Co-C-N catalyst and preparation method and application thereof

By preparing Co-C-N catalysts, using the mixing and stirring and calcining method of cobalt source, zinc source and 2-methylimidazole, the existing catalysts have been solved, and efficient formaldehyde degradation and long activity are achieved at room temperature. , low cost effect.

CN119016085AActive Publication Date: 2024-11-26INST OF URBAN ENVIRONMENT CHINESE ACAD OF SCI

Patent Information

Application Number
CN202411130127.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-26
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

In the prior art, the catalyst used for formaldehyde removal has a short life, poor activity and high cost, making it difficult to meet the needs of low cost, high activity and high stability.

Method used

Using the preparation method of Co-C-N catalyst, the surface layered Co-C-N catalyst is prepared by mixing cobalt source, zinc source and 2-methylimidazole and sonicating, stirring and calcining, and the surface layered distribution is prepared for formaldehyde degradation at room temperature. .

Benefits of technology

Excellent catalytic degradation performance of formaldehyde at room temperature is achieved, and the activity of the catalyst is maintained for a long time, is low in cost, and is even better than many precious metal catalysts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016085A_ABST
    Figure CN119016085A_ABST
Patent Text Reader

Abstract

The invention provides a Co-C-N catalyst as well as a preparation method and application thereof. The preparation method comprises the following steps: (1) uniformly mixing a cobalt source, a zinc source and water, performing secondary mixing with 2-methylimidazole, and then sequentially performing ultrasonic treatment, stirring treatment and solid-liquid separation to obtain a ZnCo-MOF material; and (2) sequentially carrying out cleaning, drying treatment and roasting treatment on the ZnCo-MOF material obtained in the step (1) to obtain the Co-C-N catalyst. The Co-C-N catalyst prepared through simple mixing, stirring and roasting can completely degrade formaldehyde into water and carbon dioxide at room temperature, the preparation process is simple, the cost is low, and the service life is long.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalysts and relates to a Co-based catalyst, in particular to a Co-CN catalyst and a preparation method and application thereof. Background Art

[0002] Currently, formaldehyde has been identified as a possible carcinogen by the U.S. Environmental Protection Agency and as a Class 1 carcinogen by the International Agency for Research on Cancer under the World Health Organization. Formaldehyde is widely released from building materials, decorative items, and furniture materials. In order to comply with increasingly stringent environmental protection laws and regulations and meet people's pursuit of a higher quality of life, effectively removing indoor formaldehyde gas has become an urgent problem to be solved.

[0003] Currently, the most commonly used formaldehyde treatment technology is mainly activated carbon adsorption absorption technology, but the traditional adsorption and absorption control technology only transfers pollutants from the gas phase to the solid phase, and does not achieve true removal. In addition, the adsorption capacity of the adsorption material is limited and needs to be regenerated or replaced regularly, which is prone to secondary pollution. Therefore, it is often difficult to meet the national indoor air quality standards in actual applications. Different from the traditional adsorption / absorption formaldehyde removal technology, the formaldehyde room temperature catalytic oxidation technology uses the catalyst's own lattice oxygen or activated adsorbed oxygen to start the catalytic reaction, and achieves harmless treatment of formaldehyde complete decomposition at room temperature. It has the characteristics of high efficiency and environmental protection, and has broad application prospects.

[0004] CN 103736484A discloses a supported monolithic catalyst for formaldehyde purification and a preparation method thereof, wherein the catalyst is composed of a titanium dioxide nanotube array carrier and a noble metal M, wherein the noble metal M is one or a mixture of at least two of Pt, Ru, Rh, Pd, and Au. The preparation method comprises the following steps: impregnating a precursor solution containing the noble metal onto the titanium dioxide nanotube array carrier, calcining to obtain a catalyst loaded with the noble metal component, and then reducing the catalyst with hydrogen or a reducing solution to directly catalyze and purify formaldehyde. However, the catalyst has a short life and relatively poor activity.

[0005] CN 106040230A discloses a method for preparing an integrated catalyst for low-temperature catalytic oxidation of formaldehyde. The method comprises: anodizing an aluminum plate and then hydrating it in deionized water at 30-95°C for 5-70 minutes to obtain a boehmite; placing the boehmite in a chloroplatinic acid solution with a concentration of 0.1-0.8 g / L, immersing it at 25°C for 1-8 hours, and drying it at room temperature for 12 hours; then reducing it in a sodium borohydride solution with a concentration of 0.05-1 mol / L at 25°C for 0.5-3 hours, and drying it at room temperature; when the platinum content is 22.5wt%, the formaldehyde conversion rate reaches 72% at room temperature, and the noble metal content is relatively high, which increases the cost and is not conducive to promotion.

