G-C3N4 / BiOBr visible light catalytic material and preparation method thereof
The g-C3N4/BiOBr visible photocatalyst prepared by thiourea low-temperature pyrolysis method and room-temperature mixed precipitation method solves the problems of high material cost and low photocatalytic efficiency in the prior art, and achieves the effect of efficient degradation of difficult-to-degrade organic wastewater.
Patent Information
- Application Number
- CN202411127508.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-26
AI Technical Summary
When existing visible photocatalysts such as TiO2 and ZnO are treated with difficult-to-degrade organic wastewater, the material price is high and the environmental friendliness is low. Carbon nitride (g-C3N4) is low in specific surface area and high photogenerating electron-hole recombination rate. The photocatalytic efficiency is not high.
G-C3N4 was synthesized by low-temperature pyrolysis method of thiourea and compounded with BiOBr by room temperature mixing and precipitation method to prepare g-C3N4/BiOBr visible photocatalyst, reducing electron-hole recombination rate, improving active sites, and enhancing photocatalytic performance.
The visible light catalytic efficiency of g-C3N4 is improved, the light absorption range is increased, and a variety of dye pollutants can be efficiently degraded, and the biotoxicity of wastewater is reduced. The preparation method is simple and cost-effective.
Smart Images

Figure CN119016084A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of photocatalysts, and in particular relates to a visible light catalyst for achieving degradation of pollutants in organic wastewater. Background Art
[0002] The effective treatment of high-concentration refractory organic wastewater is one of the current problems in the field of environmental protection and wastewater treatment. Many refractory organic pollutants cannot be effectively removed, and a series of environmental problems will arise as wastewater is discharged into the environment. Therefore, the treatment of refractory organic wastewater has a great industry demand, among which efficient and non-toxic treatment technologies are particularly in short supply.
[0003] Visible light catalytic oxidation technology uses sunlight to generate e– and h+, and produces active species through redox reactions, which can redox organic pollutants into small molecules, or even CO2 and H2O, thereby removing pollutants. Visible light catalytic oxidation technology has the advantages of fast reaction speed, no secondary pollution, and good reusability, and is considered to be a sustainable means of treating synthetic dye pollutants. At present, the catalysts that are studied more in the field of visible light catalysis are mainly semiconductor photocatalysts represented by TiO2, ZnO, etc., which have the problems of high material prices and low environmental friendliness. Carbon nitride (g-C3N4), as an emerging two-dimensional material, has attracted much attention due to its unique electronic structure and stable chemical properties. g-C3N4 can be synthesized from cheap organic materials and has a low preparation cost. g-C3N4 has a suitable band structure (medium band gap of 2.7–2.8eV), high visible light (450–460nm) absorption capacity, thermal stability and chemical stability, so g-C3N4 has a high application prospect in the field of visible light catalysis. However, due to the low specific surface area and few exposed active sites of the photocatalyst, the surface of g-C3N4 is prone to photogenerated – -h + The photocatalytic efficiency is not high due to the high recombination rate and other problems. Therefore, the development of – -h + The current research hotspot is the synthesis or modification of g-C3N4 catalysts with improved active sites. Summary of the invention
[0004] The present invention aims to improve the visible light catalytic efficiency of g-C3N4 and provides a method for reducing the photoinduced e – -h +The invention discloses a composite g-C3N4 / BiOBr visible light catalytic material and a preparation method thereof. Firstly, the g-C3N4 material is synthesized by a thiourea low temperature pyrolysis method, and then the g-C3N4 / BiOBr material is prepared by a room temperature mixed precipitation method. The prepared g-C3N4 / BiOBr visible light catalyst has the advantages of high specific surface area, strong visible light absorption capacity, low electron recombination rate, small dosage, wide pH adaptability and the like.
[0005] In order to solve the above technical problems, the present invention is implemented by the following technical solutions:
[0006] According to one aspect of the present invention, a g-C3N4 / BiOBr visible light catalytic material is provided, which is prepared by the following method:
[0007] (1) The g-C3N4 material was synthesized by thiourea low-temperature pyrolysis method at a reaction temperature of 550°C-570°C;
[0008] (2) mixing the powdered g-C3N4 material obtained in step (1) with Bi(NO3)3·5H2O solid, adding ethylene glycol to immerse the mixture, and mixing by ultrasonication until uniform;
[0009] (3) Adding a certain amount of KBr aqueous solution dropwise to the mixed solution obtained in step (2) while rapidly stirring, and continuing to stir until the mixture is uniformly mixed;
[0010] (4) After the mixed solution obtained in step (3) is allowed to settle, the yellow precipitate is collected by centrifugation, washed and dried, and the dried powder is the g-C3N4 / BiOBr composite material.
