Composite catalyst for preparing olefin through CO2 / CO hydrogenation as well as preparation method and application of composite catalyst

By constructing a composite catalyst with both hydrophobic and hydrophilic surface structures and adjusting the contents of Fe3O4 and Fe5C2, the problem of difficult control of the active components of iron-based catalysts was solved, and a highly efficient CO2/CO hydrogenation to olefins reaction was achieved, which has good prospects for industrialization.

CN119016112APending Publication Date: 2024-11-26SHANGHAI INST OF CERAMIC CHEM & TECH CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310550526.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The active component Fe5C2 in existing iron-based catalysts is difficult to control, and the catalyst stability needs to be improved, resulting in poor efficiency of CO2 to CO conversion. The byproduct water oxidation catalyst reduces its activity and is difficult to meet the requirements of large-scale industrial production.

Method used

By physically mixing surface hydrophobic catalysts and surface hydrophilic catalysts, a composite catalyst with hydrophobic and hydrophilic structures was constructed. The contents of active components Fe3O4 and Fe5C2 were adjusted to promote the rapid removal of H2O from the catalyst surface, enhance the mass transfer process, and improve the activity and stability of the catalyst.

Benefits of technology

It achieves a highly active and stable CO2/CO hydrogenation to olefins reaction, with a CO2 conversion rate of over 50% and an olefin selectivity of over 65%, significantly improving the performance of the catalyst and making it suitable for large-scale industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016112A_ABST
    Figure CN119016112A_ABST
Patent Text Reader

Abstract

The invention relates to a CO2 / CO hydrogenation olefin composite catalyst and a preparation method and application thereof. The composite catalyst for preparing olefin through CO2 / CO hydrogenation is characterized by being prepared by physically mixing and granulating a surface hydrophobic catalyst and a surface hydrophilic catalyst, the surface hydrophilic catalyst is nano iron oxide particles compounded by transition metal oxide modified by alkali metal oxide; the surface hydrophobic catalyst comprises nano iron oxide particles which are coated with surface hydrophobic material modified mesoporous oxide layers and are compounded with transition metal oxides modified by alkali metal oxides.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a composite catalyst composed of a surface hydrophobic structure and a surface hydrophilic structure, a preparation method thereof and application thereof in CO2 / CO hydrogenation to olefins, belonging to the technical field of CO2 / CO hydrogenation direct process to olefins. Background Art

[0002] With the widespread use of energy sources such as oil, coal and natural gas, humans have emitted a huge amount of carbon dioxide into the atmosphere, leading to a series of ecological and environmental problems, such as climate warming and ocean acidification. Carbon dioxide emission reduction technology has increasingly attracted widespread attention from scientists around the world. The production of chemicals such as methanol, formic acid, gasoline, aromatics and olefins through catalytic hydrogenation of carbon dioxide is of great significance for reducing carbon dioxide emissions, and at the same time realizes the conversion process of carbon dioxide into high-value-added liquid fuels and chemicals.

[0003] Olefins are a very important class of chemical industrial raw materials, mainly including low-carbon olefins and long-chain olefins. Low-carbon olefins such as ethylene, propylene, and butene are the most basic raw materials for petrochemical production, and are mainly used to produce bulk commodities such as polyethylene, polypropylene, acrylonitrile, ethylene oxide, ethylene glycol, and rubber. Long-chain olefins are mainly used in high value-added products such as synthetic lubricant base oils, detergents, plasticizers, and pesticides. At present, the production of low-carbon olefins mainly comes from the steam cracking process of naphtha. Due to the complex composition of raw materials and the unsatisfactory product structure, the cracking yield and quality are increasingly difficult to meet the growing demand for olefins. Therefore, the preparation of olefins from carbon dioxide or carbon monoxide has become a very important technical route. There are two routes to produce olefins from carbon dioxide: one is to synthesize methanol through the hydrogenation of carbon dioxide, and then produce olefins through MTO / MTP technology. This route is difficult to couple because the reaction temperature of methanol synthesis is too different from that of MTO / MTP. The other is to produce carbon monoxide from carbon dioxide through the reverse water gas shift reaction (RWGS, the active component is usually Fe3O4), and then produce olefins through Fischer-Tropsch synthesis (FTS, the active component is usually Fe5C2). This route involves two series reactions with similar temperatures, which can couple the two reactions and has better application prospects.

[0004] However, the activity, stability and selectivity of iron-based catalysts in the carbon dioxide Fischer-Tropsch synthesis reaction are not ideal and cannot meet the requirements of large-scale industrial production. Transition metal oxides and alkali metals need to be added as additives to adjust the various performance indicators of the catalyst in order to obtain higher activity and selectivity. The activity of iron-based catalysts is affected by the content of Fe3O4 and Fe5C2. Too much Fe3O4 promotes the conversion of CO2 to CO, and the formation reaction of hydrocarbons becomes the limiting step; too much Fe5C2 is not conducive to the conversion of CO2 to CO, and the RWGS reaction becomes the limiting step. In addition, the CO2 hydrogenation reaction generates a large amount of byproduct water, which will oxidize the active component Fe5C2 in the catalyst and reduce its content in the catalyst, thereby limiting the activity of the catalyst and further reducing the stability of the catalyst. Summary of the invention

[0005] In order to solve the problems in the prior art that the active component Fe5C2 in the iron-based catalyst is difficult to control and the catalyst stability needs to be improved, the present invention provides a CO2 / CO hydrogenation to olefins composite catalyst and a preparation method and application thereof.

