Sorting system and method for reinforced ferromanganese ore

By combining rotary kiln heating with fluidized bed reduction, high-temperature reduction and roasting of ferromanganese ore by using airflow suspension technology, the problems of inaccurate ore phase conversion and low reduction efficiency in the existing technology are solved, and efficient ferromanganese ore sorting is achieved and efficient use of resources.

CN119016190APending Publication Date: 2024-11-26SHANGHAI MILESTONE TECH CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202411136062.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the prior art, in the sorting process of ferromanganese ore, the oxidation atmosphere and the reduction atmosphere in the rotary kiln are in the same cavity, resulting in inaccurate ore phase conversion, low product uniformity and reduction efficiency, making it difficult to achieve efficient ferromanganese ore sorting.

Method used

Combined with the rotary kiln heating and fluidized bed reduction, the iron-manganese ore after powdering through high-pressure roller milling is heated and dehydrated in the rotary kiln and entered the fluidized bed for reduction and roasting, and high-temperature reduction is performed using airflow suspension technology. The product is then in the stirring tank Cool and sort through a multi-stage magnetic separator.

Benefits of technology

It realizes efficient sorting of ferromanganese ore, improves product quality and sorting efficiency, is suitable for sorting of different types of ferromanganese ore, and can be transformed on the existing rotary kiln production line to revitalize resources, and provides efficient utilization of ferromanganese ore and solutions for upgrading old factories.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016190A_ABST
    Figure CN119016190A_ABST
Patent Text Reader

Abstract

The invention relates to a separation system and method for reinforced ferromanganese ore, and belongs to the technical field of beneficiation, the separation system comprises a high-pressure roller mill, fine ore crushed by the high-pressure roller mill is heated and dehydrated by a rotary kiln and then is fed into a fluidized bed, and the high-temperature fine ore is in a suspended state under the action of airflow and is subjected to reduction roasting; and the reduced product discharged by the fluidized bed enters a stirring tank for cooling and pulping, and ore pulp is sequentially conveyed to a plurality of magnetic separators by a slurry pump for separation and collection. According to the method, the process advantages of rotary kiln heating and fluidized bed reduction are combined, two-stage partition control over heating oxidation and heat storage reduction is achieved, the adaptability to different types of ferromanganese ore is high, and the product quality is high. Meanwhile, under the conditions of large-area loss and production halt of an existing rotary kiln production line, the fluidized bed reduction reactor is added, the ferromanganese ore can be treated, the ineffective assets of enterprises are activated, rapid transformation is achieved, and a new solution is expected to be provided for efficient utilization of the ferromanganese ore and upgrading of old factories.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ore dressing, and in particular relates to a system and method for strengthening the separation of iron and manganese ore, which combines rotary kiln heating with fluidized bed reduction. Background Art

[0002] As an important strategic mineral resource, manganese ore has important applications in many fields such as steel production and battery manufacturing. China is one of the main consumers of manganese ore, but domestic manganese ore resources have problems such as low grade and high mining cost, resulting in a high degree of external dependence. Therefore, the efficient utilization of domestic difficult-to-select manganese ore resources is an important issue currently faced.

[0003] Manganese ore beneficiation technology includes physical beneficiation, reduction leaching and roasting combined method. For high iron, high phosphorus, lean manganese ore and polymetallic manganese ore, it is difficult to obtain satisfactory separation effect by using a single beneficiation method. Roasting combined process is the most effective and economical method for separating difficult manganese ore.

[0004] As a traditional iron ore heating equipment, rotary kiln is usually used for drying and preheating of ore. In the iron-manganese ore sorting system, rotary kiln can effectively carry out the initial heat treatment of ore to prepare for the subsequent reduction process.

