance of the bismuth oxyhalide; the bismuth oxyhalide is bismuth oxychloride BiOCl, bismuth oxybromide BiOBr or bismuth oxyiodine BiOI.

[0007] Furthermore, the bismuth oxyhalide is dispersed in an aqueous solution of cerium nitrate hexahydrate, and cerium oxide CeO2 is loaded on the surface of the bismuth oxyhalide by an in-situ photodeposition method.

[0008] Furthermore, the light source of the in-situ photodeposition method is a 300 W xenon lamp, and the illumination time is 5 to 10 min.

[0009] Furthermore, the loading amount of the cerium oxide CeO2 is 1-5 wt%.

[0010] A cerium oxide CeO2 / bismuth oxyhalide BiOX composite material, wherein the CeO2 is loaded on the surface of BiOX by an in-situ photodeposition method.

[0011] Furthermore, the bismuth oxyhalide is a nano-sheet structure.

[0012] Furthermore, the bismuth oxyhalide is prepared by dissolving bismuth nitrate pentahydrate in ethylene glycol and transferring it into a syringe, slowly injecting and dropping sodium halide dispersed in an aqueous solution, and then washing the obtained product by centrifugation and transferring it to a deionized aqueous solution with a pH of 1 for hydrothermal synthesis; the hydrothermal synthesis time is 12 to 24 hours, and the temperature is 120 to 140°C.

[0013] Application of the above-mentioned cerium oxide CeO2 / bismuth oxyhalide BiOX composite material in a photocatalytic oxygen production system.

[0014] The beneficial effects of the present invention are: (1) BiOX semiconductor materials have the advantage of being cheap and readily available as photocatalysts. The metal co-catalyst CeO2 is loaded on the BiOX photocatalyst by in-situ photodeposition. By loading CeO2, the migration distance of photogenerated carriers is shortened, the carrier separation efficiency is improved, and the photocatalytic oxygen production performance is improved.

[0015] (2) By loading CeO2, the purpose of improving the effective separation of electron-hole pairs in BiOX materials is achieved. By improving the photocurrent performance, reducing the impedance, and enhancing the transmission and migration ability of photogenerated electron-hole pairs, the anti-photocorrosion and effective improvement of the photocatalytic oxygen production performance are achieved. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 (a) X-ray powder diffraction patterns of bismuth oxybromide and cerium oxide / bismuth oxybromide composite materials obtained in Example 2, (b) scanning electron microscopy image of bismuth oxybromide, (c) scanning electron microscopy image of bismuth oxybromide after irradiation with 300 W xenon lamp for 1 h, (d) transmission electron microscopy image of cerium oxide / bismuth oxybromide composite materials, (e) and (f) energy spectra of cerium oxide / bismuth oxybromide composite materials.

[0017] Figure 2 (a) Photocurrent response diagram and (b) impedance diagram of the bismuth oxybromide and cerium oxide / bismuth oxybromide composite material obtained in Example 2.

[0018] Figure 3(a) is a photocatalytic oxygen production performance diagram of cerium oxide / bismuth oxybromide composite materials with different cerium oxide loadings, and (b) is a long-term photocatalytic oxygen production performance diagram of bismuth oxybromide and cerium oxide / bismuth oxybromide composite materials obtained in Example 2. DETAILED DESCRIPTION

[0019] In order to make the contents of the present invention easier to understand, the technical solution of the present invention is further described below in conjunction with specific implementation methods, but the present invention is not limited thereto.

[0020] Example 1 (1) Preparation of bismuth oxybromide nanosheets: Weigh 0.001 mol of bismuth nitrate pentahydrate and add it to 30 mL of ethylene glycol solvent, stir until completely dissolved (referred to as solution A), and ultrasonically dissolve 0.003 mol of sodium bromide (NaBr) in 30 mL of deionized water (referred to as solution B). Transfer solution A to a 50 mL syringe and inject solution B at a rate of 2 mL / min under magnetic stirring at a speed of 300 rpm to form a white suspension. After centrifugation, the above suspension was washed three times with deionized water and filtered. The obtained precipitate was redispersed in 30 mL of deionized water with a pH value of 1 (about 1 mL of 65% dilute nitric acid was added to 149 mL of deionized water), and transferred to a polytetrafluoroethylene autoclave (50 mL), the hydrothermal temperature was set to 140 °C, and the reaction was carried out for 12 hours. After the autoclave was cooled naturally to room temperature, the precipitate was collected by centrifugation and washed three times with deionized water and ethanol respectively, and finally placed in a 60 °C oven to dry overnight to obtain bismuth oxybromide (BiOBr) nanosheets.