[0006] In a first aspect, the present invention provides a composite catalyst for producing olefins by hydrogenation of CO2 / CO, which is formed by physically mixing and granulating a surface hydrophobic catalyst and a surface hydrophilic catalyst; The surface hydrophilic catalyst is nanometer iron oxide particles composited with transition metal oxides modified by alkali metal oxides; The surface hydrophobic catalyst comprises: nano iron oxide particles composited with alkali metal oxide-modified transition metal oxide and coated with a surface hydrophobic material-modified mesoporous oxide layer; Preferably, the physical mass ratio of the surface hydrophobic catalyst to the surface hydrophilic catalyst is 1:0.001-20.

[0007] In the present disclosure, Fe2O3 nanocrystals or mesoporous iron oxides are sequentially modified with transition metals and alkali metals, and then a mesoporous structure with hydrophobic properties is constructed on its surface, which promotes the rapid removal of H2O on the catalyst surface and strengthens the mass transfer process of carbon species, thereby improving the stability of Fe5C2 and promoting the reaction of CO hydrogenation to olefins. Moreover, according to the catalyst ratio, the modified Fe2O3 with a surface hydrophilic structure and the modified Fe2O3 with a surface hydrophobic structure are physically mixed, and a composite catalyst is obtained after tableting and granulation. By adjusting the ratio of the hydrophilic structure to the hydrophobic structure, the content of the active components of the iron-based catalyst, Fe3O4 and Fe5C2, can be controlled and adjusted during the activation and reaction process, thereby improving the overall activity of the iron-based catalyst. The composite iron-based catalyst prepared by the present invention exhibits the advantages of high carbon dioxide hydrogenation reaction activity and high stability in practical applications.

[0008] Preferably, the nano iron oxide particles are nano Fe2O3 particles, and the particle size of the nano iron oxide particles is 20nm to 100nm; The transition metal element in the transition metal oxide is selected from at least one of Zn, V, Cr, Mn and Co.

[0009] Preferably, the mass ratio of iron element to transition metal element in the transition metal oxide composite nano iron oxide particles is 1:0.01-1, preferably 1:0.03-0.5.

[0010] Preferably, the alkali metal element in the alkali metal oxide is selected from at least one of Li, Na, K and Rb.

[0011] Preferably, the mass ratio of iron element to alkali metal oxide in the hydrophilic catalyst is 1:0.001-0.1, preferably 1:0.005-0.08.

[0012] Preferably, the mass ratio of iron element to alkali metal oxide in the hydrophobic catalyst is 1:0.001-0.1, preferably 1:0.005-0.08.

[0013] Preferably, the material of the mesoporous oxide layer is selected from at least one of SiO2, ZrO2 and Al2O3; the mass ratio of the iron element in the hydrophobic catalyst to the mesoporous oxide layer is 1:0.005-0.2, preferably 1:0.01-0.2.

[0014] Preferably, the hydrophobic material is chlorosilane, preferably one selected from methylchlorosilane, dimethylchlorosilane and trimethylchlorosilane.

[0015] Preferably, the mass ratio of the hydrophobic catalyst to the hydrophilic catalyst is 1:1-20, preferably 1:5-15.

[0016] In a second aspect, the present invention provides a method for preparing a composite catalyst for CO2 / CO hydrogenation to olefins, comprising: (1) mixing transition metal oxide composite nano iron oxide particles and an alkali metal salt solution, and then subjecting the mixture to heat treatment to obtain a hydrophilic catalyst; (2) preparing a mesoporous oxide layer on the surface of the transition metal oxide composite nano iron oxide particles and dispersing the layer in a solvent, adding a hydrophobic material for silanization modification, and subjecting the mixture to heat treatment to obtain hydrophobic transition metal oxide composite nano iron oxide particles coated with the mesoporous oxide layer; (3) dispersing hydrophobic transition metal oxide composite nano-iron oxide particles coated with a mesoporous oxide layer in an organic solvent, mixing with an alkali metal salt solution, and then subjecting to heat treatment to obtain a hydrophobic catalyst; (4) The hydrophilic catalyst and the hydrophobic catalyst are mixed and granulated according to a mass ratio to obtain the CO2 / CO hydrogenation to olefins composite catalyst.

[0017] Preferably, in step (1), the method for preparing the transition metal oxide composite nano iron oxide particles comprises: 1) adding a precipitant solution to an iron salt solution and mixing, then subjecting the mixture to hydrothermal treatment, washing and drying to obtain nano-Fe2O3; 2) preparing the nano-Fe2O3 into a nano-Fe2O3 dispersion, then adding a transition metal salt solution and mixing, and finally subjecting the mixture to heat treatment to obtain nano-iron oxide particles composited with transition metal oxides.

[0018] Furthermore, preferably, in step 1), the iron salt in the iron salt solution is selected from at least one of ferric chloride, ferric nitrate, and ferric acetate; the solvent of the iron salt solution is selected from at least one of ethanol, ethylene glycol, and water; the concentration of the iron salt solution is 0.1 to 5 mol / L; The precipitant is selected from at least one of an alkali metal hydroxide and an alkali metal carbonate, and the concentration of the precipitant solution is selected from 0.05 to 1M; The temperature of the hydrothermal treatment is 100-200°C and the time is 3-48h; The drying temperature is 60-250° C., and the drying time is 6-48 hours.

[0019] Furthermore, preferably, in step 2), the transition metal salt solution contains at least one of nitrate, chloride and acetate of the transition metal element; the solvent of the transition metal salt solution is selected from at least one of ethanol, ethylene glycol and water; the concentration of the transition metal salt solution is 0.1 to 5 mol / L; The solvent of the nano-Fe2O3 dispersion is ethylene glycol; the mass ratio of the nano-Fe2O3 to ethylene glycol is 1:8-50; The heat treatment temperature is 100-300° C. and the time is 2-48 hours.