[0006] Although supported noble metal (Pt, Au, Pd) catalysts can efficiently degrade formaldehyde at room temperature, their high cost limits their widespread application. Non-noble metal catalysts are inexpensive and easy to use, but their performance in degrading formaldehyde at room temperature is poor compared to supported noble metal catalysts. In order to further improve the room temperature performance of non-noble metal catalysts, it is urgent to propose a synthesis scheme for new non-noble metal catalysts.

[0007] MOF materials have a three-dimensional structure, a large specific surface area, and a rich and complex pore structure, which provide ample space for the adsorption and reaction of gas molecules. Two-dimensional materials are a class of materials with special structural properties. Electrons move in a two-dimensional plane, providing multiple possibilities for reactions. MOF and two-dimensional materials and their derivatives can flexibly adjust the active sites, interface structures, spatial confinement, etc. of catalysts. They have excellent electron transfer capabilities, which facilitate the optimization of the electronic structure of active metals and make them develop in the optimal structural direction of redox active substances, thereby improving the intrinsic activity of catalytic reactions and increasing the density and accessibility of active sites.

[0008] In summary, it is necessary to provide a low-cost, highly active and highly stable catalyst that can be widely used in indoor formaldehyde removal. Summary of the invention

[0009] The purpose of the present invention is to provide a Co-CN catalyst and its preparation method and application. At room temperature, the Co-CN catalyst has excellent catalytic degradation ability for formaldehyde, even better than many precious metal catalysts; and the catalyst raw materials are cheap and easy to obtain, the preparation method is simple, and the overall process cost is low.

[0010] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0011] In a first aspect, the present invention provides a method for preparing a Co-CN catalyst, the preparation method comprising the following steps:

[0012] (1) After the cobalt source, the zinc source and the solvent are uniformly mixed, 2-methylimidazole is mixed for a second time, and then ultrasonic treatment, stirring treatment and solid-liquid separation are sequentially performed to obtain a ZnCo-MOF material;

[0013] (2) The ZnCo-MOF material obtained in step (1) is sequentially cleaned, dried and calcined to obtain the Co-CN catalyst.

[0014] The present invention can prepare an irregular polyhedral ZnCo-MOF material through a simple mixing and stirring method, and the outer surface presents a two-dimensional layered structure, and then obtain a Co-CN catalyst with a layered distribution on the surface through calcination; the Co-CN catalyst has excellent performance in degrading formaldehyde at room temperature and maintains its activity for a long time.

[0015] In the present invention, when water or ethanol is used as the solvent, the amine N of 2-methylimidazole (2-MIM) is more inclined to form hydrogen bonds with hydrated protons (this is because the dissociation constant of 2-MIM in water is lower), which leads to the formation of Co 2+ The cross-linking between 2-MIM and 2-MIM forms connected building units and irregular stacking structures.

[0016] As a preferred technical solution of the present invention, the cobalt source in step (1) includes cobalt nitrate.

[0017] Preferably, the zinc source in step (1) comprises zinc nitrate and / or zinc acetate.

[0018] As a preferred technical solution of the present invention, the molar mass ratio of the cobalt source, the zinc source and the 2-methylimidazole in step (1) is 40:480:1 to 20, for example, it can be 40:480:1, 40:480:4, 40:480:8, 40:480:12, 40:480:16 or 40:480:20, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0019] Preferably, the solvent in step (1) comprises water or ethanol.

[0020] Preferably, the solid-to-liquid ratio of the total mass of the cobalt source and the zinc source to the solvent in step (1) is 0.76 g:50-70 mL, for example, 0.76 g:50 mL, 0.76 g:54 mL, 0.76 g:58 mL, 0.76 g:62 mL, 0.76 g:66 mL or 0.76 g:70 mL, but is not limited to the listed values, and other values ​​not listed within the numerical range are equally applicable.

[0021] As a preferred technical solution of the present invention, the mixing temperature in step (1) is 25-35°C, for example, it can be 25°C, 27°C, 29°C, 31°C, 33°C or 35°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0022] Preferably, the ultrasonic treatment time in step (1) is 20 to 40 min, for example, 20 min, 24 min, 28 min, 32 min, 36 min or 40 min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0023] In the present invention, the ultrasonic treatment can make the cobalt source and the zinc source in the solvent fully mixed and uniform, which is more conducive to the appearance of the layered structure.