[0021] (2) Preparation of cerium nitrate hexahydrate aqueous solution: Take 1 g of cerium nitrate hexahydrate solid and dissolve it in 1 mL of deionized water to obtain cerium nitrate hexahydrate Ce(NO3)3·6H2O aqueous solution.

[0022] (3) Preparation of cerium oxide / bismuth oxybromide composite material: Weigh 0.05 g of the above BiOBr nanosheets and disperse them in 100 mL of deionized water, then drop 2.52 mL of Ce(NO3)3·6H2O solution (1 wt%) with a density of 1 g / mL to obtain a suspension, and then irradiate the suspension with a 300W xenon lamp for 5 min. After the reaction is completed, the reaction solution is centrifuged and washed three times with deionized water and ethanol respectively, and then placed in an oven to dry overnight at 60°C.

[0023] Example 2 (1) Preparation of bismuth oxybromide nanosheets: Weigh 0.001 mol of bismuth nitrate pentahydrate and add it to 30 mL of ethylene glycol solvent, stir until completely dissolved (referred to as solution A), and ultrasonically dissolve 0.003 mol of sodium bromide (NaBr) in 30 mL of deionized water (referred to as solution B). Transfer solution A to a 50 mL syringe and inject solution B at a rate of 2 mL / min under magnetic stirring at a speed of 300 rpm to form a white suspension. After centrifugation, the above suspension was washed three times with deionized water by centrifugation, filtered, and the obtained precipitate was redispersed in 30 mL of deionized water with a pH value of 1 (about 1 mL of 65% dilute nitric acid was added to 149 mL of deionized water), transferred to a polytetrafluoroethylene autoclave (50 mL), the hydrothermal temperature was set to 140 °C, and the reaction was carried out for 12 hours. After the autoclave was cooled naturally to room temperature, the precipitate was collected by centrifugation and washed three times with deionized water and ethanol respectively, and finally placed in an oven at 60 °C for drying overnight to obtain bismuth oxybromide nanosheets.

[0024] (2) Preparation of cerium nitrate hexahydrate aqueous solution: Take 1 g of cerium nitrate hexahydrate solid and dissolve it in 1 mL of deionized water to obtain cerium nitrate hexahydrate aqueous solution.

[0025] (3) Preparation of cerium oxide / bismuth oxybromide composite material: Weigh 0.05 g of the above BiOBr nanosheets and disperse them in 100 mL of deionized water, then drop 7.57 mL of 1 g / mL Ce(NO3)3·6H2O solution (3 wt.%) to disperse them evenly to obtain a suspension, which was then irradiated with a 300 W xenon lamp for 5 min. After the reaction was completed, the reaction solution was centrifuged and washed three times with deionized water and ethanol respectively, and then dried in an oven at 60°C overnight.

[0026] Example 3 (1) Preparation of bismuth oxybromide nanosheets: Weigh 0.001 mol of bismuth nitrate pentahydrate and add it to 30 mL of ethylene glycol solvent, stir until completely dissolved (referred to as solution A), and ultrasonically dissolve 0.003 mol of sodium bromide (NaBr) in 30 mL of deionized water (referred to as solution B). Transfer solution A to a 50 mL syringe and inject it into solution B at a rate of 2 mL / min under magnetic stirring at a speed of 300 rpm to form a white suspension. After centrifugation, the above suspension was washed three times with deionized water and filtered. The resulting precipitate was redispersed in 30 mL of deionized water with a pH value of 1 (about 1 mL of 65% dilute nitric acid was added to 149 mL of deionized water), and transferred to a polytetrafluoroethylene autoclave (50 mL), the hydrothermal temperature was set to 140 °C, and the reaction was carried out for 12 hours. After the autoclave was cooled naturally to room temperature, the precipitate was collected by centrifugation, washed three times with deionized water and ethanol respectively, and finally placed in an oven at 60 °C to dry overnight to obtain bismuth oxybromide nanosheets.