[0020] Preferably, in step (2), the preparation method of the mesoporous oxide layer comprises: dispersing transition metal oxide composite nano-iron oxide particles in ethanol, adding a template agent and mixing evenly, then adding a silicon source and stirring in a water bath, then adding ammonia water and deionized water and continuing stirring in a water bath, and finally washing, filtering, drying and calcining to obtain transition metal oxide composite nano-iron oxide particles coated with a mesoporous oxide layer; Preferably, the mass ratio of the transition metal oxide composite nano iron oxide particles, template, silicon source, ammonia water, deionized water, and ethanol is 1:0.1-1:0.1-0.8:1-50:20-100:500-1000; Preferably, the calcination temperature is 300-550°C and the calcination time is 2-12 hours;

[0021] Preferably, in step (2), the preparation method of the hydrophobic transition metal oxide composite nano iron oxide particles coated with a mesoporous oxide layer comprises: dispersing the transition metal oxide composite nano iron oxide particles coated with a mesoporous oxide layer in a solvent, adding chlorosilane, stirring and ultrasonicating, and drying to obtain the hydrophobic transition metal oxide composite nano iron oxide particles coated with a mesoporous oxide layer; The solvent is at least one of n-hexane, water, ethanol and ether; The hydrophobic material is chlorosilane, preferably one selected from methylchlorosilane, dimethylchlorosilane and trimethylchlorosilane; The mass ratio of the transition metal oxide composite nano iron oxide particles coated with a mesoporous oxide layer, chlorosilane and solvent is 1:0.01-10:50-500; The washing is performed by washing with a solvent for 3 to 5 times; The drying temperature is 60 to 120° C. and vacuum drying is performed for 6 to 24 hours.

[0022] Preferably, in step (3), the organic solvent is a mixed solution of diethyl ether and anhydrous ethanol; preferably, the mass ratio of diethyl ether to anhydrous ethanol in the organic solvent is 1:5-20. The concentration of the alkali metal salt solution is 0.1-2 mol / L; The mass ratio of the hydrophobic transition metal oxide composite nano iron oxide particles coated with a mesoporous oxide layer, the alkali metal salt solution and the organic solvent is 1:0.1-10:20-40; The heat treatment temperature is 100-400° C. and the time is 2-48 hours.

[0023] In a third aspect, the present invention provides an application of a CO2 / CO hydrogenation to olefins composite catalyst in CO2 / CO hydrogenation to olefins.

[0024] Preferably, the CO2 / CO hydrogenation to olefins composite catalyst is activated and then introduced into the raw gas for catalytic reaction; the raw gas comprises at least one of CO2 and CO and H2; The volume ratio of CO2 or / and CO to H2 in the raw gas is 0.1 to 5; The temperature of the catalytic reaction is 200-360°C; The pressure of the raw gas is 0.1-6 MPa, and the space velocity is 800-10000 mL / (g·h).

[0025] Preferably, the activation treatment parameters include: introducing reducing gas with a composition of 0-10% CO / H2, a space velocity of 800-10000 mL / (g·h), a pressure of 0.1-6 MPa, a gradient temperature increase to 150-400°C, and an activation time of 8-100 h.

[0026] Beneficial effects of the present invention: (1) The iron salt, transition metal salt, alkali metal salt and structural additive used in the synthesis of the composite catalyst precursor of the present invention are convenient and easy to obtain, have a wide range of applications, and are easy to realize industrially; (2) The types and contents of active components in the composite catalyst of the present invention are controllable and adjustable, and the composite catalyst is not only applicable to CO2 hydrogenation to olefins, but also to Fischer-Tropsch synthesis of olefins, and has good practicality; (3) The catalyst of the present invention has shown no deactivation trend after continuous reaction testing and has good stability. Therefore, the technical solution of the present invention has good industrial prospects; (4) The application of the present invention converts CO2 waste gas that has an impact on the climate environment into olefins. The industrial basis of the unit operations involved is mature, easy to apply on a large scale, and has good economic efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 is a SEM image of the catalyst sample (Example 1) of the present invention; Figure 2 is the XRD spectrum of the catalyst sample in the present invention; Figure 3 The catalyst sample CO in the present invention 2- TPD diagram; Figure 4 It is a comparison chart of the hydrophobic iron-based catalyst and the hydrophilic iron-based catalyst in the catalyst sample (Example 1) of the present invention. DETAILED DESCRIPTION

[0028] The present invention is further described below by the following embodiments. It should be understood that the following embodiments are only used to illustrate the present invention, but not to limit the present invention.

[0029] In the present disclosure, based on the activity characteristics of iron-based catalysts in catalyzing CO2 hydrogenation, an iron-based catalyst with a hydrophobic surface is constructed to reduce the residence time of byproduct water on the catalyst surface, thereby achieving controllable and adjustable contents of the catalyst active components Fe3O4 and Fe5C2, ultimately achieving the purpose of improving the activity and stability of the catalyst.

[0030] In the present invention, the CO2 / CO hydrogenation to olefins composite catalyst comprises iron oxide, transition metal oxide, alkali metal and structural additive. Preferably, the transition metal element in the transition metal oxide is selected from at least one of Zn, V, Cr, Mn and Co. The alkali metal element in the alkali metal oxide is selected from one or more of Li, Na, K and Rb. The mass ratio of the iron element to the transition metal element is 1:0.01 to 1, preferably 1:0.03 to 0.5. The mass ratio of the iron element to the alkali metal oxide additive is 1:0.001 to 0.1, preferably 1:0.005 to 0.08. The structural additive is selected from one or more of silicon oxide, aluminum oxide and zirconium oxide, and the mass ratio of the iron element to the structural additive is 1:0.01 to 0.2.