[0024] Preferably, the stirring time in step (1) is 12 to 48 hours, for example, 12 hours, 16 hours, 20 hours, 24 hours, 28 hours, 32 hours, 36 hours, 40 hours, 44 hours or 48 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0025] Preferably, the rotation speed of the stirring treatment in step (1) is 8000-10000 r / min, for example, it can be 8000 r / min, 8400 r / min, 8800 r / min, 9200 r / min, 9600 r / min or 10000 r / min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0026] Preferably, the solid-liquid separation in step (1) comprises centrifugation.

[0027] As a preferred technical solution of the present invention, the cleaning solution used in step (2) comprises ethanol.

[0028] As a preferred technical solution of the present invention, the drying treatment in step (2) includes vacuum drying.

[0029] Preferably, the vacuum drying temperature is 60-80°C, for example, 60°C, 64°C, 68°C, 72°C, 76°C or 80°C, but is not limited to the listed values.

[0030] Preferably, the vacuum drying time is 10 to 12 hours, for example, 10 hours, 10.4 hours, 10.8 hours, 11.2 hours, 11.6 hours or 12 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0031] As a preferred technical solution of the present invention, the calcination treatment in step (2) is carried out under an inert gas atmosphere.

[0032] Preferably, the inert gas comprises any one of nitrogen, argon or helium, or a combination of at least two of them. Typical but non-limiting combinations include: a combination of nitrogen and argon, a combination of argon and helium, a combination of nitrogen and helium, or a combination of nitrogen, argon and helium.

[0033] Preferably, the temperature of the calcination treatment in step (2) is 900-1050°C, for example, 900°C, 940°C, 980°C, 1020°C or 1050°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0034] Preferably, the calcination time in step (2) is 1 to 3 h, for example, 1 h, 1.2 h, 1.4 h, 1.6 h, 1.8 h, 2 h, 2.2 h, 2.4 h, 2.6 h, 2.8 h or 3 h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0035] In the present invention, the purpose of the calcination treatment is to remove the Zn element in the ZnCo-MOF material. If the calcination temperature is too low, it will be difficult to remove the Zn element completely and a high-performance Co-CN catalyst cannot be formed. If the calcination temperature is too high, the three-dimensional structure of the catalyst will be affected, and pore collapse and / or Co atom agglomeration may occur, resulting in reduced activity of the catalyst.

[0036] As a preferred technical solution of the present invention, the preparation method of the Co-CN catalyst provided in the first aspect of the present invention comprises the following steps:

[0037] (1) mixing a cobalt source (cobalt nitrate), a zinc source (zinc nitrate) and a solvent at 25 to 35° C., then mixing 2-methylimidazole for a second time, and then performing ultrasonic treatment for 20 to 40 minutes, stirring at a speed of 8000 to 10000 r / min for 12 to 48 hours, and solid-liquid separation to obtain a ZnCo-MOF material;

[0038] The molar mass ratio of the cobalt source, the zinc source and the 2-methylimidazole is 40:480:1-20; the solid-liquid ratio of the total mass of the cobalt source and the zinc source to the solvent is 0.76g:50-70mL;

[0039] (2) The ZnCo-MOF material obtained in step (1) is washed with ethanol, dried at 60 to 80° C. for 10 to 12 h, and then calcined at 900 to 1050° C. for 1 to 3 h in an inert gas atmosphere to obtain the Co-CN catalyst.

[0040] In a second aspect, the present invention provides a Co-CN catalyst, which is obtained by the preparation method provided in the first aspect.

[0041] In a third aspect, the present invention provides an application of a Co-CN catalyst prepared by the preparation method of the first aspect, wherein the Co-CN catalyst is used to degrade formaldehyde.