[0005] A Chinese patent (publication number: CN112301213A, publication date: February 2, 2021) discloses a manganese ore roasting rotary kiln system, which detects and adjusts the roasting process of manganese ore through a kiln tail gas detection device and a batching quality detection device to achieve high efficiency of the roasting reaction. A Chinese patent (publication number: CN105331800A, publication date: February 17, 2016) discloses a low-grade high-iron manganese ore reduction roasting process, which reduces Fe2O3 / MnO2 in high-iron manganese ore to Fe3O4 / MnO through a rotary kiln, thereby expanding the magnetic difference between iron minerals, manganese minerals and gangue, strengthening subsequent magnetic separation operations, and realizing the separation of manganese, iron and gangue. However, in the above patent, there is an oxidizing atmosphere and a reducing atmosphere in the reactor in the same cavity, and the oxidation reaction and the reduction reaction are carried out simultaneously, which cannot achieve accurate control of the ore phase transformation of manganese ore, and the uniformity of the reduced product needs to be improved. A Chinese patent (publication number: CN108285973A, publication date: July 17, 2018) discloses a roasting device and method for iron oxide and manganese oxide ore. By preheating the material and then statically stacking and reducing it, oxidation and reduction chamber reactions are achieved. The invention utilizes the magnetic difference between the reduced iron and manganese minerals to strengthen the sorting process of iron-manganese ore and achieve the enrichment of manganese concentrate. However, the product uniformity and reduction efficiency of the stacked reduction are still relatively low.

[0006] As an advanced reduction method, fluidized bed technology can achieve the reduction of iron and manganese ore at a lower temperature. Under the action of reducing gas (such as hydrogen or carbon monoxide), the ore particles in the fluidized bed form a fluid-like state, thereby improving the reaction efficiency and reduction speed. This technology is particularly suitable for processing fine particle materials and can significantly improve the reduction efficiency and product quality.

[0007] Based on the above understanding, the present invention provides an enhanced iron-manganese ore sorting system and method that combines rotary kiln heating with fluidized bed reduction, fully utilizing the preheating effect of the rotary kiln and the efficient reduction characteristics of the fluidized bed, strengthening the sorting process of the iron-manganese ore, and realizing the efficient utilization of difficult-to-select iron-manganese ore. Summary of the invention

[0008] In view of the shortcomings of the prior art, the present invention provides a system and method for strengthening the separation of ferromanganese ore, which combines rotary kiln heating with fluidized bed reduction to achieve efficient utilization of difficult-to-separate ferromanganese ore.

[0009] A system for strengthening the separation of iron-manganese ore comprises a high-pressure roller mill. The powder ore crushed by the high-pressure roller mill is heated and dehydrated in a rotary kiln and then fed into a fluidized bed. The high-temperature powder ore is suspended under the action of airflow and subjected to reduction roasting. The reduction product discharged from the fluidized bed enters a stirring tank for cooling and slurrying. The slurry is sequentially transported by a slurry pump to a plurality of magnetic separators for separation and collection.

[0010] A quantitative feeder is arranged between the high pressure roller mill and the rotary kiln, the discharge end of the high pressure roller mill is connected to the inlet of the silo, a quantitative feeder is arranged below the bottom outlet of the silo, and the discharge port of the quantitative feeder matches the feed port of the rotary kiln.

[0011] A multi-channel and multi-stage dust removal system is arranged between the rotary kiln and the fluidized bed.

[0012] The multi-channel multi-stage dust removal system includes a first cyclone separator, a discharge port of a rotary kiln is connected to a feed port of a first flow sealing valve, an air outlet of a rotary kiln is connected to an inlet of the first cyclone separator, an outlet at the bottom end of the first cyclone separator is connected to an inlet of a second flow sealing valve, an air hole at the top of the first cyclone separator is connected to an inlet of a first bag filter; the outlet of the first bag filter is connected to an air inlet of a first induced draft fan, and the bottom ash outlet of the first bag filter is matched with an inlet of a tube chain conveyor; the outlet of the tube chain conveyor is connected to an inlet of an ash hopper, and the bottom discharge port of the ash hopper is connected to a feed port of the first flow sealing valve; the discharge ports of the first flow sealing valve and the second flow sealing valve are both connected to a feed port of a fluidized bed.

