Preparation method of monolithic bipolar membrane based on polyarylether sulfone
The bipolar membrane was prepared by using polyarylethersulfone base film to react with FeCl3 chelation and grafting, and the problem of insufficient adhesion of the bipolar membrane was solved, and a single-piece bipolar membrane with high stability and high efficiency hydrolysis efficiency was achieved.
Patent Information
- Application Number
- CN202411193251.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-28
AI Technical Summary
The existing bipolar films lack adhesion during the preparation process of the bonding method, resulting in the film falling off and affecting performance and stability.
Polyaryl ether sulfone is used as the base film, and the metal ions are fixed through the -NH2 group and the FeCl3 are chelated to prevent the leakage of the catalyst. The negative and positive layers are prepared through grafting reaction to form a monolithic bipolar film to ensure that The layers are tightly bonded.
It improves the mechanical and electrochemical stability of the bipolar membrane, prevents catalyst leakage, enhances hydrolysis efficiency and operating stability, avoids "bubble" phenomenon, and improves stability in an acid-base environment.
Smart Images

Figure CN119016118A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of ion exchange membranes, in particular to a method for preparing a monolithic bipolar membrane based on polyarylethersulfone. Background Art
[0002] Bipolar membrane is a type of ion exchange membrane with a special "sandwich" structure, which is composed of an anion exchange membrane, a cation exchange membrane and an intermediate catalyst layer (Journal of Physical Chemistry, 1956, 60 (4): 435-439). In recent decades, bipolar membranes have broad application prospects in water electrolysis, fuel cells, and flow batteries. Studies have shown that the water dissociation reaction of bipolar membranes mainly occurs in the middle layer of the bipolar membrane, that is, the catalyst layer of the bipolar membrane. The catalyst layer of the bipolar membrane plays a key role in the effect of water dissociation. The bipolar membrane interface catalyst mainly includes metal complex catalysts, metal oxides or metal hydroxide catalysts, metal organic frameworks (MOFs) catalysts, graphene oxide and macromolecular substances containing weak acid and weak base functional groups such as amino groups, sulfonic acid groups, and quaternary amine groups. The ideal interface composition of the bipolar membrane should meet the following requirements: (1) The anion exchange layer and the cation exchange layer do not penetrate each other and the two membrane layers are tightly combined and not easy to delaminate. (2) The thickness of the catalytic layer is small, which is conducive to reducing the working voltage and energy consumption. (3) Introducing a catalyst that has the effect of enhancing the water dissociation of the membrane, enhancing the water dissociation reaction and improving the water dissociation efficiency. The construction of the bipolar membrane interface layer is crucial to the performance of the bipolar membrane. The main construction methods include hot pressing, bonding, casting, electrodeposition, electrospinning, and introducing ion exchange groups on both sides of the base membrane.
[0003] At present, bipolar membranes are mainly divided into monolithic bipolar membranes and composite bipolar membranes. Composite bipolar membranes, as a new type of ion exchange composite membrane, are composed of a cation exchange layer, an interfacial hydrophilic / catalytic layer and an anion exchange membrane. Although bipolar membrane technology has many advantages, in practical applications, especially bipolar membranes prepared by bonding, there is a significant problem, that is, the bonding force between the two membranes is easily insufficient. This deficiency may cause one of the membranes to fall off, thereby affecting the performance and stability of the membrane to a certain extent.