[0011] According to another aspect of the present invention, a method for preparing a g-C3N4 / BiOBr visible light catalytic material is provided, characterized in that it comprises the following steps:
[0012] (1) The g-C3N4 material was synthesized by thiourea low-temperature pyrolysis method at a reaction temperature of 550°C-570°C;
[0013] (2) mixing the powdered g-C3N4 material obtained in step (1) with Bi(NO3)3·5H2O solid, adding ethylene glycol to immerse the mixture, and mixing by ultrasonication until uniform;
[0014] (3) Adding a certain amount of KBr aqueous solution dropwise to the mixed solution obtained in step (2) while rapidly stirring, and continuing to stir until the mixture is uniformly mixed;
[0015] (4) After the mixed solution obtained in step (3) is allowed to settle, the yellow precipitate is collected by centrifugation, washed and dried, and the dried powder is the g-C3N4 / BiOBr composite material.
[0016] In the above g-C3N4 / BiOBr visible light catalytic material and preparation method thereof:
[0017] Furthermore, the step (1) comprises: using nitrogen-containing precursor thiourea as raw material, first grinding it into a uniform powder, then heating it to 550°C-570°C and maintaining it for 2-3 hours; then naturally annealing and cooling to room temperature, then taking it out, and grinding the fired yellow block solid into powder, namely the g-C3N4 material.
[0018] Furthermore, in the step (2), based on the conversion of Bi in Bi(NO3)3 to BiOBr, the mass ratio of g-C3N4 to BiOBr is 1:10-1:2.
[0019] Furthermore, in step (3), the speed of rapid stirring is 300-350 r·min -1 .
[0020] Furthermore, in step (3), the amount of bromide ions in the KBr aqueous solution is equal to the amount of Bi element in the Bi(NO3)3·5H2O solid in step (2).
[0021] Furthermore, in step (4), the mixed solution is allowed to stand for precipitation for 12-14 hours.
[0022] Furthermore, in step (4), washing is performed using anhydrous ethanol and ultrapure water for three times respectively.
[0023] Furthermore, in step (4), the drying is performed at 40-60° C. for 12-24 hours.
[0024] The beneficial effects of the present invention are:
[0025] The present invention uses cheap thiourea as a raw material, and adopts a method of low-temperature pyrolysis and room-temperature stirring precipitation to quickly prepare a visible light catalyst. The prepared catalyst has high activity:
[0026] (i) The visible light photocatalyst g-C3N4 / BiOBr prepared by the present invention has both the heptazine ring unit layered structure of g-C3N4 and the tetragonal crystal structure of BiOBr. The material surface is tightly arranged, the monomer particles are small and full, and it has dispersed nano-discs with relatively thin layers.
[0027] (ii) The visible light photocatalyst g-C3N4 / BiOBr prepared by the present invention follows the S-type charge transfer mechanism, has a high charge separation rate, reduces the recombination of electrons and holes, and can efficiently generate e under visible light catalysis. – and h + , which is then further generated when degrading pollutants· OH, · O2 – Active substances such as chlorinated polyols have high degradation efficiency.
[0028] (III) The visible light catalyst g-C3N4 / BiOBr prepared by the present invention increases the utilization range of visible light, and the visible light region can reach 480nm.
[0029] (IV) The visible light photocatalyst g-C3N4 / BiOBr prepared by the present invention exhibits superior performance in degrading high-chroma dyes and can efficiently degrade a variety of dye pollutants (methyl orange, reactive yellow 145, reactive black 5, Ponceau S, reactive blue 4, alizarin red S), achieving 100% complete degradation within 20-60 minutes, and has a wide range of applications.
[0030] (V) The visible light photocatalyst g-C3N4 / BiOBr prepared by the present invention can significantly reduce the biological toxicity of wastewater after degrading dye wastewater.
[0031] (VI) The present invention adopts the method of low-temperature pyrolysis (550°C-570°C) and stirring precipitation at room temperature to quickly prepare g-C3N4 / BiOBr, which can simply and quickly synthesize the heptazine ring unit layered structure of g-C3N4 and the tetragonal crystal structure of BiOBr with regular morphology and high catalytic activity.