[0027] (2) Preparation of cerium nitrate hexahydrate aqueous solution: Take 1 g of cerium nitrate hexahydrate solid and dissolve it in 1 mL of deionized water to obtain cerium nitrate hexahydrate aqueous solution.

[0028] (3) Preparation of cerium oxide / bismuth oxybromide composite material: Weigh 0.05 g of the above BiOBr nanosheets and disperse them in 100 mL of deionized water, add 12.61 mL of 1 g / mL Ce(NO3)3·6H2O solution (5 wt.%), stir and disperse evenly to obtain a suspension, and then irradiate the suspension with a 300 W xenon lamp for 5 min. After the reaction is completed, the reaction solution is centrifuged and washed three times with deionized water and ethanol respectively, and then placed in an oven to dry overnight at 60°C.

[0029] Example 4 (1) Preparation of bismuth oxybromide nanosheets: Weigh 0.003 mol of bismuth nitrate pentahydrate (Bi(NO3)3·5H2O) and add it to 30 mL of ethylene glycol solvent, stir until completely dissolved (referred to as solution A), and ultrasonically dissolve 0.001 mol of sodium bromide (NaBr) in 30 mL of deionized water (referred to as solution B). Transfer solution A to a 50 mL syringe and inject it into solution B at a rate of 2 mL / min under magnetic stirring at a speed of 300 rpm to form a white suspension. After centrifugation, the above suspension was washed three times with deionized water and filtered. The resulting precipitate was redispersed in 30 mL of deionized water with a pH value of 1 (about 1 mL of 65% dilute nitric acid was added to 149 mL of deionized water), and transferred to a polytetrafluoroethylene autoclave (50 mL). The hydrothermal temperature was set to 140°C and the reaction was carried out for 12 hours. After the autoclave is naturally cooled to room temperature, the precipitate is collected by centrifugation, washed three times with deionized water and ethanol respectively, and finally dried in an oven at 60° C. overnight to obtain bismuth oxybromide nanosheets.

[0030] (2) Preparation of cerium nitrate hexahydrate aqueous solution: Take 1 g of cerium nitrate hexahydrate solid and dissolve it in 1 mL of deionized water to obtain cerium nitrate hexahydrate aqueous solution.

[0031] (3) Preparation of cerium oxide / bismuth oxybromide composite material: Weigh 0.05 g of the synthesized BiOBr nanosheets and disperse them in 100 mL of deionized water, add 2.52 mL of 1 g / mL Ce(NO3)3·6H2O solution (1 wt.%), stir and disperse evenly to obtain a suspension, and then irradiate the suspension with a 300 W xenon lamp for 10 min. After the reaction is completed, the reaction solution is centrifuged, washed three times with deionized water and ethanol respectively, and then placed in an oven to dry overnight at 60°C.

[0032] Example 5 (1) Preparation of bismuth oxybromide nanosheets: Weigh 0.001 mol of bismuth nitrate pentahydrate and add it to 30 mL of ethylene glycol solvent, stir until completely dissolved (referred to as solution A), and ultrasonically dissolve 0.001 mol of sodium bromide (NaBr) in 30 mL of deionized water (referred to as solution B). Transfer solution A to a 50 mL syringe and inject it into solution B at a rate of 2 mL / min under magnetic stirring at a speed of 300 rpm to form a white suspension. After centrifugation, the above suspension was washed three times with deionized water and filtered. The resulting precipitate was redispersed in 30 mL of deionized water with a pH value of 1 (about 1 mL of 65% dilute nitric acid was added to 149 mL of deionized water), and transferred to a polytetrafluoroethylene autoclave (50 mL), the hydrothermal temperature was set to 120 °C, and the reaction was carried out for 24 hours. After the autoclave was cooled naturally to room temperature, the precipitate was collected by centrifugation, washed three times with deionized water and ethanol respectively, and finally placed in an oven at 60 °C to dry overnight to obtain bismuth oxybromide nanosheets.

[0033] (2) Preparation of cerium nitrate hexahydrate aqueous solution: Take 1 g of cerium nitrate hexahydrate solid and dissolve it in 1 mL of deionized water to obtain cerium nitrate hexahydrate aqueous solution.