[0042] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0043] Compared with the prior art, the present invention has the following beneficial effects:

[0044] (1) The Co-CN catalyst provided by the present invention has excellent room temperature activity, even better than most precious metal catalysts, and can be widely used as indoor formaldehyde removal catalyst;

[0045] (2) The Co-CN catalyst provided by the present invention has excellent selectivity for CO2, and the product has no secondary pollution;

[0046] (3) The raw materials for preparing the Co-CN catalyst provided by the present invention are cheap and readily available, the preparation method is simple, and the overall process cost is low. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 SEM images of the ZnCo-MOF material provided in Example 1 of the present invention at different magnifications;

[0048] Figure 2 SEM images of the Co-CN catalyst provided in Example 1 of the present invention at different magnifications;

[0049] Figure 3 is a TEM image of the Co-CN catalyst provided in Example 1 of the present invention;

[0050] Figure 4 This is a graph showing the test results of catalytic oxidation of formaldehyde by the Co-CN catalyst provided in Example 1 of the present invention. DETAILED DESCRIPTION

[0051] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0052] Example 1

[0053] This embodiment provides a Co-CN catalyst, and the preparation method of the Co-CN catalyst comprises the following steps:

[0054] (1) After uniformly mixing a cobalt source, a zinc source and 60 mL of water at 30° C., 2-methylimidazole was mixed for a second time, and then ultrasonic treatment was performed for 30 min, stirring treatment was performed at a speed of 9000 r / min for 36 h, and solid-liquid separation was performed in sequence to obtain a ZnCo-MOF material;

[0055] The molar mass ratio of the cobalt source, the zinc source and the 2-methylimidazole is 40:480:10; the solid-liquid ratio of the total mass of the cobalt source and the zinc source to the solvent is 0.76 g:60 mL;

[0056] (2) The ZnCo-MOF material obtained in step (1) was washed with ethanol, dried at 70° C. for 11 h, and then calcined at 1000° C. for 2 h in an inert gas atmosphere to obtain the Co-CN catalyst.

[0057] The SEM images of the ZnCo-MOF material obtained in step (1) of this embodiment at different magnifications are as follows: Figure 1 As shown, the SEM images of the Co-CN catalyst obtained in step (2) at different magnifications are as follows Figure 2 As shown in the TEM image Figure 3 shown.

[0058] according to Figure 1 It can be seen that the microstructure of the ZnCo-MOF material is an irregular polyhedron, and its outer surface is a two-dimensional layered structure; Figure 2 and Figure 3 It can be seen that the microstructure of the Co-CN catalyst provided in this embodiment is an irregular polyhedron.

[0059] Example 2

[0060] This embodiment provides a Co-CN catalyst, and the preparation method of the Co-CN catalyst comprises the following steps:

[0061] (1) After uniformly mixing a cobalt source (cobalt nitrate), a zinc source (zinc nitrate) and ethanol at 25°C, 2-methylimidazole was added for a second time, and then ultrasonic treatment was performed for 40 minutes, stirring was performed at a speed of 10000 r / min for 12 hours, and solid-liquid separation was performed in sequence to obtain a ZnCo-MOF material;

[0062] The molar mass ratio of the cobalt source, the zinc source and the 2-methylimidazole is 40:480:1; the solid-liquid ratio of the total mass of the cobalt source and the zinc source to the solvent is 0.76 g:50 mL;

[0063] (2) The ZnCo-MOF material obtained in step (1) was washed with ethanol, dried at 60° C. for 12 h, and then calcined at 900° C. for 3 h in an inert gas atmosphere to obtain the Co-CN catalyst.

[0064] Example 3

[0065] This embodiment provides a Co-CN catalyst, and the preparation method of the Co-CN catalyst comprises the following steps:

[0066] (1) After uniformly mixing a cobalt source (cobalt nitrate), a zinc source (zinc acetate) and water at 35°C, 2-methylimidazole was added for a second time, and then ultrasonic treatment was performed for 20 minutes, stirring was performed at a speed of 8000 r / min for 48 hours, and solid-liquid separation was performed in sequence to obtain a ZnCo-MOF material;

[0067] The molar mass ratio of the cobalt source, the zinc source and the 2-methylimidazole is 40:480:20; the solid-liquid ratio of the total mass of the cobalt source and the zinc source to the solvent is 0.76 g:70 mL;

[0068] (2) The ZnCo-MOF material obtained in step (1) was washed with ethanol, dried at 80° C. for 12 h, and then calcined at 1050° C. for 1 h in an inert gas atmosphere to obtain the Co-CN catalyst.

[0069] Example 4

[0070] This embodiment provides a Co-CN catalyst, and the preparation method of the Co-CN catalyst is different from that of Embodiment 1 only in that:

[0071] In this example, the molar mass ratio of the cobalt source, the zinc source and the 2-methylimidazole in step (1) is adjusted to 200:480:20.