[0031] Wherein, the iron oxide is selected from nano iron oxide prepared by hydrothermal synthesis method or oxalate thermal decomposition method;.

[0032] The composite catalyst is formed by physically mixing an iron-based catalyst with a surface hydrophobic structure and an iron-based catalyst with a surface hydrophilic structure, and the mass ratio of the surface hydrophobic iron-based catalyst to the surface hydrophilic iron-based catalyst is 1:0-20, preferably 1:0-10.

[0033] The following is an exemplary description of the preparation method of the CO2 / CO hydrogenation to olefins composite catalyst.

[0034] A soluble iron salt and a transition metal salt are prepared into solutions to obtain an iron salt solution and a transition metal salt solution, respectively. The soluble iron salt is selected from one of ferric chloride, ferric nitrate, and ferric acetate. The soluble transition metal salt is selected from one of nitrate, chloride, and acetate. The solvent used is selected from at least one of ethanol, ethylene glycol, and water. The concentrations of the iron salt solution and the transition metal salt solution can be 0.1 to 5 mol / L, respectively.

[0035] The soluble alkali metal precipitant is prepared into a solution, namely, a precipitant solution. In the precipitant solution, the soluble alkali metal is selected from one of hydroxide and carbonate. The concentration of the precipitant solution can be 0.05-1M.

[0036] Add the precipitant solution to the iron salt solution, transfer it to a hydrothermal kettle after stirring, wash, filter and dry it after hydrothermal treatment to obtain non-magnetic nano Fe2O3 oxide. The hydrothermal temperature is 100-200°C, and the hydrothermal time is 3-48h. The drying temperature is 60-120°C, and the drying time is 6-48h.

[0037] Ultrasonic dispersion of nano-Fe2O3 oxide in ethylene glycol, adding transition metal salt solution, stirring and ultrasonication for multiple times, and heat treatment to obtain transition metal modified nano-Fe2O3 oxide. The mass ratio of nano-Fe2O3 to ethylene glycol is 1:8-50, the heat treatment temperature is 100-300°C, and the time is 8-48h.

[0038] Ultrasonic dispersion of transition metal modified nano Fe2O3 oxide in ethanol, adding template (CTAB or F117) and stirring, then adding silicon source (TEOS) and stirring in water bath, adding ammonia and deionized water and continuing stirring, washing, filtering, drying and roasting, to obtain mesoporous SiO2 coated transition metal modified nano Fe2O3 oxide. Preferably, the mass ratio of transition metal modified nano iron oxide: CTAB or F117: TEOS: ammonia: deionized water: ethylene glycol = 1: 0.1-1: 0.1-0.8: 1-50: 20-100: 500-1000. The roasting (calcining) temperature can be 300-550°C, and the time can be 2-12h.

[0039] The transition metal modified nano Fe2O3 oxide coated with mesoporous SiO2 is dispersed in n-hexane, chlorosilane is added, and the surface is washed and dried after ultrasonic treatment for 2 to 3 hours to obtain a surface hydrophobic substance. Preferably, the mass ratio of the transition metal modified nano Fe2O3 oxide coated with mesoporous SiO2: chlorosilane: n-hexane is 1:0.2 to 10:50 to 500. The chlorosilane is selected from one of methyl chlorosilane, dimethyl chlorosilane and trimethyl chlorosilane. The washing method uses n-hexane for washing 3 to 5 times and vacuum drying at 60 to 120°C for 6 to 24 hours.

[0040] The surface hydrophobic substance is dispersed in a mixed solution of ether and anhydrous ethanol to obtain a hydrophobic mesoporous silica-coated nano-iron oxide, and then an alkali metal salt solution is added, stirred and ultrasonicated for 5 to 15 minutes, and then heat-treated to obtain an alkali metal-modified surface iron-based catalyst with a hydrophobic structure. Preferably, the mass ratio of hydrophobic mesoporous silica-coated nano-iron oxide: alkali metal solution: ether: anhydrous ethanol is 1: 0.1 to 10: 10 to 20: 10 to 20.

[0041] The transition metal-modified nano-Fe2O3 oxide is added into an equal volume of an alkali metal salt solution, stirred and ultrasonicated for 5 to 15 minutes, and then heat-treated to obtain an alkali metal-modified iron-based catalyst with a hydrophilic surface.

[0042] The surface hydrophobic iron-based catalyst and the surface hydrophilic iron-based catalyst are physically mixed according to a composition ratio to obtain the CO2 / CO hydrogenation to olefins iron-based catalyst.

[0043] In the present invention, a raw material gas containing CO2 or CO and hydrogen is contacted with the above-mentioned CO2 / CO hydrogenation composite catalyst for reaction to obtain a product containing olefins. Compared with the prior art, the catalyst in the present invention can significantly improve the activity of the catalyst when applied to CO2 hydrogenation, with a CO2 conversion rate higher than 50%, an olefin selectivity higher than 65%, and significantly enhanced stability; and can significantly reduce the CO2 selectivity to 13.4% when applied to CO hydrogenation reaction. Therefore, the present invention provides a new idea for efficient conversion of CO2 / CO hydrogenation and has a good industrialization prospect.

[0044] In an optional embodiment, the iron-based catalyst needs to be activated before being used in the reaction. The activation method is: introducing a reducing gas with a composition of 1-10% CO / H2, a space velocity of 800-10000 mL / (g·h), a pressure of 0.1-6 MPa, a gradient temperature increase to 150-400°C, and activation for 8-100 hours.

[0045] In an optional embodiment, the catalytic reaction conditions are: the molar ratio of the raw gas H2 / CO2 (CO) is 0.1-5; the reaction temperature is 200-360°C; the pressure is 0.1-6MPa; and the space velocity is 800-10000mL / (g·h).