[0034] (3) Preparation of cerium oxide / bismuth oxybromide composite material: Weigh 0.05 g of the above BiOBr nanosheets and disperse them in 100 mL of deionized water, add 12.61 mL of 1 g / mL Ce(NO3)3·6H2O solution (5 wt.%), stir and disperse evenly to obtain a suspension, and then irradiate the suspension with a 300 W xenon lamp for 5 min. After the reaction is completed, the reaction solution is centrifuged, washed three times with deionized water and ethanol respectively, and then placed in an oven to dry overnight at 60°C.

[0035] Figure 1(a) is the X-ray powder diffraction pattern (XRD) of the bismuth oxybromide (BiOBr) and cerium oxide / bismuth oxybromide (CeO2 / BiOBr) composite materials obtained in Example 2. The experimental results show that the crystal plane diffraction peak of BiOBr corresponds to the standard diffraction peak of PDF#09-0393 tetragonal crystal, indicating the successful synthesis of BiOBr. For the CeO2 / BiOBr composite material, no characteristic peak of CeO2 was detected in its XRD diffraction spectrum, which may be due to the small CeO2 particles loaded. Figure (b) is a scanning electron microscope image of BiOBr, which shows that BiOBr is mainly in the form of square nanosheets. Figure (c) is an electron microscope image of BiOBr after irradiation with a 300W xenon lamp for 1 h. It can be seen that after irradiation, the originally smooth bismuth oxybromide edge is wrapped with a thick jagged oxide film, which reduces its photocatalytic reaction sites. Figures (d) and (e) show that after photodeposition, the loaded CeO2 particles wrap the edges of bismuth oxybromide, protecting BiOBr and effectively inhibiting the growth of the oxide film Bi2O3, thereby improving the photocorrosion resistance of bismuth oxybromide. The energy spectrum (f) shows that Bi, O, and Br are evenly distributed throughout the nanosheet, while Ce is distributed on the edges of the nanosheet, further illustrating the successful synthesis of the cerium oxide / bismuth oxybromide (CeO2 / BiOBr) composite material.

[0036] Figure 2 The (a) photocurrent response diagram and (b) impedance diagram of the bismuth oxybromide (BiOBr) and cerium oxide / bismuth oxybromide (CeO2 / BiOBr) composite materials obtained in Example 2. It can be clearly seen from Figure (a) that the photocatalysts before and after loading are photosensitivity, but in the process of the on-off cycle of the light source, the photocurrent density of the CeO2 / BiOBr composite material is always better than that of the pure BiOBr sample, indicating that the loading of CeO2 effectively promotes the separation and migration of photogenerated electron-hole pairs, and the effective separation of photogenerated electron-hole pairs can ensure that electrons or holes participate more effectively in photocatalytic reduction or oxidation reactions, thereby improving the photocatalytic performance. Electrochemical impedance spectroscopy (EIS) is used to detect the interface migration dynamics of carriers. Figure (b) shows the impedance diagram of bismuth oxybromide (BiOBr) and cerium oxide / bismuth oxybromide (CeO2 / BiOBr) composite materials. Compared with bismuth oxybromide (BiOBr), the (impedance) curvature radius of the cerium oxide / bismuth oxybromide (CeO2 / BiOBr) composite material is smaller, revealing that the loading of CeO2 can promote the charge transfer at the BiOBr interface, indicating that the charge transfer ability and conductivity of the composite material are better than those of the pure BiOBr sample, which is beneficial to improving the photocatalytic oxygen production performance of bismuth oxybromide (BiOBr).