[0004] The manufacturing of monolithic bipolar membrane mainly uses a specific film as a base membrane, and functionalizes the anion exchange group and cation exchange group on both sides of the base membrane through chemical reactions, such as sulfonation, chloromethylation reaction and amination or quaternization reaction, so as to obtain a monolithic bipolar membrane. The monolithic bipolar membrane can realize the three functional structures of the bipolar membrane on a single membrane, that is, the anion and cation layers will not produce "bubbling" phenomenon, thus ensuring that the monolithic bipolar membrane has a longer service life and stability. Due to its unique manufacturing method and excellent performance, the monolithic bipolar membrane provides efficient and economical solutions for fields such as water treatment and chemical production. Summary of the invention
[0005] The present invention provides a method for preparing a monolithic bipolar membrane of polyarylethersulfone. The monolithic bipolar membrane containing amino groups prepared by the method is not easy to fall off. The -NH2 group of the polymer substrate membrane reacts with Fe in FeCl3 to form a monolithic bipolar membrane. 3+ Chelation is beneficial to fix metal ions, prevent catalyst leakage, improve the stability of bipolar membranes, and increase ion conductivity. The specific technical solution is as follows:
[0006] A method for preparing a monolithic bipolar membrane based on polyarylethersulfone comprises the following steps:
[0007] Step (1): Preparation of amino group-containing polyarylethersulfone
[0008] A certain amount of 4,4'-difluorodiphenyl sulfone monomer, 2,2'-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, hexafluorobisphenol A monomer and potassium carbonate are weighed, dissolved in a high boiling point polar aprotic solvent, precipitated in the solvent after the reaction is completed under nitrogen protection at a certain reaction temperature and reaction time, and vacuum dried at a certain temperature to obtain a main chain amino-containing polyarylethersulfone (PAES-NH2); in formula (I), x and y represent the molar percentages of two links, which are x% and y%, respectively, and x+y=100; wherein x=1-100, y=1-100; wherein the molar ratio of 2,2'-bis(3-amino-4-hydroxyphenyl)hexafluoropropane to hexafluorobisphenol A monomer is 1-80%:99-20%, and its chemical structure is shown in formula (I);
[0009]
[0010] Step (2): Preparation of amino-containing polyarylethersulfone film
[0011] A certain amount of amino-containing polyarylethersulfone is weighed and dissolved in a certain amount of solvent under nitrogen protection. After the polymer is completely dissolved, the casting solution is placed on a clean glass plate and vacuum dried at a certain temperature for several hours to obtain an aminopolyarylethersulfone film.
[0012] Step (3): Preparation of the amino-containing polyarylethersulfone film positive layer
[0013] The amino-containing polyarylethersulfone film is sandwiched in a jacket reactor, so that one side of the base membrane is exposed to the cation grafting small molecule solution, and the other side is immersed in a NaCl solution, and the cation layer side of the grafted membrane is immersed in a sulfonation reagent, and a sulfonation reaction is carried out at a certain temperature, and nitrogen is introduced. The jacket reactor is placed in a constant temperature water bath in a sealed state, and a suitable temperature is set to carry out a cation grafting reaction for a certain period of time, and then a hydrolysis reaction is carried out in a NaOH solution, and then washed with deionized water and dried to obtain a cation exchange layer, whose structural formula is shown in formula (II);
[0014]
[0015] Step (4): Preparation of the negative layer of the amino-containing polyarylethersulfone film
[0016] The single-sided functionalized poly(arylethersulfone) film positive layer obtained in step (3) is sandwiched in a jacketed reactor, and the non-functionalized side is exposed to the grafting hole of the negative layer, and a grafting reaction is carried out at a certain temperature, and nitrogen is introduced. The reactor is placed in a sealed state in a constant temperature water bath and set to a suitable temperature for a certain period of time to carry out a grafting reaction, thereby obtaining a poly(arylethersulfone) bipolar membrane; wherein the negative layer structure of the amino-containing poly(arylethersulfone) film is as shown in formula (III);
[0017]
[0018] Step (5): FeCl3 complexation based on poly(arylethersulfone) bipolar membrane
[0019] The polyarylethersulfone bipolar membrane was immersed in a FeCl3 solution at a certain temperature to react for several hours, and then washed with deionized water for several times.
[0020] Preferably, the reaction temperature in step (1) is 100-180° C., the reaction time is 3-24 hours, the high boiling point polar aprotic solvent can be N-methylpyrrolidone, and the solvent for precipitation can be isopropanol.
[0021] Preferably, the amount of the polyarylethersulfone in step (2) is 1 to 2 g, the amount of the solvent is 15 to 30 mL, the vacuum drying temperature is 60 to 80° C., and the vacuum drying time is 18 to 24 h.
[0022] Preferably, in step (3), the temperature of the water bath placed in the constant temperature water bath for reaction can be 60-90°C, the reaction time can be 4-20h, the functional small molecule in the cationic layer grafted small molecule solution can be 1,3-propane sultone; the solvent of the cationic layer grafted functional small molecule solution can be ethanol; the temperature of the sulfonation reaction can be 25-70°C, and the sulfonation reaction time can be 1-6h.