[0032] In summary, the visible light catalyst g-C3N4 / BiOBr and its preparation method of the present invention have a simple preparation method, greatly shorten the preparation time and reduce energy consumption; the prepared catalyst further improves the light conversion rate of visible light, and the degradation rate of dye pollutants reaches more than 99%. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a flow chart for preparing the g-C3N4 / BiOBr visible light catalytic material of the present invention;
[0034] Figure 2 This is a scanning electron microscope image of the g-C3N4 / BiOBr visible light catalytic material prepared in Example 1;
[0035] Figure 3 This is the UV-visible diffuse reflectance spectrum of the g-C3N4 / BiOBr visible light photocatalyst prepared in Example 1;
[0036] Figure 4 This is a scanning electron microscope image of the g-C3N4 / BiOBr visible light photocatalyst prepared in Example 2;
[0037] Figure 5This is a transmission electron microscope (TEM) image of the g-C3N4 / BiOBr visible light photocatalyst prepared in Example 3;
[0038] Figure 6 This is the surface chemical state analysis (XPS) diagram of the g-C3N4 / BiOBr visible light photocatalyst prepared in Example 3;
[0039] Figure 7 This is a comparison diagram of the removal rates and degradation rate constants of g-C3N4 / BiOBr visible light photocatalyst prepared in Example 3 when catalyzing the degradation of methyl orange at different dosages;
[0040] Figure 8 The removal rate comparison diagram and degradation rate constant diagram of methyl orange degradation at different pH values by g-C3N4 / BiOBr visible light photocatalyst prepared in Example 3;
[0041] Fig. 9 The active species capture kinetics experiment of the g-C3N4 / BiOBr visible light photocatalyst prepared in Example 3 for the degradation of methyl orange and the comparison diagram of the degradation rate constant and the removal rate;
[0042] Fig.10 This is the EPR spectrum of the g-C3N4 / BiOBr visible light photocatalyst prepared in Example 3 under visible light excitation;
[0043] Fig.11 A comparison chart of the photocatalytic degradation rate constants of various dyes at different concentrations in the g-C3N4 / BiOBr visible light catalyst system prepared in Example 3 is shown. DETAILED DESCRIPTION
[0044] like Figure 1 As shown, the present invention provides a g-C3N4 / BiOBr visible light catalytic material and a preparation method thereof, which are prepared according to the following steps:
[0045] (1) The g-C3N4 material was synthesized by thiourea low-temperature pyrolysis method at a reaction temperature of 550℃-570℃.
[0046] In some preferred embodiments of the present invention, the nitrogen-containing precursor thiourea is used as a raw material, which is first ground into a uniform powder, and then heated to 550°C-570°C and maintained for 2-3 hours; thereafter, it is naturally annealed and cooled to room temperature and then taken out, and the fired yellow block solid is ground into powder, which is the g-C3N4 material.
[0047] (2) Mix the powdered g-C3N4 material obtained in step (1) and Bi(NO3)3·5H2O solid, add ethylene glycol to immerse them, and mix them evenly by ultrasonic mixing.
[0048] In some preferred embodiments of the present invention, based on the conversion of Bi in Bi(NO3)3 to BiOBr, the mass ratio of g-C3N4 to BiOBr is 1:10-1:2.
[0049] Among them, the amount of ethylene glycol added can completely immerse the mixture of powdered g-C3N4 material and Bi(NO3)3·5H2O solid.
[0050] (3) To the mixed solution obtained in step (2), a certain amount of KBr aqueous solution is added dropwise while rapidly stirring, and stirring is continued until the mixture is uniformly mixed.
[0051] In some preferred embodiments of the present invention, the speed of rapid stirring is 300-350 r·min -1 .
[0052] In some preferred embodiments of the present invention, the amount of bromide ions in the KBr aqueous solution is equal to the amount of Bi element in the Bi(NO3)3·5H2O solid of step (2).
[0053] (4) After the mixed solution obtained in step (3) is allowed to settle, the yellow precipitate is collected by centrifugation, washed and dried, and the dried powder is the g-C3N4 / BiOBr composite material.
[0054] In some preferred embodiments of the present invention, the mixed solution is allowed to settle for 12-14 hours.
[0055] In some preferred embodiments of the present invention, washing is performed by washing with anhydrous ethanol and ultrapure water three times respectively.
[0056] In some preferred embodiments of the present invention, the drying is performed at 40-60° C. for 12-24 hours.
[0057] The present invention is further described in detail below through specific examples. The following examples can enable those skilled in the art to more fully understand the present invention, but do not limit the present invention in any way.