[0037] The photocatalytic oxygen production performance test experiment was illuminated by a CEL-HXE300 xenon lamp (300 W). 0.05 g of catalyst and 0.4 g of ferrous nitrate nonahydrate were added to 100 mL of deionized water and dispersed evenly by ultrasound. The suspension was placed in a photocatalytic water splitting reaction device and stirred at a speed of 600 rpm in a closed circulation system for 1 h. The types and yields of the generated gases were then analyzed by a gas chromatograph (GC-2014C, Shimadzu, Japan). Figure 3 The photocatalytic oxygen production performance diagram of the BiOBr and CeO2 / BiOBr composite materials obtained in Examples 1-3. As shown in Figure (a), when the cerium oxide loading content is 3 wt.%, its photocatalytic performance is the best, about 86.1 μmol / h. When the cerium oxide loading content is 1 wt.%, the photocatalytic activity of the composite material is low. This is because the amount of CeO2 in the CeO2 / BiOBr composite is small, resulting in a low separation efficiency of the catalyst electron-hole pairs. The photocatalytic oxygen production of the composite material with a cerium oxide loading content of 5 wt.% is relatively low because too much CeO2 is compounded, causing the BiOBr edge to be transitionally wrapped by CeO2, covering the reaction active sites on its surface, reducing the photocatalytic activity of CeO2 / BiOBr. Figure (b) is a 10-hour photocatalytic oxygen production performance diagram of CeO2, BiOBr obtained in Example 2, and CeO2 / BiOBr composite materials. The photocatalytic performance and anti-photocorrosion ability of BiOBr and CeO2 / BiOBr composite materials are evaluated by the photocatalytic oxygen production and oxygen production rate within 10 hours. As can be seen from the figure, the photocatalytic oxygen production of BiOBr after CeO2 loading is increased to 2.8 times that of pure BiOBr. The photocatalytic oxygen production of pure CeO2 is much lower than that of BiOBr and CeO2 / BiOBr composite materials, and there is no obvious increase after long-term illumination. In the 10-hour continuous oxygen production test, it was found that the photocatalytic oxygen production rate of pure BiOBr gradually tended to the level after the photocatalytic time reached 5 hours, while the reaction rate of CeO2 / BiOBr composite photocatalyst remained basically unchanged after a long-term photocatalytic reaction. This long-term photocatalytic oxygen production performance test shows that the photocatalytic oxygen production performance of BiOBr is enhanced after CeO2 loading.

[0038] In summary, the present invention forms a BiOX-CeO2 heterojunction structure with halogen atoms by loading the co-catalyst CeO2, which is conducive to the transmission of electron holes, so that the catalytic performance of the composite is improved. The holes that cause photocorrosion are guided away and not allowed to accumulate on the BiOX surface. After being guided away by this heterojunction structure, the anti-photocorrosion ability is improved, thereby promoting the performance of photocatalytic oxygen production.

[0039] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the present invention.

Claims

1. A method for improving the photocatalytic oxygen production performance of bismuth oxyhalide, characterized in that: The co-catalyst cerium oxide CeO2 is loaded on the surface of the bismuth oxyhalide BiOX to improve the photocatalytic oxygen production performance of the bismuth oxyhalide; the bismuth oxyhalide is bismuth oxychloride BiOCl, bismuth oxybromide BiOBr or bismuth oxyiodine BiOI.

2. The method for improving the photocatalytic oxygen production performance of bismuth oxyhalide according to claim 1, characterized in that: Specifically, bismuth oxyhalide is dispersed in an aqueous solution of cerium nitrate hexahydrate, and cerium oxide CeO2 is loaded on the surface of the bismuth oxyhalide by an in-situ photodeposition method.

3. The method for improving the photocatalytic oxygen production performance of bismuth oxyhalide according to claim 2, characterized in that: The light source of the in-situ photodeposition method is a 300 W xenon lamp, and the illumination time is 5 to 10 min.

4. The method for improving the photocatalytic oxygen production performance of bismuth oxyhalide according to claim 2, characterized in that: The loading amount of CeO2 is 1-5 wt%.

5. A cerium oxide CeO2 / bismuth oxyhalide BiOX composite material, characterized in that: The CeO2 is loaded on the BiOX surface by in-situ photodeposition.

6. The composite material according to claim 5, characterized in that: The bismuth oxyhalide is a nano-sheet structure.

7. The composite material according to claim 5, characterized in that: The bismuth oxyhalide is prepared by dissolving bismuth nitrate pentahydrate in ethylene glycol and transferring the solution into a syringe, slowly injecting and dropping sodium halide dispersed in an aqueous solution, and then washing the obtained product by centrifugation and transferring the product to a deionized aqueous solution with a pH of 1 for hydrothermal synthesis; the hydrothermal synthesis time is 12 to 24 hours, and the temperature is 120 to 140°C.

8. Use of the cerium oxide CeO2 / bismuth oxyhalide BiOX composite material as claimed in claim 5 in a photocatalytic oxygen production system.

Citation Information

Patent Citations

  • Synthesis method of BiOCl / g-C3N4 / CeO2 three-phase photo-catalytic material

    CN112090438A

  • Preparation method and application of BiOBr / CeO2 nanosheet composite photocatalyst