[0072] Example 5

[0073] This embodiment provides a Co-CN catalyst, and the preparation method of the Co-CN catalyst is different from that of Embodiment 1 only in that:

[0074] In this embodiment, the temperature of the calcination treatment in step (2) is adjusted to 850°C.

[0075] Example 6

[0076] This embodiment provides a Co-CN catalyst, and the preparation method of the Co-CN catalyst is different from that of Embodiment 1 only in that:

[0077] In this embodiment, the temperature of the calcination treatment in step (2) is adjusted to 1100°C.

[0078] Example 7

[0079] This embodiment provides a Co-CN catalyst, and the preparation method of the Co-CN catalyst is different from that of Embodiment 1 only in that:

[0080] In this embodiment, the calcination time in step (2) is adjusted to 0.5 h.

[0081] Example 8

[0082] This embodiment provides a Co-CN catalyst, and the preparation method of the Co-CN catalyst is different from that of Embodiment 1 only in that:

[0083] In this embodiment, the calcination time in step (2) is adjusted to 3.5 hours.

[0084] Comparative Example 1

[0085] This comparative example provides a Co-CN catalyst, and the preparation method of the Co-CN catalyst is different from that of Example 1 only in that:

[0086] In this comparative example, the ultrasonic treatment process described in step (1) was omitted.

[0087] Comparative Example 2

[0088] This comparative example provides a Co-CN catalyst, and the preparation method of the Co-CN catalyst is different from that of Example 1 only in that:

[0089] In this comparative example, the mixing process of step (1) is adjusted as follows: (a) mixing cobalt nitrate, water and 2-methylimidazole to obtain a first mixed solution; (b) mixing zinc nitrate, water and 2-methylimidazole to obtain a second mixed solution; and (c) mixing the first mixed solution and the second mixed solution.

[0090] Comparative Example 3

[0091] This comparative example provides a catalyst, which is a noble metal catalyst for catalytic oxidation of formaldehyde provided in Example 1 of Chinese patent CN 115301231A.

[0092] The catalysts provided in the above examples and comparative examples were used to catalyze the degradation of formaldehyde, and the test method was as follows:

[0093] 30 mg of catalyst was placed in a fixed bed reactor, the temperature was controlled at 25°C, the relative humidity was 35%, He was used as the balance gas, the total flow rate was 100 mL / min, and the test was carried out at a space velocity of 200,000 mL / (g·h). The initial concentration of formaldehyde was 115 ppm. The concentration of formaldehyde in the gas after 150 hours of catalysis was tested, and the formaldehyde removal rate was calculated. The results are shown in Table 1.

[0094] In addition, the test results of the catalytic oxidation of formaldehyde by the Co-CN catalyst provided in Example 1 are shown in FIG. Figure 4 shown.

[0095] Table 1

[0096] Formaldehyde conversion rate after 150h / % Example 1 100 Example 2 92 Example 3 94 Example 4 42 Example 5 0 Example 6 35 Example 7 60 Example 8 85 Comparative Example 1 88 Comparative Example 2 85 Comparative Example 3 87

[0097] From Table 1, we can see the following points:

[0098] (1) Comprehensive analysis of Examples 1-3 shows that the Co-CN catalyst provided by the present invention can completely degrade formaldehyde into water and carbon dioxide at room temperature, has a simple preparation process, does not involve precious metal loading, has low cost and a long service life;

[0099] according to Figure 4 It can be seen that the catalyst provided by the present invention can maintain the formaldehyde conversion rate above 95% within 300 hours;

[0100] (2) Comprehensive analysis of Example 1 and Example 4 shows that the molar ratio of the Co element in Example 4 is too high, which easily forms larger Co particles and fails to form an effective reaction interface, resulting in a decrease in its formaldehyde catalytic activity;

[0101] (3) Comprehensive analysis of Example 1 and Examples 5-8 shows that the parameters of the calcination treatment will affect the catalytic effect of the obtained catalyst on formaldehyde;

[0102] When the calcination temperature is too high (such as in Example 5), the internal structure of the catalyst will collapse; when the calcination temperature is too low (such as in Example 6), the zinc element cannot be completely removed;

[0103] When the calcination time is too short (such as in Example 7), the zinc element cannot be completely removed; when the calcination time is too long (such as in Example 8), the structure collapses;

[0104] (4) Comprehensive analysis of Example 1 and Comparative Example 1 shows that the ultrasonic treatment process is very important for the formation of the structure; if the ultrasonic treatment is omitted, a layered structure will be formed on the surface, but a two-dimensional structure cannot be formed;

[0105] (5) Comprehensive analysis of Example 1 and Comparative Example 3 shows that, compared with precious metal catalysts, although the catalyst provided by the present invention does not contain precious metals, its catalytic effect is even better than that of precious metal catalysts.