[0046] After the reaction product is condensed by a cold trap (temperature 0-10°C), the H2, CO, and CO2 components in the gas phase product are analyzed online by a gas chromatograph equipped with a TCD detector equipped with a TDX-01 filling column, and the content of light hydrocarbon components (C1-C6) can be analyzed online by a gas chromatograph equipped with a FID detector equipped with an HP-PLOT Q capillary column. After the reaction is completed, the liquid hydrocarbon components in the cold trap are collected, weighed, and the mass of the oil phase and the water phase are measured separately. The components of the oil phase liquid product are analyzed by an offline gas chromatography-mass spectrometry (GC-MS) equipped with an FID detector equipped with an SH-Rxi-5MS capillary column. The results of the gas phase product and liquid phase product analysis are normalized to obtain the selectivity of various components and the CO2 conversion rate.

[0047] The following further examples are given to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values ​​​​exemplified below.

[0048] Embodiment 1: (1) Preparation of nano-Fe2O3 oxide. Dissolve 40.5 g Fe(NO3)3·9H2O and 17.0 mol KOH in 60 mL deionized water, add Fe(NO3)3 solution to the KOH solution, and stir for 15 min; then transfer to a hydrothermal reactor, hydrothermal at 170°C for 12 h, centrifuge, wash three times, and dry in a forced air oven at 80°C for 12 h to obtain nano-Fe2O3 oxide; (2) Preparation of Mn-modified nano-Fe2O3 oxide. Add 1.0 g of nano-Fe2O3 oxide to 10 mL of ethylene glycol, ultrasonicate for 15 min, stir for 15 min to make it evenly dispersed, and place it in a blast oven at 100°C to dry for 24 h. Then add 0.90 g of 50% Mn(NO3)2 solution and 4 ml of ethylene glycol, stir, ultrasonicate for 15 min, and place it in an oven at 200°C to dry for 12 h to obtain Mn-modified nano-Fe2O3 oxide; (3) Preparation of K-modified nano-FeMn oxide. 1.0 g of Mn-modified nano-Fe2O3 oxide was ultrasonically dispersed in 10 mL of ethanol, and 2.0 mL of 0.1 M K2CO3 solution was added. After ultrasonication for 15 min, the mixture was stirred and placed in a forced air oven at 60 °C for 12 h to obtain K-modified nano-Fe-Mn oxide as a hydrophilic catalyst. (4) Preparation of surface hydrophobic FeMn oxide. Ultrasonic dispersion of 1.0 g FeMn oxide in 500 ml ethanol, add 0.6 g CTAB and stir for 30 min, add 0.5 mL TEOS and stir in a water bath (450 rpm, 30 ° C) for 5 h, then add 10 ml ammonia water and 50 ml deionized water and continue stirring for 5 h, wash and filter, place in a blast oven at 100 ° C for 12 h, and calcine in a muffle furnace at 500 ° C for 3 h. Then disperse the calcined material in 100 ml n-hexane, add 2 ml trimethylsilyl chloride, ultrasonicate for 3 h, wash the product with n-hexane, and then place in an oven at 100 ° C for 12 h to obtain surface hydrophobic FeMn oxide; (5) Preparation of K-modified surface hydrophobic FeMn oxide. 1.0 g of surface hydrophobic FeMn oxide was ultrasonically dispersed in 10 mL of ethanol and 10 mL of ether, and 0.3 mL of 0.1 M K2CO3 solution was added. After ultrasonication for 15 min, the mixture was stirred and placed in a forced air oven at 60 °C for 12 h to obtain K-modified surface hydrophobic FeMn oxide as a hydrophobic catalyst. (6) Preparation of catalysts with different hydrophobic ratios. K-modified surface hydrophobic FeMn oxide (surface hydrophobic) and K-modified nano FeMn oxide (surface hydrophilic) were physically mixed and granulated at a mass ratio of 1:0.2 to obtain the CO2 / CO hydrogenation to olefins composite catalyst.

[0049] Example 1 Evaluation of the CO2 hydrogenation performance of the catalyst obtained: (1) The catalyst hydrogenation performance was evaluated using a high-pressure fixed bed device, with a catalyst loading of 0.5 g, a 5% CO / H2 reducing gas introduced, a space velocity of 4000 mL / (g·h), a pressure of 0.1 MPa, a programmed temperature rise to 350°C, and activation for 48 hours. (2) The H2 / CO2 molar ratio was switched to 3, the Ar volume concentration was 5%; the reaction temperature was 340°C, the pressure was 2 MPa, and the space velocity was 4000 mL / (g·h). (3) After the reaction tail gas was condensed by a cold trap (temperature 0-10°C), the H2, CO, CO2, and Ar in the gas phase components were analyzed online by a gas chromatograph equipped with a TCD detector of a TDX-01 filling column, and the content of light hydrocarbon components (C1-C6) was analyzed online by a gas chromatograph equipped with a FID detector of an HP-PLOT Q capillary column. After 48 hours of reaction, the liquid product components in the cold trap were collected, and the oil phase and the water phase were separated and weighed separately. The oil phase and liquid product components were analyzed offline by gas chromatography-mass spectrometry (GC-MS) with a FID detector equipped with a SH-Rxi-5 MS capillary column. The results of the gas phase product and liquid phase product analysis were normalized to obtain the selectivity of various components and CO2 conversion rate.