[0013] The bottom end of the fluidized bed discharge port is connected with the inlet of the second cyclone separator, the bottom outlet of the second cyclone separator is connected with the feed port in the middle of the top of the fluidized bed, and the top outlet of the second cyclone separator matches with the inlet of the second bag dust collector; the air outlet of the second bag dust collector is connected with the air inlet of the second induced draft fan, the ash outlet of the second bag dust collector matches with the inlet of the ash hopper, and the air outlet of the second induced draft fan matches with the air inlet of the rotary kiln.

[0014] The discharge port of the fluidized bed is connected with the feed port of the third flow sealing valve, the discharge port of the third flow sealing valve is matched with the stirring tank, the slurry in the stirring tank is connected with the inlet of the first magnetic separator through the slurry pump, the tailings outlet of the first magnetic separator is matched with the inlet of the manganese concentrate collector, the concentrate outlet of the first magnetic separator is matched with the inlet of the stirred mill, the outlet of the stirred mill is connected with the outlet of the second magnetic separator, the tailings outlet of the second magnetic separator is matched with the inlet of the manganese middling collector, and the concentrate outlet of the second magnetic separator is matched with the inlet of the iron concentrate collector.

[0015] A method for strengthening the separation of iron-manganese ore, using the above-mentioned system for strengthening the separation of iron-manganese ore, comprises the following steps:

[0016] S1: The crushed iron-manganese ore is further pulverized through a high pressure roller mill to obtain -1.5 mm powder ore, which is stored in a silo;

[0017] S2: Start the rotary kiln and continuously transport the powder ore in the silo to the feed port of the rotary kiln through the quantitative feeder;

[0018] S3: Start the first induced draft fan to generate negative pressure in the first bag filter and the first cyclone separator; introduce high-temperature flue gas generated by natural gas combustion into the rotary kiln to mix it with the powder ore, and heat it to remove the adsorbed water and structure water of the powder ore;

[0019] The heated material enters the first flow sealing valve from the rotary kiln outlet;

[0020] S 4: After the dusty flue gas discharged from the rotary kiln is separated into gas and solid by the first cyclone separator, the dust enters the second flow sealing valve, and the flue gas is discharged from the top of the first cyclone separator, filtered by the first bag filter, and discharged by the first induced draft fan; the dust produced by the first bag filter is transported to the ash hopper by the pipe chain conveyor, and then enters the first flow sealing valve to mix with the high-temperature material discharged from the rotary kiln;

[0021] S5: The materials of the first flow sealing valve and the second flow sealing valve are fed into the fluidized bed from their respective outlets and mixed with each other; coal gas is introduced into the bottom of the fluidized bed, and the high-temperature powder ore is suspended under the action of the airflow and is reduced and roasted, wherein the weakly magnetic Fe 2 O 3 Transformed into strong magnetic Fe3 O 4 , Mn 2 O 3 Converted into MnO; the material after reduction roasting is discharged from the outlet of the fluidized bed as a reduction product;

[0022] S 6: Start the second induced draft fan, and the flue gas in the fluidized bed enters the second cyclone separator from above the discharge port for gas-solid separation. The flue gas contains reduced powder and excess reducing gas; the dust and sand of the second cyclone separator returns to the fluidized bed, and the gas of the second cyclone separator is filtered by the second bag filter and then returned to the rotary kiln for combustion through the second induced draft fan;

[0023] S7: The reduction product discharged from the fluidized bed enters the stirring tank through the third flow sealing valve for cooling and slurrying. The slurry is transported by the slurry pump to the first magnetic separator for magnetic separation. The concentrate separated by magnetic separation is coarse iron concentrate, and the tailings are manganese concentrate, which enter the manganese concentrate collector; the coarse iron concentrate of the first magnetic separator is transported to the stirring mill, and then enters the second magnetic separator for magnetic separation. The concentrate separated by magnetic separation is iron concentrate, and the tailings are manganese middlings, which enter the manganese middling collector. According to actual conditions, it can be added to the manganese concentrate or sold separately, and can also be used as a raw material for smelting manganese-rich slag.