[0058] The following examples mainly use g-C3N4 / BiOBr as a photocatalyst, a 300W xenon lamp light source to simulate a natural light environment, and methyl orange (0) as a typical dye pollutant.
[0059] Example 1
[0060] A method for preparing a thermally polymerized g-C3N4 / BiOBr visible light catalytic material, the specific method steps are as follows:
[0061] Weigh a certain amount of thiourea and place it in a ceramic mortar. Grind it for 5 min to obtain a nitrogen-containing precursor powder. Weigh 10 g of the nitrogen-containing precursor powder in a 100 mL alumina crucible, cover it, wrap it with tin foil, and seal it in a muffle furnace. -1 The sample was heated to 550°C at a heating rate of 1000 °C and kept at this temperature for 2 hours. It was then naturally annealed and cooled to room temperature before being taken out. The fired yellow block solid was ground into yellow powder in a mortar, which is carbon nitride (g-C3N4).
[0062] Weigh 30.49 mg of powdered g-C3N4 and 1 mmol of analytically pure solid Bi(NO3)3·5H2O (according to the conversion that Bi in Bi(NO3)3 can generate BiOBr, the mass ratio of g-C3N4:BiOBr is 1:10) in a 150 mL beaker, add 30 mL of ethylene glycol and ultrasonicate for 2 h; at the same time, prepare 1 mmol / 20 mL of KBr solution.
[0063] After the ultrasound is finished, transfer the yellow suspension to the stirrer, add a stir bar, and set the speed to 300 r / min. -1 , stirred for 2 h, and 20 mL of KBr solution was added dropwise to the yellow suspension while stirring.
[0064] After stirring, the mixture in the beaker was transferred to a 50 mL centrifuge tube and allowed to settle for 12 h. The yellow precipitate was then collected by centrifugation and washed three times with anhydrous ethanol and ultrapure water, respectively. The mixture was then placed in a 60 ° C oven for drying for 12 h, and the dried photocatalyst was ground into powder to obtain g-C3N4 / BiOBr.
[0065] Figure 2 The scanning electron microscope (SEM) image of the g-C3N4 / BiOBr composite photocatalyst prepared in Example 1 is shown. Figure 2 It can be seen that the surface of the g-C3N4 / BiOBr composite catalyst is rough and consists of elliptical flake-like nanosheet structures with a flake diameter of about 50–100 nm and a flake thickness of less than 20 nm. The nanosheet structure is obvious, the flakes are thin, and the distribution is relatively dispersed.
[0066] Figure 3 is the UV-visible diffuse reflectance spectrum of the g-C3N4 / BiOBr composite photocatalyst prepared in Example 1, Figure 3 It is shown that the light absorption range and intensity of the composite material are greatly improved compared with single g-C3N4 and BiOBr materials, respectively, indicating that the visible light catalytic performance of the composite material prepared in Example 1 is greatly improved.
[0067] Example 2
[0068] A method for preparing a thermally polymerized g-C3N4 / BiOBr visible light catalytic material, the specific method steps are as follows:
[0069] A certain amount of thiourea was weighed and placed in a ceramic mortar and ground for 5 min to obtain a nitrogen-containing precursor powder. 10 g of the nitrogen-containing precursor powder was weighed and placed in a 100 mL alumina crucible, which was covered and sealed with tin foil and placed in a muffle furnace. The mixture was heated from room temperature at 5 °C min -1 The sample was heated to 570°C at a heating rate of 1000 ℃ and kept at this temperature for 2 hours. It was then naturally annealed and cooled to room temperature before being taken out. The fired yellow block solid was ground into yellow powder in a mortar. The obtained substance was g-C3N4.
[0070] Weigh 30.49 mg of powdered g-C3N4 and 1 mmol of Bi(NO3)3·5H2O analytical pure solid (according to the conversion of Bi in Bi(NO3)3 to BiOBr, the mass ratio of g-C3N4:BiOBr is 1:10) in a 150 mL beaker, add 30 mL of ethylene glycol and ultrasonicate for 2 h; at the same time, prepare 1 mmol / 20 mL of KBr solution. After the ultrasonication, transfer the yellow suspension to the stirrer, add a stirrer, and set the speed to 300 r·min -1 , stirred for 2 h, and 20 mL of KBr solution was added dropwise to the yellow suspension while stirring.
[0071] After stirring, the mixture in the beaker was transferred to a 50 mL centrifuge tube and allowed to settle for 12 h. The yellow precipitate was then collected by centrifugation and washed three times with anhydrous ethanol and ultrapure water, respectively. The mixture was then placed in a 60 ° C oven for drying for 12 h, and the dried photocatalyst was ground into powder to obtain g-C3N4 / BiOBr.