[0050] The results of the evaluation of the CO2 hydrogenation performance of the catalyst obtained in Example 1 are as follows: the CO2 conversion rate is 37.7%, the CO selectivity is 4.0%, the CH4 selectivity is 30.1%, and the C 2+ The selectivity is 23.6%, C 2+ = The selectivity was 42.3%, and the olefin / alkane ratio O / P was 1.8; the catalyst showed no activity decline trend after 200 hours of reaction.

[0051] Embodiment 2-10 Preparation of catalysts in Examples 2-10: The detailed steps for preparing the catalysts are the same as those in Example 1, and the specific reagents, solvents, and process parameters are shown in Tables 1 and 2.

[0052] Evaluation of CO2 hydrogenation performance of the catalyst obtained in Example 2-10: The catalyst performance evaluation conditions are shown in Table 3.

[0053] The results of the evaluation of the CO2 hydrogenation performance of the catalysts obtained in Examples 2-10 are shown in Table 4 for details.

[0054] Table 1 shows the preparation parameters of the catalysts in Examples 1-10:

[0055] Table 2 shows the preparation parameters of the catalysts in Examples 1-10:

[0056] Embodiment 11 Example 11 Catalyst preparation: 28g FeSO4·7H2O was dissolved in 100mL deionized water, and then 7.2g 50% Mn(NO3)2 solution was added and stirred for 15min. 16.2g anhydrous oxalic acid was dissolved in 100mL deionized water. The FeMn mixed solution was slowly added to the oxalic acid solution and stirred for 30min to obtain a light yellow precipitate, which was centrifuged and washed three times, placed in a blast oven at 100℃ for 12h, and heated in a muffle furnace at 2℃min. -1 The temperature was raised to 350°C at a rate of 100 °C and kept for 4 hours to obtain mesoporous FeMn oxide. 1 g of mesoporous FeMn oxide was ultrasonically dispersed in 20 mL of ethanol, 2 ml of 0.1 M K2CO3 solution was added, ultrasonicated for 15 minutes, and placed in an oven at 80°C for 12 hours to obtain a K-modified mesoporous FeMn catalyst as a hydrophilic catalyst. The hydrophobic catalyst was then obtained by hydrophobic modification, and the specific steps were the same as in Example 1. The mass ratio of hydrophobic catalyst:hydrophilic catalyst was 1:6.

[0057] Example 11 Catalyst CO2 Hydrogenation Performance Evaluation: The catalyst performance evaluation conditions are shown in Table 3. Example 11 Catalyst CO2 Hydrogenation Performance Evaluation Results: See Table 4 for details.

[0058] Example 11 Evaluation of the performance of CO hydrogenation of catalyst: (1) The performance of the catalyst hydrogenation was evaluated by using a high-pressure fixed bed device. The catalyst was a uniformly hydrophobic catalyst, loaded with 0.5 g, and a reducing gas of 5% CO / H2 was introduced, the air velocity was 4000 mL / (g·h), the pressure was 0.1 MPa, the temperature was programmed to 350°C, and the activation was performed for 24 hours. (2) The raw gas was switched to a H2 / CO molar ratio of 2 and Ar accounted for 5%; the reaction temperature was 320°C, the pressure was 2 MPa, and the air velocity was 4000 mL / (g·h). (3) After the reaction tail gas was condensed by a cold trap (temperature 0-10°C), the H2, CO, CO2, and Ar in the gas phase components were analyzed online by a gas chromatograph equipped with a TCD detector of a TDX-01 filling column, and the content of light hydrocarbon components (C1-C6) was analyzed online by a gas chromatograph equipped with a FID detector of an HP-PLOT Q capillary column. After 48 hours of reaction, the liquid product components in the cold trap were collected, and the oil phase and the water phase were separated and weighed separately. The oil phase and liquid product components were analyzed offline by gas chromatography-mass spectrometry (GC-MS) with a FID detector equipped with a SH-Rxi-5 MS capillary column. The results of the gas phase product and liquid phase product analysis were normalized to obtain the selectivity of various components and CO2 conversion rate.

[0059] Example 11 Catalyst CO hydrogenation performance evaluation results: CO conversion rate is 66.8%, CO2 selectivity is 13.4%, CH4 selectivity is 11.2%, C 2+ 0 The selectivity is 9.8%, C 2+ = The selectivity was 65.6% and the olefin / alkane ratio O / P was 6.7.

[0060] Example 12 The preparation process of the CO2 / CO hydrogenation to olefins composite catalyst in this Example 12 refers to Example 1, with the only difference being that in step (6), K-modified surface hydrophobic FeMn oxide (surface hydrophobic) and K-modified nano FeMn oxide (surface hydrophilic) are physically mixed and granulated in a mass ratio of 1:1 to obtain the CO2 / CO hydrogenation to olefins composite catalyst.

[0061] Example 13 The preparation process of the CO2 / CO hydrogenation to olefins composite catalyst in this Example 13 refers to Example 1, with the only difference being that in step (6), K-modified surface hydrophobic FeMn oxide (surface hydrophobic) and K-modified nano FeMn oxide (surface hydrophilic) are physically mixed and granulated in a mass ratio of 1:5 to obtain the CO2 / CO hydrogenation to olefins composite catalyst.

[0062] Embodiment 14 The preparation process of the CO2 / CO hydrogenation to olefins composite catalyst in this Example 15 refers to Example 1, with the only difference being that in step (6), K-modified surface hydrophobic FeMn oxide (surface hydrophobic) and K-modified nano FeMn oxide (surface hydrophilic) are physically mixed and granulated in a mass ratio of 1:10 to obtain the CO2 / CO hydrogenation to olefins composite catalyst.