[0024] In the step S1, the crushed ferromanganese ore is 0-15 mm, with an iron grade of TFe of 20-50 and a manganese grade of TMn of 10-35%.

[0025] In step S3, the ore powder entering the rotary kiln stays in the rotary kiln for 20 to 40 minutes, the material is heated, and the material temperature at the rotary kiln outlet is controlled to be 500 to 650° C.;

[0026] In step S5, the temperature of reduction roasting is 450-600°C;

[0027] The high temperature powder ore stays in the fluidized bed for a period of 25 to 45 minutes, i.e., the reduction roasting time.

[0028] The coal gas is producer gas, coke oven gas, blast furnace gas, converter gas or natural gas cracking gas. The main effective components of the coal gas are CO and H 2 , the volume concentration is 40-45%, and the rest includes N 2 , CO 2 With H 2 O; the amount of gas introduced is based on H 2 / CO and Fe 2 O 3 / MnO 2 The excess coefficient is 1.05 to 1.35 times the theoretical amount required for complete reaction, that is, 1.05 to 1.35. The reaction formula is as follows:

[0029] H2 / CO+Fe 2 O 3 →H 2 O / CO 2 +Fe 3 O 4 (1)

[0030] H 2 / CO+MnO 2 →H 2 O / CO 2 +MnO (2).

[0031] In the step S7, the part ground to -0.074 mm accounts for 70-85% of the total mass; the magnetic field strength of the first magnetic separator is 1500-2500 Oe, and the magnetic field strength of the second magnetic separator is 1000-1500 Oe; the TFe grade of the iron concentrate is 57-66%, and the TMn grade of the manganese concentrate is 50-60%. The manganese middlings can be added to the manganese concentrate or sold separately according to actual conditions, and can also be used as a raw material for smelting manganese-rich slag.

[0032] The beneficial effects of the present invention are as follows: the present invention combines the process advantages of rotary kiln heating and fluidized bed reduction, realizes two-stage zoning control of heating oxidation and thermal storage reduction, has strong adaptability to different types of ferromanganese ores, and has high product quality. At the same time, in the case of large-scale losses and shutdowns of existing rotary kiln production lines, the existing excess rotary kiln production lines in the cement and metallurgical industries are transformed and fluidized bed reduction reactors are added to process ferromanganese ores, revitalize the stagnant assets of enterprises and realize rapid transformation, which is expected to provide new solutions for the efficient utilization of ferromanganese ores and the upgrading of old plants. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 A schematic diagram of the enhanced iron-manganese ore separation system provided by the present invention;

[0034] in,

[0035] 1-high pressure roller mill, 2-bin, 3-quantitative feeder, 4-rotary kiln, 5-first induced draft fan, 6-first bag dust collector, 7-tube chain conveyor, 8-first cyclone separator, 9-first flow sealing valve, 10-second flow sealing valve, 11-ash hopper, 12-fluidized bed, 13-second cyclone separator, 14-second bag dust collector, 15-second induced draft fan, 16-third flow sealing valve, 17-stirring tank, 18-first magnetic separator, 19-stirred mill, 20-second magnetic separator, 21-manganese concentrate collector, 22-manganese middling collector, 23-iron concentrate collector. DETAILED DESCRIPTION

[0036] In order to better explain the present invention and facilitate understanding, the technical solutions and effects of the present invention are described in detail below through specific implementation modes in conjunction with the accompanying drawings.