[0072] Figure 4 The scanning electron microscope (SEM) image of the g-C3N4 / BiOBr composite photocatalyst prepared in Example 2 is shown. Figure 4 It can be seen that increasing the calcination temperature for preparing carbon nitride does not cause a significant change in the morphology of the catalyst, which is still composed of elliptical flake-like nanosheet structures.
[0073] Example 3
[0074] A method for preparing a thermally polymerized g-C3N4 / BiOBr visible light catalytic material, the specific method steps are as follows:
[0075] A certain amount of thiourea was weighed and placed in a ceramic mortar and ground for 5 min to obtain a nitrogen-containing precursor powder. 10 g of the nitrogen-containing precursor powder was weighed and placed in a 100 mL alumina crucible, which was covered and sealed with tin foil and placed in a muffle furnace. The mixture was heated from room temperature at 5 °C min -1The sample was heated to 570°C at a heating rate of 1000 ℃ and kept at this temperature for 2 hours. It was then naturally annealed and cooled to room temperature before being taken out. The fired yellow block solid was ground into yellow powder in a mortar. The obtained substance was g-C3N4.
[0076] Weigh 152.45 mg of powdered g-C3N4 and 1 mmol of Bi(NO3)3·5H2O analytical pure solid (according to the conversion of Bi in Bi(NO3)3 to BiOBr, the mass ratio of g-C3N4:BiOBr is 1:2) in a 150 mL beaker, add 30 mL of ethylene glycol and ultrasonicate for 2 h, and prepare 1 mmol / 20 mL of KBr solution at the same time. After the ultrasonication, transfer the yellow suspension to the stirrer, add a stirrer, and set the speed to 300 r·min -1 , stirred for 2 h, and 20 mL of KBr solution was added dropwise to the yellow suspension while stirring.
[0077] After stirring, the mixture in the beaker was transferred to a 50 mL centrifuge tube and allowed to settle for 12 h. The yellow precipitate was then collected by centrifugation and washed three times with anhydrous ethanol and ultrapure water, respectively. The mixture was then placed in a 60 ° C oven for drying for 12 h, and the dried photocatalyst was ground into powder to obtain g-C3N4 / BiOBr.
[0078] Figure 5 The transmission electron microscope (TEM) image of the g-C3N4 / BiOBr composite photocatalyst prepared in Example 3 is shown, and it can be clearly observed that the BiOBr nanosheets are covered on the g-C3N4, forming a tightly bonded heterojunction interface.
[0079] Figure 6 is the surface chemical state analysis (XPS) of the g-C3N4 / BiOBr composite photocatalyst prepared in Example 3, Figure 6 It is shown that the binding energy of C1s and N1s in the g-C3N4 / BiOBr composite shows an obvious positive shift (0.4–1.0 eV) compared with that of g-C3N4, and the binding energy of Bi 4f shows a slight positive shift compared with that of BiOBr, indicating that the electrons of g-C3N4 migrate to BiOBr after contact.
[0080] The photocatalyst prepared in Example 3 was used in an experiment to degrade methyl orange, and the adsorption and degradation effect on the dye pollutant - methyl orange was studied under simulated light conditions.
[0081] Prepare 0.5M dilute H2SO4 solution and 0.5M NaOH solution as stock solutions for adjusting the initial pH value of the methyl orange reaction solution; weigh different masses of pre-prepared photocatalysts and add them into a 250ml beaker filled with 50mL ultrapure water to prepare 0.1, 0.2, 0.3, 0.5 and 1.0g·L -1 The suspension was placed in an ultrasonic cleaner (frequency 40kHz) for 10 minutes to make the catalyst powder disperse more evenly in the aqueous solution. A magnetic particle was added and the suspension was placed on a magnetic stirrer for stirring; 50 mL of a certain concentration of methyl orange stock solution (prepared immediately before use) was added to make 100 mL of an initial concentration of 10 mg·L -1 The methyl orange reaction solution was added, and the pH value of the reaction solution was adjusted to 6.0; it was stirred for 30 minutes in the dark (the negative time in all the figures in this article represents the adsorption time) to allow the reaction solution to reach an adsorption-desorption dynamic equilibrium; the light source was turned on (the photocurrent was 15A) to carry out photocatalytic degradation reaction, and samples were taken at different fixed time points. 4-5mL of the reaction liquid was drawn into a 5mL centrifuge tube with a disposable dropper, and it was immediately filtered through a 0.22μm aqueous needle filter membrane to separate the catalyst from the pollutant, and then the measurement was carried out.