[0023] Preferably, in step (4), the functional small molecule in the anion-grafted small molecule solution can be Br-3C-IM; the solvent of the anion-grafted small molecule solution can be water; the reaction temperature can be room temperature, and the reaction time can be 1 to 6 hours.
[0024] Preferably, in step (5), the temperature for soaking FeCl3 can be 20-80°C, and the reaction time is 3-10h.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] (1) The cathode and anode layers of the monolithic bipolar membrane prepared by the present invention use the same polymer main chain with the same molecular weight and have opposite charges between the two layers. There is no obvious cathode / cation interface and no obvious "bubbling" phenomenon, thereby effectively improving the mechanical and electrochemical stability of the prepared bipolar membrane.
[0027] (2) The monolithic bipolar membrane prepared by the present invention uses the -NH2 group of the amino-containing polyarylethersulfone substrate membrane to react with the Fe in FeCl3. 3+ Chelation is beneficial to fix metal ions, prevent catalyst leakage, and improve the hydrolysis efficiency and operating stability of the bipolar membrane.
[0028] (3) The ion exchange capacity of the anion / cation layer of the monolithic bipolar membrane prepared by the present invention can be regulated by the concentration of the grafted functional small molecules, the reaction time, and the reaction temperature, and the ratio of the anion layer to the cation layer can be independently regulated by the grafting rate.
[0029] (4) The monolithic bipolar membrane prepared by the present invention adopts hexafluoromethyl polyarylethersulfone as the main chain structure and a rigid fluorine-containing structure, which is beneficial to improving the stability of the bipolar membrane in an acidic and alkaline environment and improving the long-term operation stability of the bipolar membrane. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 Schematic diagram of a possible structure of a monolithic bipolar membrane based on polyarylethersulfone of the present invention;
[0031] Figure 2 It is a schematic diagram of the structure of a jacketed reactor used in the preparation of a monolithic bipolar membrane based on polyarylethersulfone according to the present invention. DETAILED DESCRIPTION
[0032] To further illustrate the technical solution of the present invention, the preferred implementation scheme of the present invention is described below in conjunction with specific examples, but it should be understood that these descriptions are only to further illustrate the features and advantages of the present invention, rather than to limit the claims of the present invention.
[0033] Example 1
[0034] (1) Synthesis of amino-containing polyarylethersulfone:
[0035] Weigh 5.09g (20.00mmol) of 4,4'-difluorodiphenyl sulfone monomer, 4.39g (12.00mmol) of 2,2'-bis (3-amino 4-hydroxyphenyl) hexafluoropropane monomer and 2.69g (8.00mmol) of hexafluorobisphenol A, add 60mL of NMP to a 250mL round-bottom flask equipped with a water separator, and add 5.54g of K2CO3 as a salt-forming agent and 40mL of toluene as a water-carrying agent under nitrogen protection, react at 145℃ for 4h, and heat to 165℃ for 3h. When the solution cools to room temperature, pour it into 400mL of isopropanol, and flocculate to obtain a precipitate under high-speed stirring. After separation by suction filtration, a brown solid is obtained, which is repeatedly washed with isopropanol and water for many times, and vacuum dried at 70℃ for 24h to obtain 12.18g of amino-containing polyarylethersulfone with a molecular weight of 56000.
[0036] (2) Preparation of base film:
[0037] Weigh 1.0 g of the amino-containing polyarylethersulfone obtained in step (1) and place it in a 100 mL three-necked flask equipped with a condenser, add 15 mL of NMP, set the temperature to 60°C under nitrogen protection and react for 3 h. After it is fully dissolved, filter it with a G3 sand core funnel and cast the casting liquid on a clean glass plate. After the solvent is completely evaporated, peel off the film on the glass plate and vacuum dry it at 80°C for 24 h. After completely removing the solvent, obtain an amino-containing polyarylethersulfone film as a substrate membrane.
[0038] (3) Preparation of grafted functional small molecule solution:
[0039] A 30% wt. / v 1,3-propane sultone ethanol solution was selected as the cation grafting functional small molecule solution, and a 86% wt. / v Br-3C-IM aqueous solution was selected as the anion grafting functional small molecule solution. 0.03 mol·L -1 FeCl3 solution and 10 wt. / v NaCl solution.