[0106] In summary, the Co-CN catalyst prepared by simple mixing, stirring and calcining in the present invention can completely degrade formaldehyde into water and carbon dioxide at room temperature, and has a simple preparation process, low cost and long service life.

[0107] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a Co-CN catalyst, characterized in that: The preparation method comprises the following steps: (1) After the cobalt source, the zinc source and the solvent are uniformly mixed, 2-methylimidazole is mixed for a second time, and then ultrasonic treatment, stirring treatment and solid-liquid separation are sequentially performed to obtain a ZnCo-MOF material; (2) The ZnCo-MOF material obtained in step (1) is sequentially cleaned, dried and calcined to obtain the Co-CN catalyst.

2. The preparation method according to claim 1, characterized in that: The cobalt source in step (1) comprises cobalt nitrate; Preferably, the zinc source in step (1) comprises zinc nitrate and / or zinc acetate.

3. The preparation method according to claim 1 or 2, characterized in that: The molar mass ratio of the cobalt source, the zinc source and the 2-methylimidazole in step (1) is 40:480:1-20; Preferably, the solvent in step (1) comprises water or ethanol; Preferably, the liquid-to-solid ratio of the solvent to the total mass of the cobalt source and the zinc source in step (1) is 50-70 mL:0.76 g.

4. The preparation method according to any one of claims 1 to 3, characterized in that: The mixing temperature in step (1) is 25 to 35° C. Preferably, the ultrasonic treatment time in step (1) is 20 to 40 minutes; Preferably, the stirring time in step (1) is 12 to 48 hours; Preferably, the speed of the stirring treatment in step (1) is 8000-10000 r / min; Preferably, the solid-liquid separation in step (1) comprises centrifugation.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The cleaning solution used in step (2) includes ethanol.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The drying process in step (2) includes vacuum drying; Preferably, the vacuum drying temperature is 60-80°C; Preferably, the vacuum drying time is 10 to 12 hours.

7. The preparation method according to any one of claims 1 to 6, characterized in that: The calcination treatment in step (2) is carried out under an inert gas atmosphere; Preferably, the inert gas comprises any one of nitrogen, argon or helium, or a combination of at least two thereof; Preferably, the temperature of the calcination treatment in step (2) is 900-1050°C; Preferably, the calcination time in step (2) is 1 to 3 hours.

8. The preparation method according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: (1) After uniformly mixing a cobalt source, a zinc source and a solvent at 25 to 35° C., 2-methylimidazole is mixed for a second time, and then ultrasonic treatment is performed for 20 to 40 minutes, stirring treatment is performed at a speed of 8000 to 10000 r / min for 12 to 48 hours, and solid-liquid separation is performed in sequence to obtain a ZnCo-MOF material; The molar mass ratio of the cobalt source, the zinc source and the 2-methylimidazole is 40:480:1-20; the solid-liquid ratio of the total mass of the cobalt source and the zinc source to the solvent is 0.76g:50-70mL; (2) The ZnCo-MOF material obtained in step (1) is washed with ethanol, dried at 60 to 80° C. for 10 to 12 h, and then calcined at 900 to 1050° C. for 1 to 3 h in an inert gas atmosphere to obtain the Co-CN catalyst.

9. A Co-CN catalyst, characterized in that The Co-CN catalyst is obtained by the preparation method according to any one of claims 1 to 8.

10. Use of the Co-CN catalyst as claimed in claim 9, characterized in that: The Co-CN catalyst is used for catalytic degradation of formaldehyde.

Citation Information

Patent Citations

  • Supported integrated catalyst for formaldehyde purification and preparation method thereof

    CN103736484A

  • Method for preparing integrated catalyst for low-temperature catalytic oxidation of formaldehyde

    CN106040230A

  • Precious metal catalyst for catalytic oxidation of formaldehyde and preparation method thereof

    CN115301231A

  • Catalyst for VIII group single atomic dispersion and preparation method thereof

    CN108242549A

  • Porous nitrogen-doped carbon material-loaded bicrystal phase cobalt-based catalyst as well as preparation and application thereof

    CN114797925A

Cited By

  • Preparation method and application of surface hydroxylation monatomic catalyst with Co-O-Zn structure