[0082] Figure 7 The effect of the g-C3N4 / BiOBr catalyst dosage on the photocatalytic process is shown. Figure 7 It can be seen that as the catalyst dosage increases from 0.1 g·L –1 Increase to 1.0 g·L –1 The adsorption and removal rate of methyl orange by g-C3N4 / BiOBr catalyst gradually increased, and the removal rate of methyl orange became faster and faster, indicating that g-C3N4 / BiOBr visible light catalyst has excellent pollutant adsorption capacity and excellent photocatalytic reaction performance.
[0083] The g-C3N4 / BiOBr photocatalyst prepared in Example 3 was used in an experiment to degrade methyl orange. The photocatalytic degradation effect of methyl orange under different pH values was studied under simulated light conditions.
[0084] Prepare 0.5M dilute H2SO4 solution and 0.5M NaOH solution as stock solutions for adjusting the initial pH value of the methyl orange reaction solution; weigh a certain amount of pre-prepared photocatalyst and add it to a 250ml beaker containing 50mL ultrapure water to prepare 0.2g·L -1 The suspension was then placed in an ultrasonic cleaner (frequency 40kHz) for 10 minutes to make the catalyst powder more evenly dispersed in the aqueous solution. A magnetic particle was added and the suspension was stirred on a magnetic stirrer; 50 mL of a certain concentration of methyl orange stock solution (prepared on the spot) was added to make 100 mL of an initial concentration of 10 mg·L-1 methyl orange reaction solution; add different volumes of 0.5M H2SO4 solution and 0.5M NaOH solution to the reaction solution to adjust the methyl orange reaction solution with different pH values (3.0, 4.5, 6.0, 7.5, 9.0). Stir for 30 minutes in the dark (the negative time in all figures in this article represents the adsorption time) to make the reaction solution reach the adsorption-desorption dynamic equilibrium; turn on the light source (photocurrent is 15A) to carry out the photocatalytic degradation reaction, take samples at different fixed times, use a disposable dropper to draw 4-5mL of the reaction liquid into a 5mL centrifuge tube, and immediately use a 0.22μm aqueous needle filter to separate the catalyst from the pollutant, and then measure it.
[0085] The pH value can affect the zeta potential of the catalyst, the dissociation form of methyl orange, and the efficiency of generating active substances. Therefore, it is necessary to evaluate the efficiency of g-C3N4 / BiOBr system in adsorbing methyl orange and photocatalytically degrading methyl orange at different pH values. Figure 8 The catalytic effect diagram of g-C3N4 / BiOBr visible light photocatalyst for degradation of methyl orange at different pH values. Figure 8 As shown in the figure, as the pH value increases from 3.0 to 9.0, the adsorption removal rates are 21.66%, 10.58%, 15.80%, 6.28% and 6.75%, respectively; after 30 minutes of degradation, the removal efficiency of MO can reach more than 80%, that is, under acidic and alkaline conditions, the g-C3N4 / BiOBr photocatalytic system has a high degradation rate.
[0086] The g-C3N4 / BiOBr prepared in Example 3 was used as a photocatalyst. Under simulated light conditions, methyl orange was used as a typical dye pollutant to explore the main active substances in the g-C3N4 / BiOBr photocatalytic system.
[0087] IPA, KBrO3, EDTA-2Na, and BQ were used as active species in the capture system. – 、h + , ·O 2– The initial pH value was 6.0 and the dosage of g-C3N4 / BiOBr photocatalyst was 0.2 g·L -1 , methyl orange concentration is 10 mg·L -1 The quenching experiment of photocatalytic degradation of methyl orange was carried out.
[0088] Prepare 0.5M dilute H2SO4 solution and 0.5M NaOH solution as stock solutions for adjusting the initial pH value of the methyl orange reaction solution; weigh a certain amount of pre-prepared photocatalyst and add it to a 250ml beaker containing 50mL ultrapure water to prepare 0.2g·L -1The suspension was then placed in an ultrasonic cleaner (frequency 40kHz) for 10 minutes to make the catalyst powder more evenly dispersed in the aqueous solution. A magnetic particle was added and the suspension was stirred on a magnetic stirrer; 50 mL of a certain concentration of methyl orange stock solution (prepared on the spot) was added to make 100 mL of an initial concentration of 10 mg·L -1 methyl orange reaction solution; add different volumes of 0.5M H2SO4 solution and 0.5M NaOH solution to the reaction solution to adjust the pH value of 6 to obtain a methyl orange reaction solution. Then add 1mmol of IPA, KBrO3, EDTA-2Na, and BQ as quenchers, stir for 30min in the dark (negative time in all figures in this article represents adsorption time) to make the reaction solution reach adsorption-desorption dynamic equilibrium; turn on the light source (photocurrent is 15A) to carry out photocatalytic degradation reaction, take samples at different fixed times, use a disposable dropper to draw 4-5mL of reaction liquid into a 5mL centrifuge tube, and immediately use a 0.22μm aqueous needle filter to separate the catalyst from the pollutant, and then measure it.