[0040] The synthesis routes of Br-3C-IM and Br-6C-IM are similar (Journal of Membrane Science, 574 (2019), 181-195). The synthesis method is as follows:
[0041] Add 54.9mL 1,3-dibromopropane and 240mL acetone to a 500mL round-bottom flask, and add 11.16mL N-methylimidazole and 60mL acetone to a constant pressure dropping funnel; under stirring, slowly drip the N-methylimidazole-acetone mixed solution into the round-bottom flask (about 30min), set the temperature to 40℃, and turn on the heating; after the addition is completed, continue to stir the reaction for 24h; after the reaction is completed, filter the white solid by-product with a sand core funnel to obtain a transparent colorless solution; concentrate the filtered solution by rotary evaporation; the concentrated solution is alternately washed with ethyl acetate and anhydrous ether for about 4 times each; the washed solution is rotary evaporated to obtain a light yellow viscous solution, which is the product.
[0042] (4) Preparation of amino-containing polyarylethersulfone positive layer:
[0043] The amino-containing polyarylethersulfone substrate membrane is sandwiched in a jacket reactor. The jacket reactor is as follows: Figure 2 As shown, a 30% ethanol solution of 1,3-propane sultone by weight volume fraction (wt. / v) was selected as the cation grafting functional small molecule solution, one side of the substrate membrane was immersed in the cation grafting functional small molecule solution, and the other side was immersed in a 10% NaCl solution by weight volume fraction (wt. / v). Nitrogen was introduced to eliminate the interference of air. The jacketed reactor was placed in a constant temperature water bath in a sealed state and the temperature was set at 50°C for grafting for 3 hours, so that one side of the membrane was sulfonated and grafted with propane sulfonate. After the reaction was completed, the membrane was placed in 0.1 mol·L -1 The membrane was then hydrolyzed in a NaOH aqueous solution at room temperature for 12 hours. After the reaction, the residual functional small molecule solution and homopolymer in the membrane were removed and dried for later use to obtain a cation exchange layer.
[0044] (5) Preparation of amino-containing polyarylethersulfone film cathode layer:
[0045] The single-sided functionalized poly(arylethersulfone) film obtained in step (4) is sandwiched in a jacket reactor, so that one side of the substrate membrane is the single-sided functionalized poly(arylethersulfone) film obtained in step (4), and the other non-functionalized side is immersed in Br-3C-IM with a mass volume fraction (wt. / v) of 86%, and the other side is an aqueous solution, and nitrogen is introduced to eliminate air interference. The jacket reactor is placed in a constant temperature water bath in a sealed state and the temperature is set to 50°C and maintained for 3 hours, so that different charged functional small molecules are grafted on both sides of the substrate membrane to obtain a "sandwich" bipolar membrane.
[0046] (6) Preparation of FeCl3 complex bipolar membrane:
[0047] The "sandwich" bipolar membrane was placed in a jacketed reactor, nitrogen was introduced to eliminate the influence of air in the system, the device was sealed, and immersed in 0.03 mol·L -1The reaction temperature was room temperature and the reaction time was 2 h. After the reaction, the membrane was washed with deionized water for several times to remove the residual functional small molecule solution and homopolymer in the membrane, and then dried for later use.
[0048] The bipolar membrane prepared in Example 1 was measured to have a thickness of 0.26 mm and a conductivity of 0.025 S·cm at 30°C. -1 ; Water content is 27%; Swelling rate is 12.1%; Cation exchange capacity is 1.11mmol·g -1 ; Anion exchange capacity is 0.32mmol·g -1 ; Transmembrane voltage is 1.15V; Acid-base conversion rate is 90.3%; Current efficiency is 87.1%; Explosion strength is 10.46kg·cm -2 (For specific testing methods, please refer to the literature reports: Journal of Membrane Science 577(2019)153–164; Journal of Materials Chemistry A 9(2021)5485–5496).
[0049] Example 2
[0050] (1) The synthesis of amino-containing polyarylethersulfone is consistent with that in Example 1.
[0051] (2) The preparation of the basement membrane is consistent with that in Example 1.