[0063] Embodiment 15 The preparation process of the CO2 / CO hydrogenation to olefins composite catalyst in this Example 17 refers to Example 1, with the only difference being that in step (6), K-modified surface hydrophobic FeMn oxide (surface hydrophobic) and K-modified nano FeMn oxide (surface hydrophilic) are physically mixed and granulated in a mass ratio of 1:20 to obtain the CO2 / CO hydrogenation to olefins composite catalyst.

[0064] Comparative Example 1 Preparation of Fe2O3 catalyst: 32.4g Fe(Cl)3 was dissolved in 60mL deionized water, 14.3g 50% Mn(NO3)2 solution was added, and stirred for 15min; Fe(NO3)3 and Mn(NO3)2 mixed solution were added to 200mL 4M KOH solution, and stirred for 15min, aged at room temperature for 4h, filtered, washed to neutrality, placed in a blast oven at 120℃ for 6h, and calcined at 550℃ in a muffle furnace for 3h to obtain FeMn oxide catalyst. Comparative Example Catalyst CO2 Hydrogenation Performance Evaluation: The catalyst performance evaluation conditions were the same as those in Example 1. Comparative Example Catalyst CO2 Hydrogenation Performance Evaluation Results: See Table 4 for details.

[0065] Comparative Example 2 The hydrophobic catalyst prepared in Example 1 was selected as Comparative Example 2.

[0066] Comparative Example 3 The hydrophilic catalyst prepared in Example 1 was selected as Comparative Example 3.

[0067] Comparative Example 4 The preparation process of the CO2 / CO hydrogenation to olefins composite catalyst in this comparative example 4 refers to that in Example 1, with the only difference being that in step (6), K-modified surface hydrophobic FeMn oxide (surface hydrophobic) and K-modified nano FeMn oxide (surface hydrophilic) are physically mixed in a mass ratio of 1:25 to obtain the CO2 / CO hydrogenation to olefins composite catalyst.

[0068] Table 3 shows the evaluation conditions of the CO2 hydrogenation catalytic performance of the catalysts of Examples 1-11 and the comparative catalysts:

[0069] Table 4 shows the evaluation results of the catalytic performance of CO2 hydrogenation to olefins of the catalysts of Examples 1-11 and the comparative catalysts:

[0070] Figure 1 The SEM image of the catalyst sample of Example 1 (the upper image is nano-Fe2O3 oxide, and the lower image is FeMn oxide coated with SiO2). It can be seen from the image that SiO2 is coated on the surface of nano-Fe2O3 oxide in a layered porous structure; Figure 2 The XRD spectra of the catalyst samples of Example 1 and Example 10 show that the iron oxide exists in the α-Fe2O3 phase; the manganese oxide is uniformly dispersed in the iron oxide or on its surface, and does not form a separate phase; Figure 3CO of the catalyst sample 2- TPD diagram, from which we can see that alkali metals can adjust the basicity of the catalyst surface; Figure 4 This is a picture of the hydrophobic (left) iron-based catalyst and the hydrophilic (right) iron-based catalyst in Example 1 after being stirred in water for 5 minutes. It can be seen from the picture that the hydrophobic catalyst floats on the water surface and the hydrophilic catalyst sinks to the bottom of the water, indicating that the hydrophobic (left) iron-based catalyst has good hydrophobicity.

[0071] It can be seen from the evaluation results of the corresponding catalysts in the above embodiments that, compared with the prior art, the catalyst in the present invention can significantly improve the activity of the catalyst when applied to CO2 hydrogenation, with a CO2 conversion rate higher than 50%, an olefin selectivity higher than 65%, and significantly enhanced stability; when applied to CO hydrogenation reaction, it can significantly reduce the CO2 selectivity to 13.4%, providing a new idea for the efficient conversion of CO2 / CO hydrogenation, and has a good industrial prospect.

Claims

1. A CO2 / CO hydrogenation to olefins composite catalyst, characterized in that: It is formed by physically mixing and granulating a surface hydrophobic catalyst and a surface hydrophilic catalyst; The surface hydrophilic catalyst is nanometer iron oxide particles composited with transition metal oxides modified by alkali metal oxides; The surface hydrophobic catalyst comprises: nano iron oxide particles composited with alkali metal oxide-modified transition metal oxide and coated with a surface hydrophobic material-modified mesoporous oxide layer; Preferably, the physical mass ratio of the surface hydrophobic catalyst to the surface hydrophilic catalyst is 1:0.001-20.

2. The CO2 / CO hydrogenation to olefins composite catalyst according to claim 1, characterized in that: The nano iron oxide particles are nano Fe2O3 particles, and the particle size of the nano iron oxide particles is 20nm to 100nm; The transition metal element in the transition metal oxide is selected from at least one of Zn, V, Cr, Mn and Co; The alkali metal element in the alkali metal oxide is selected from at least one of Li, Na, K and Rb; The material of the mesoporous oxide layer is selected from at least one of SiO2, ZrO2 and Al2O3; The hydrophobic material is chlorosilane, preferably one selected from methylchlorosilane, dimethylchlorosilane and trimethylchlorosilane; The mass ratio of iron element: transition metal element: alkali metal oxide in the surface hydrophilic catalyst is 1: 0.01 to 1: 0.001 to 0.1, preferably 1: 0.03 to 0.5: 0.005 to 0.08; The mass ratio of iron element: transition metal element: alkali metal oxide: mesoporous oxide layer in the surface hydrophobic catalyst is 1: 0.01-1: 0.001-0.1: 0.005-0.2, preferably 1: 0.03-0.5: 0.005-0.08: 0.01-0.

2.