[0089] Fig. 9 The figure shows the active species capture kinetics experiment of g-C3N4 / BiOBr in the visible light catalytic degradation of methyl orange and the comparison of degradation rate constant and removal rate. Fig. 9 It can be seen that h + and · O2 – It plays a major role in the visible light photocatalytic degradation of methyl orange; in the g-C3N4 / BiOBr visible light photocatalytic system, e – and · Involvement of OH.
[0090] The free radicals and holes generated by the catalyst were tested using an EMXplus-6 / 1 electron paramagnetic resonance (EPR) instrument from Bruker, Germany, under 300W xenon lamp irradiation. · OH) and superoxide radicals ( · O2 – ) Using DMPO capture agent, holes (h + ) The capture agent is TEMPO. Take 30 μL of sample, add 30 μL of DMPO (100 mM methanol as solvent), mix well, draw a certain amount of the mixture with a capillary, put it in a quartz tube, and put it into the EPR sample chamber for · O2 – Similarly, · OH uses water as solvent, and the other experimental conditions are the same as · O2 – The sample height in the paramagnetic tube is less than 1 cm, and the peak intensity in the measured results is normalized by mass.
[0091] Fig.10 This is the EPR spectrum of g-C3N4 / BiOBr under visible light excitation. Fig.10 It can be seen that g-C3N4 / BiOBr can simultaneously produce · O2 – and · According to the active species capture experiment and EPR characterization results, h + 、e – , · O2 – , · OH four active species, the contribution order is: h + > · O2 – >e – > · OH. In summary, h + and · O2 – It plays a major role in the visible light photocatalytic degradation of methyl orange. – and · OH is also involved to some extent.
[0092] Using g-C3N4 / BiOBr prepared in Example 3 as a photocatalyst, the adsorption and degradation effect of the photocatalytic system on different dye pollutants was studied under simulated light conditions.
[0093] Prepare 0.5M dilute H2SO4 solution and 0.5M NaOH solution as stock solutions; weigh a certain mass of the pre-prepared photocatalyst and add it to a 250mL beaker filled with 50mL ultrapure water to prepare a 0.2g / L suspension, then put it into an ultrasonic cleaner (frequency 40kHz) for 10 minutes to make the catalyst powder disperse more evenly in the aqueous solution. Add a magnet and stir the suspension on a magnetic stirrer; add 50mL of a certain concentration of active black 5, active blue 4, active yellow 145, Ponceau S, and Alizarin Red S stock solutions (prepared as needed) to prepare 100mL of a series of initial concentrations (5, 10, 20, 50mg·L –1 ) and adjust the initial pH value to 6.0; stir in the dark for 30 min (negative time in all figures in this article represents adsorption time) to allow the reaction solution to reach adsorption-desorption dynamic equilibrium. Turn on the light source (photocurrent is 15A) to carry out photocatalytic degradation reaction, and take samples at different fixed times, that is, use a disposable dropper to draw 4-5 mL of the reaction liquid into a 5 mL centrifuge tube, and immediately use a 0.22 μm aqueous needle filter to separate the catalyst from the pollutant, and then measure it.
[0094] Fig.11 The photocatalytic degradation rate constants of various dyes at different concentrations in the g-C3N4 / BiOBr photocatalytic system are shown. The adsorption removal rates of different dyes within 30 min under different concentration conditions are as follows: anthraquinone dyes (Reactive Blue 4, Alizarin Red S) > monoazo dyes (Reactive Yellow 145) > disazo dyes (Reactive Black 5, Ponceau S). The photodegradation rate constant k decreases with the increase of dye concentration: (1) The order of photocatalytic degradation rate: anthraquinone dyes (Reactive Blue 4, Alizarin Red S) > disazo dyes (Reactive Black 5, Ponceau S) > monoazo dyes (Reactive Yellow 145); (2) 20 mg·L -1 Complete degradation time of dye concentration: anthraquinone (within 20 minutes) < disazo (within 45 minutes) < monoazo (within 60 minutes), 50 mg·L -1 The anthraquinone dyes in the g-C3N4 / BiOBr visible light catalytic system can completely degrade different dyes of different concentrations in a short time, and has excellent photocatalytic performance.