[0052] (3) Preparation of grafted functional small molecule solution:
[0053] The grafted functional small molecule solution of the positive layer is an ethanol solution of 1,3-propane sultone with a mass volume fraction (wt. / v) of 75%, and the grafted functional small molecule solution of the negative layer is an aqueous solution of Br-3C-IM with a mass volume fraction (wt. / v) of 30%, and the solution is prepared with 0.03 mol·L -1 FeCl3 solution and 32% NaCl solution by weight volume fraction (wt. / v).
[0054] (4) Preparation of amino-containing polyarylethersulfone film positive layer:
[0055] The amino polyarylethersulfone substrate membrane was sandwiched in a jacket reactor, and a 75% 1,3-propanesulfone ethanol solution was selected as the cation grafting functional small molecule solution. One side of the substrate membrane was immersed in the cation grafting functional small molecule solution, and the other side was immersed in a 32% NaCl solution. Nitrogen was introduced to eliminate the interference of air. The jacket reactor was placed in a constant temperature water bath in a sealed state and set at 50°C for 6 hours to graft one side of the membrane with propanesulfonate. After the reaction was completed, the membrane was placed in 0.1 mol·L -1 After the reaction, the residual functional small molecule solution and homopolymer in the membrane were removed and dried for later use to obtain a cation exchange layer; (5) Preparation of the negative layer of amino-containing polyarylethersulfone film:
[0056] The single-sided functionalized polyarylethersulfone film obtained in step (4) is sandwiched in a jacket reactor, so that one side of the base membrane is the single-sided functionalized polyarylethersulfone film obtained in step (4), and the other non-functionalized side is immersed in Br-3C-IM with a mass volume fraction (wt. / v) of 30%, and the other side is an aqueous solution, and nitrogen is introduced to eliminate air interference. The jacket reactor is placed in a constant temperature water bath in a sealed state and the temperature is set to 50°C and maintained for 6 hours. One side of the membrane is grafted with imidazole salt, and different charged functional small molecules are grafted on both sides of the base membrane to obtain a "sandwich" bipolar membrane.
[0057] (6) Preparation of FeCl3 complex bipolar membrane:
[0058] The "sandwich" bipolar membrane was placed in a jacketed reactor, nitrogen was introduced to eliminate the influence of air in the system, the device was sealed, and immersed in 0.03 mol·L -1 The reaction temperature was room temperature and the reaction time was 2 h. After the reaction, the membrane was washed with deionized water for several times to remove the residual functional small molecule solution and homopolymer in the membrane, and then dried for later use.
[0059] The bipolar membrane prepared in Example 2 was measured to have a thickness of 0.21 mm and a conductivity of 0.029 S·cm at 30°C. -1 ; Water content is 25%; Swelling rate is 9.3%; Cation exchange capacity is 1.03mmol·g -1 ; Anion exchange capacity is 0.52mmol·g -1 ; Transmembrane voltage is 1.09V; Acid-base conversion rate is 93.2%; Current efficiency is 88.6%; Explosion strength is 12.98kg·cm -2(For specific testing methods, please refer to the literature reports: Journal of Membrane Science 577(2019)153–164; Journal of Materials Chemistry A 9(2021)5485–5496).
[0060] Example 3
[0061] (1) The synthesis of amino-containing polyarylethersulfone is consistent with that in Example 1.
[0062] (2) The preparation of the basement membrane is consistent with that in Example 1.
[0063] (3) Preparation of grafted functional small molecule solution:
[0064] The grafted functional small molecule solution of the positive layer is a 35% 1,3-propane sultone ethanol solution, and the grafted functional small molecule solution of the negative layer is a 60% Br-3C-IM aqueous solution, with a 0.03 mol·L -1 FeCl3 solution and 12% NaCl solution by weight volume fraction (wt. / v).
[0065] (4) Preparation of amino-containing polyarylethersulfone film positive layer:
[0066] The amino polyarylethersulfone substrate membrane was sandwiched in a jacket reactor, and a 35% ethanol solution of 1,3-propanesulfone was selected as the cation grafting functional small molecule solution. One side of the substrate membrane was immersed in the cation grafting functional small molecule solution, and the other side was immersed in a 12% NaCl solution. Nitrogen was introduced to eliminate the interference of air. The jacket reactor was placed in a constant temperature water bath in a sealed state and set to 40°C for 12 hours to make one side of the membrane undergo sulfonation reaction and graft propanesulfonate. After the reaction was completed, the membrane was placed in 0.1 mol·L -1 The membrane was hydrolyzed in a NaOH aqueous solution at room temperature for 12 hours. After the reaction, the residual functional small molecule solution and homopolymer in the membrane were removed and dried for later use to obtain a cation exchange layer.