3. A method for preparing a CO2 / CO hydrogenation to olefins composite catalyst as claimed in claim 1 or 2, characterized in that: include: (1) mixing transition metal oxide composite nano iron oxide particles and an alkali metal salt solution, and then subjecting the mixture to heat treatment to obtain a hydrophilic catalyst; (2) preparing a mesoporous oxide layer on the surface of the transition metal oxide composite nano iron oxide particles and dispersing the layer in a solvent, adding a hydrophobic material for silanization modification, and subjecting the mixture to heat treatment to obtain hydrophobic transition metal oxide composite nano iron oxide particles coated with the mesoporous oxide layer; (3) dispersing hydrophobic transition metal oxide composite nano-iron oxide particles coated with a mesoporous oxide layer in an organic solvent, mixing with an alkali metal salt solution, and then subjecting to heat treatment to obtain a hydrophobic catalyst; (4) The hydrophilic catalyst and the hydrophobic catalyst are mixed and granulated according to a mass ratio to obtain the CO2 / CO hydrogenation to olefins composite catalyst.

4. The preparation method according to claim 3, characterized in that: In step (1), the method for preparing the transition metal oxide composite nano iron oxide particles comprises: 1) adding the precipitant solution to the iron salt solution and mixing, and then subjecting the mixture to hydrothermal treatment, washing and drying to obtain nano-Fe2O3; 2) Nano-Fe2O3 is prepared into a nano-Fe2O3 dispersion, and then a transition metal salt solution is added and mixed, and finally heat-treated to obtain transition metal oxide composite nano-iron oxide particles.

5. The preparation method according to claim 4, characterized in that: In step 1), the iron salt in the iron salt solution is selected from at least one of ferric chloride, ferric nitrate, and ferric acetate; the solvent of the iron salt solution is selected from at least one of ethanol, ethylene glycol, and water; the concentration of the iron salt solution is 0.1 to 5 mol / L; The precipitant is selected from at least one of an alkali metal hydroxide and an alkali metal carbonate, and the concentration of the precipitant solution is selected from 0.05 to 1M; The temperature of the hydrothermal treatment is 100-200°C and the time is 3-48h; The heat treatment temperature is 60-250° C. and the time is 6-48 hours.

6. The preparation method according to claim 4, characterized in that: In step 2), the transition metal salt solution contains at least one of nitrates, chlorides and acetates of transition metal elements; the solvent of the transition metal salt solution is selected from at least one of ethanol, ethylene glycol and water, and the mass ratio of nano-Fe2O3 to the solvent is 1:8-50; the concentration of the transition metal salt solution is 0.1-5 mol / L; the temperature of the heat treatment is 100-300°C, and the time is 2-48h.

7. The preparation method according to claim 4, characterized in that: In step (2), the preparation method of the mesoporous oxide layer comprises: dispersing transition metal oxide composite nano iron oxide particles in ethanol, adding a template agent and mixing evenly, then adding a silicon source and stirring in a water bath, then adding ammonia water and deionized water and continuing stirring in a water bath, and finally washing, filtering, drying and calcining to obtain transition metal oxide composite nano iron oxide particles coated with a mesoporous oxide layer; Preferably, the mass ratio of the transition metal oxide composite nano iron oxide particles, template, silicon source, ammonia water, deionized water, and ethanol is 1:0.1-1:0.1-0.8:1-50:20-100:500-1000; Preferably, the calcination temperature is 300-550° C. and the calcination time is 2-12 hours.

8. The preparation method according to any one of claims 3 to 7, characterized in that: In step (2), the preparation method of the transition metal oxide composite nano iron oxide particles modified by alkali metal oxide with a mesoporous oxide layer modified by a surface hydrophobic material comprises: dispersing the transition metal oxide composite nano iron oxide particles coated with a mesoporous oxide layer in a solvent, adding chlorosilane, stirring and ultrasonicating, and drying to obtain hydrophobic transition metal oxide composite nano iron oxide particles coated with a mesoporous oxide layer; The solvent is at least one of n-hexane, water, ethanol and ether; The hydrophobic material is chlorosilane, preferably one selected from methylchlorosilane, dimethylchlorosilane and trimethylchlorosilane; The mass ratio of the transition metal oxide composite nano iron oxide particles coated with a mesoporous oxide layer, chlorosilane and solvent is 1:0.01-10:50-500; The washing is performed by washing with a solvent for 3 to 5 times; The drying is performed under vacuum at 60 to 120° C. for 6 to 24 hours.

9. The preparation method according to any one of claims 3 to 8, characterized in that: In step (3), the organic solvent is a mixed solution of diethyl ether and anhydrous ethanol; preferably, the mass ratio of diethyl ether to anhydrous ethanol in the organic solvent is 1:5-20; The concentration of the alkali metal salt solution is 0.1-2 mol / L; The mass ratio of the hydrophobic transition metal oxide composite nano iron oxide particles coated with a mesoporous oxide layer, the alkali metal salt solution and the organic solvent is 1:0.1-10:20-40; The heat treatment temperature is 100-400° C. and the time is 2-48 hours.

10. Use of the CO2 / CO hydrogenation to olefins composite catalyst according to any one of claims 1 to 9 in CO2 / CO hydrogenation to olefins, characterized in that: The CO2 / CO hydrogenation to olefins composite catalyst is activated and then introduced into a raw gas for catalytic reaction; the raw gas comprises at least one of CO2 and CO and H2; The total molar content of CO2 and / or CO in the raw gas: the molar content of H2 = 0.1-5; The temperature of the catalytic reaction is 200-360°C; The pressure of the raw gas is 0.1-6 MPa, and the space velocity is 800-10000 mL / (g·h); The activation treatment conditions include: introducing a mixed reducing gas with a composition of 0-10% CO / H2, an air velocity of 800-10000 mL / (g·h), a pressure of 0.1-6 MPa, a gradient temperature increase to 150-400°C, and an activation time of 8-100 hours.