[0095] Although the preferred embodiments of the present invention have been described above in conjunction with the accompanying drawings, the present invention is not limited to the above-mentioned specific embodiments, which are merely illustrative and not restrictive. Under the guidance of the present invention, ordinary technicians in this field can also make many forms of specific changes without departing from the scope of protection of the present invention and the claims, all of which fall within the scope of protection of the present invention.
Claims
1. A gC 3 N 4 / BiOBr visible light photocatalytic material, It is characterized in that Obtained by the following preparation method: (1) Synthesis of gC by thiourea low temperature pyrolysis 3 N 4 Materials, reaction temperature is 550℃-570℃; (2) The powdery gC obtained in step (1) 3 N 4 Materials and Bi(NO 3 ) 3 ·5H 2 O solid mixture, then add ethylene glycol to immerse, and mix evenly by ultrasonication; (3) Adding a certain amount of KBr aqueous solution dropwise to the mixed solution obtained in step (2) while rapidly stirring, and continuing to stir until the mixture is uniformly mixed; (4) After the mixed solution obtained in step (3) is allowed to settle, the yellow precipitate is collected by centrifugation, washed and dried, and the dried powder is gC 3 N 4 / BiOBr composites.
2. A gC according to claim 1 3 N 4 / BiOBr visible light photocatalytic material, It is characterized in that The step (1) comprises: using nitrogen-containing precursor thiourea as raw material, first grinding it into a uniform powder, then heating it to 550°C-570°C and maintaining it for 2-3 hours; then naturally annealing and cooling to room temperature, then taking it out, and grinding the fired yellow block solid into powder, namely gC 3 N 4 Material.
3. A gC according to claim 1 3 N 4 / BiOBr visible light photocatalytic material, It is characterized in that In the step (2), according to Bi(NO 3 ) 3 Bi can generate BiOBr conversion, gC 3 N 4 The mass ratio of BiOBr is 1:10-1:
2.
4. A gC according to claim 1 3 N 4 / BiOBr visible light photocatalytic material, It is characterized in that In step (3), the speed of rapid stirring is 300-350 r·min -1 .
5. A gC according to claim 1 3 N 4 / BiOBr visible light photocatalytic material, It is characterized in that In the step (3), the amount of bromide ions in the KBr aqueous solution is equal to the amount of Bi(NO 3 ) 3 ·5H 2 The amount of Bi element in the O solid is equal.
6. A gC according to claim 1 3 N 4 / BiOBr visible light photocatalytic material, It is characterized in that In the step (4), the mixed solution is allowed to stand for precipitation for 12-14 hours.
7. A gC according to claim 1 3 N 4 / BiOBr visible light photocatalytic material, It is characterized in that In the step (4), washing is performed by washing with anhydrous ethanol and ultrapure water three times respectively.
8. A gC according to claim 1 3 N 4 / BiOBr visible light photocatalytic material, It is characterized in that In the step (4), the drying is performed at 40-60° C. for 12-24 hours.
9. A gC 3 N 4 / Preparation method of BiOBr visible light catalytic material, It is characterized in that The steps include: (1) Synthesis of gC by thiourea low temperature pyrolysis 3 N 4 Materials, reaction temperature is 550℃-570℃; (2) The powdery gC obtained in step (1) 3 N 4 Materials and Bi(NO 3 ) 3 ·5H 2 O solid mixture, then add ethylene glycol to immerse, and mix evenly by ultrasonication; (3) Adding a certain amount of KBr aqueous solution dropwise to the mixed solution obtained in step (2) while rapidly stirring, and continuing to stir until the mixture is uniformly mixed; (4) After the mixed solution obtained in step (3) is allowed to settle, the yellow precipitate is collected by centrifugation, washed and dried, and the dried powder is gC 3 N 4 / BiOBr composites.
Citation Information
Patent Citations
Preparation method of two-dimensional Z type heterojunction visible light photocatalyst
CN109759121A
Flower-like g-C3N4 / g-C3N4 / BiOBr ternary heterojunction photocatalytic material and preparation method thereof
CN110639586A
S-doped BiOBr nano photocatalyst, and preparation and application thereof
CN110773204A