[0067] (5) Preparation of amino-containing polyarylethersulfone film cathode layer:
[0068] The single-sided functionalized polyarylethersulfone film obtained in step (4) is sandwiched in a jacket reactor, so that one side of the base membrane is the single-sided functionalized polyarylethersulfone film obtained in step (4), and the other non-functionalized side is immersed in Br-3C-IM with a mass volume fraction (wt. / v) of 30%, and the other side is an aqueous solution, and nitrogen is introduced to eliminate air interference. The jacket reactor is placed in a constant temperature water bath in a sealed state and the temperature is set to 40°C and maintained for 12 hours. One side of the membrane is grafted with imidazole salt, and different charged functional small molecules are grafted on both sides of the base membrane to obtain a "sandwich" bipolar membrane.
[0069] (6) Preparation of FeCl3 complex bipolar membrane:
[0070] The "sandwich" bipolar membrane was placed in a jacketed reactor, nitrogen was introduced to eliminate the influence of air in the system, the device was sealed, and immersed in 0.03 mol·L -1 The reaction temperature was room temperature and the reaction time was 2 h. After the reaction, the membrane was washed with deionized water for several times to remove the residual functional small molecule solution and homopolymer in the membrane, and then dried for later use.
[0071] The bipolar membrane prepared in Example 3 was measured to have a thickness of 0.23 mm and a conductivity of 0.027 S·cm at 30°C. -1 ; Water content is 29%; Swelling rate is 12.8%; Cation exchange capacity is 0.98mmol·g -1 ; Anion exchange capacity is 0.71mmol·g -1 ; Transmembrane voltage is 1.13V; Acid-base conversion rate is 93.1%; Current efficiency is 78.7%; Explosion strength is 11.76kg·cm -2 (For specific testing methods, please refer to the literature reports: Journal of Membrane Science 577(2019)153–164; Journal of Materials Chemistry A 9(2021)5485–5496).
[0072] Example 4
[0073] (1) The synthesis of amino-containing polyarylethersulfone is consistent with that in Example 1.
[0074] (2) The preparation of the basement membrane is consistent with that in Example 1.
[0075] (3) Preparation of grafted functional small molecule solution:
[0076] The grafted functional small molecule solution of the positive layer is an ethanol solution of 1,3-propane sultone with a mass volume fraction (wt. / v) of 80%, and the grafted functional small molecule solution of the negative layer is an aqueous solution of Br-3C-IM with a mass volume fraction (wt. / v) of 30%, and the solution is prepared with 0.03 mol·L -1 FeCl3 solution and 38% NaCl solution by weight volume fraction (wt. / v).
[0077] (4) Preparation of amino-containing polyarylethersulfone film positive layer:
[0078] The amino polyarylethersulfone substrate membrane was sandwiched in a jacket reactor, and an ethanol solution of 1,3-propanesulfone with a mass volume fraction (wt. / v) of 80% was selected as the cation grafting functional small molecule solution. One side of the substrate membrane was immersed in the cation grafting functional small molecule solution, and the other side was immersed in a 38% NaCl solution with a mass volume fraction (wt. / v). Nitrogen was introduced to eliminate the interference of air. The jacket reactor was placed in a constant temperature water bath in a sealed state and set to 40°C, and maintained for 24 hours to allow one side of the membrane to undergo sulfonation reaction and graft propanesulfonate. After the reaction was completed, the membrane was placed in 0.1 mol·L -1 The membrane was hydrolyzed in a NaOH aqueous solution at room temperature for 12 hours. After the reaction, the residual functional small molecule solution and homopolymer in the membrane were removed and dried for later use to obtain a cation exchange layer.
[0079] (5) Preparation of amino-containing polyarylethersulfone film cathode layer:
[0080] The single-sided functionalized polyarylethersulfone film obtained in step (4) is sandwiched in a jacket reactor, so that one side of the base membrane is the single-sided functionalized polyarylethersulfone film obtained in step (4), and the other non-functionalized side is immersed in 30% Br-3C-IM. The other side is an aqueous solution, and nitrogen is introduced to eliminate air interference. The jacket reactor is placed in a sealed state in a constant temperature water bath set at 40°C and maintained for 24 hours. One side of the membrane is grafted with imidazole salt, and different charged functional small molecules are grafted on both sides of the base membrane to obtain a "sandwich" bipolar membrane.
[0081] (6) Preparation of FeCl3 complex bipolar membrane:
[0082] The "sandwich" bipolar membrane was placed in a jacketed reactor, nitrogen was introduced to eliminate the influence of air in the system, the device was sealed, and immersed in 0.03 mol·L -1 The reaction temperature was room temperature and the reaction time was 2 h. After the reaction, the membrane was washed with deionized water for several times to remove the residual functional small molecule solution and homopolymer in the membrane, and then dried for later use.
[0083] The bipolar membrane prepared in Example 4 has a thickness of 0.25 mm and a conductivity of 0.028 S·cm at 30°C. -1 ; Water content is 23%; Swelling rate is 8.4%; Cation exchange capacity is 1.02mmol·g -1 ; Anion exchange capacity is 0.34mmol·g -1 ; Transmembrane voltage is 1.11V; Acid-base conversion rate is 93.3%; Current efficiency is 85.9%; Explosion strength is 12.84kg·cm -2 (For specific testing methods, please refer to the literature reports: Journal of Membrane Science 577(2019)153–164; Journal of Materials Chemistry A 9(2021)5485–5496).
[0084] Example 5
[0085] Similar to Example 1, except that in step (5), a constant temperature water bath was placed at 50°C for grafting for 8 hours. After measurement, the bipolar membrane prepared in Example 5 had a thickness of 0.27 mm and a conductivity of 0.035 S·cm at 30°C. -1 ; Water content is 26%; Swelling rate is 11.7%; Cation exchange capacity is 1.31mmol·g -1 ; Anion exchange capacity is 0.41mmol·g -1 ; Transmembrane voltage is 1.05V; Acid-base conversion rate is 95.6%; Current efficiency is 92.4%; Explosion strength is 13.43kg·cm -2 (For specific testing methods, please refer to the literature reports: Journal of Membrane Science 577(2019)153–164; Journal of Materials Chemistry A 9(2021)5485–5496).
[0086] Example 6
[0087] Similar to Example 3, the difference is that in step (4), the temperature is set to 50°C in a constant temperature water bath for grafting for 8 hours. The bipolar membrane prepared in Example 6 is measured to have a thickness of 0.29 mm and a conductivity of 0.031 S·cm at 30°C. -1 ; Water content is 26%; Swelling rate is 11.7%; Cation exchange capacity is 1.11mmol·g -1 ; Anion exchange capacity is 0.79mmol·g -1 ; Transmembrane voltage is 1.07V; Acid-base conversion rate is 94.1%; Current efficiency is 89.7%; Explosion strength is 13.25kg·cm-2 (For specific testing methods, please refer to the literature reports: Journal of Membrane Science 577(2019)153–164; Journal of Materials Chemistry A 9(2021)5485–5496).
[0088] The performance test data of the monolithic bipolar membrane of each embodiment is shown in Table 1:
[0089]
[0090] Table 1 Performance test data of the monolithic bipolar membrane of each embodiment.
Claims
1. A method for preparing a monolithic bipolar membrane based on polyarylethersulfone, characterized in that The steps include: Step (1): Preparation of amino-containing polyarylethersulfone A certain amount of 4,4'-difluorodiphenyl sulfone monomer, 2,2'-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, hexafluorobisphenol A monomer and potassium carbonate are weighed, dissolved in a high boiling point polar aprotic solvent, precipitated in the solvent after the reaction is completed under nitrogen protection at a certain reaction temperature and reaction time, and vacuum dried at a certain temperature to obtain a main chain amino-containing polyarylethersulfone (PAES-NH2); in formula (I), x and y represent the molar percentages of two links, which are x% and y%, respectively, and x+y=100; wherein x=1-100, y=1-100; wherein the molar ratio of 2,2'-bis(3-amino-4-hydroxyphenyl)hexafluoropropane to hexafluorobisphenol A monomer is 1-80%:99-20%, and its chemical structure is shown in formula (I); Step (2): Preparation of amino-containing polyarylethersulfone film Weigh a certain amount of the amino-containing polyarylethersulfone obtained in step (1), dissolve it in a certain amount of solvent under nitrogen protection, place the casting solution on a clean glass plate after the polymer is completely dissolved, and vacuum dry it at a certain temperature for several hours to obtain an amino-containing polyarylethersulfone film; Step (3): Preparation of the amino-containing polyarylethersulfone film positive layer The amino-containing polyarylethersulfone film obtained in step (2) is sandwiched in a jacket reactor, so that one side of the base membrane is immersed in the cation grafting functional small molecule solution, and the other side is immersed in the NaCl solution, and the cation layer side of the grafted membrane is immersed in the sulfonation reagent, and the sulfonation reaction is carried out at a certain temperature, and nitrogen is introduced. The jacket reactor is placed in a constant temperature water bath in a sealed state, and the cation grafting reaction is carried out at a suitable temperature for a certain period of time, and then a hydrolysis reaction is carried out in a NaOH solution, and then washed with deionized water and dried to obtain a cation exchange layer, whose structural formula is shown in formula (II); Step (4): Preparation of the negative layer of the amino-containing polyarylethersulfone film The single-sided functionalized poly(arylethersulfone) film positive layer obtained in step (3) is sandwiched in a jacketed reactor, and the non-functionalized side is immersed in a solution of small molecules grafted with the negative layer function, and an anion grafting reaction is carried out at a certain temperature, and nitrogen is introduced. The reactor is placed in a sealed state in a constant temperature water bath and set at a suitable temperature to carry out a grafting reaction for a certain period of time, thereby obtaining a poly(arylethersulfone) bipolar membrane; wherein the negative layer structure of the amino-containing poly(arylethersulfone) film is as shown in formula (III); Step (5): FeCl3 complexation based on poly(arylethersulfone) bipolar membrane The polyarylethersulfone bipolar membrane was immersed in a FeCl3 solution at a certain temperature to react for several hours, and then washed with deionized water for several times.
2. The method for preparing a monolithic bipolar membrane according to claim 1, characterized in that: The reaction temperature in step (1) is 100-180° C., the reaction time is 3-24 hours, the high boiling point polar aprotic solvent is N-methylpyrrolidone, and the solvent used for precipitation is isopropanol.
3. The method for preparing a monolithic bipolar membrane according to claim 1, characterized in that: The amount of the polyarylethersulfone described in step (2) is 1-2 g, the amount of the solvent is 15-30 mL, the vacuum drying temperature is 60-80° C., and the vacuum drying time is 18-24 h.
4. The method for preparing a monolithic bipolar membrane according to claim 1, characterized in that: In step (3), the temperature of the constant temperature water bath is 60-90° C., the reaction time can be 4-20 hours, the functional small molecule in the cationic layer grafted functional small molecule solution can be 1,3-propane sultone; the solvent of the cationic layer grafted functional small molecule solution can be ethanol; the temperature of the sulfonation reaction can be 25-70° C., and the sulfonation reaction time can be 1-6 hours.
5. The method for preparing a monolithic bipolar membrane according to claim 1, characterized in that: In step (4), the functional small molecule in the anion layer grafted functional small molecule solution can be Br-3C-IM; the solvent of the anion layer grafted functional small molecule solution can be water; the reaction temperature can be room temperature, and the reaction time can be 1 to 6 hours.
6. The method for preparing a monolithic bipolar membrane according to claim 1, characterized in that: In step (5), the temperature may be 20 to 80° C., and the reaction time may be 3 to 10 hours.
Citation Information
Patent Citations
Single-sheet type bipolar membrane and preparation method thereof
CN105833737A
Ppreparation method for poly(aryl ether sulfone) anion exchange membrane with homogeneous cross-linked structure
CN110756230A
Preparation method of monolithic poly(aryl ether sulfone ketone) bipolar membrane with side chain containing phthalocyanine water dissociation catalytic group
CN111495215A
Preparation method of monolithic polyether sulphone ketone bipolar membrane containing phthalocyanine hydrolysis catalytic group
CN111530298A
Monolithic polytrifluorochloroethylene bipolar membrane containing metal phthalocyanine derivative water dissociation catalyst and preparation method of monolithic polytrifluorochloroethylene bipolar membrane
CN114643083A
Cited By