[0037] Example 1

[0038] like Figure 1 As shown, a separation system for strengthening iron-manganese ore includes a high-pressure roller mill 1, the discharge end of the high-pressure roller mill 1 is connected to the inlet of the silo 2, and a quantitative feeder 3 is provided below the bottom outlet of the silo 2, and the discharge port of the quantitative feeder 3 matches the feed port of the rotary kiln 4. The discharge port of the rotary kiln 4 is connected to the feed port of the first flow sealing valve 9, the air outlet of the rotary kiln 4 is connected to the inlet of the first cyclone separator 8, the bottom outlet of the first cyclone separator 8 is connected to the inlet of the second flow sealing valve 10, the top air hole of the first cyclone separator 8 is connected to the inlet of the first bag dust collector 6, the outlet of the first bag dust collector 6 is connected to the air inlet of the first induced draft fan 5, the bottom ash outlet of the first bag dust collector 6 matches the inlet of the tube chain conveyor 7, the outlet of the tube chain conveyor 7 is connected to the inlet of the ash hopper 11, and the bottom discharge port of the ash hopper 11 is connected to the feed port of the first flow sealing valve 9. The outlets of the first flow sealing valve 9 and the second flow sealing valve 10 are both connected to the feed inlet of the fluidized bed 12 .

[0039] The bottom end of the discharge port of the fluidized bed 12 is connected to the inlet of the second cyclone separator 13, the bottom outlet of the second cyclone separator 13 is connected to the feed port in the middle of the top of the fluidized bed 12, and the top outlet of the second cyclone separator 13 matches the inlet of the second bag dust collector 14. The air outlet of the second bag dust collector 14 is connected to the air inlet of the second induced draft fan 15, and the ash outlet of the second bag dust collector 14 matches the inlet of the ash hopper 11. The air outlet of the second induced draft fan 15 matches the air inlet of the rotary kiln 4.

[0040] The discharge port of the fluidized bed 12 is connected with the feed port of the third flow sealing valve 16, the discharge port of the third flow sealing valve 16 is matched with the stirring tank 17, the slurry in the stirring tank 17 is connected with the inlet of the first magnetic separator 18 through the slurry pump, the tailings outlet of the first magnetic separator 18 is matched with the inlet of the manganese concentrate collector 21, the concentrate outlet of the first magnetic separator 18 is matched with the inlet of the stirring mill 19, the outlet of the stirring mill 19 is connected with the outlet of the second magnetic separator 20, the tailings outlet of the second magnetic separator 20 is matched with the inlet of the manganese medium ore collector 22, and the concentrate outlet of the second magnetic separator 20 is matched with the inlet of the iron concentrate collector 23.

[0041] Example 2

[0042] A method for enhancing the separation of iron-manganese ore using an enhanced iron-manganese ore separation system provided in Example 1 specifically comprises the following steps:

[0043] S1: The crushed 0-15mm iron-manganese ore with an iron grade of 28.14% TFe and a manganese grade of 22.34% TMn is further pulverized through a high pressure roller mill 1 to obtain -1.5mm powder ore, which is stored in a silo 2.

[0044] S2: Start the rotary kiln 4 and continuously transport the powder ore in the silo 2 to the feed port of the rotary kiln 4 through the quantitative feeder 3.

[0045] S 3: Start the first induced draft fan 5 to generate negative pressure in the first bag filter 6 and the first cyclone separator 8; introduce high-temperature flue gas generated by natural gas combustion into the rotary kiln 4 to mix it with the powder ore, and heat it to remove adsorbed water and structural water in the powder ore;

[0046] The ore powder entering the rotary kiln 4 stays in the rotary kiln 4 for 25 minutes, and the material is heated; the heated material enters the first flow sealing valve 9 from the outlet of the rotary kiln 4;

[0047] In this step, the material temperature at the discharge port of the rotary kiln 4 is controlled to be 550°C.

[0048] S 4: The dust-containing flue gas discharged from the rotary kiln 4 is separated into gas and solid by the first cyclone separator 8, and the dust enters the second flow sealing valve 10. The flue gas is discharged from the top of the first cyclone separator 8, filtered by the first bag filter 6, and discharged by the first induced draft fan 5; the dust produced by the first bag filter 6 is transported to the ash hopper 11 through the pipe chain conveyor 7, and then enters the first flow sealing valve 9 to mix with the high-temperature material discharged from the rotary kiln 4.

[0049] S5: The materials of the first flow sealing valve 9 and the second flow sealing valve 10 are fed into the fluidized bed 12 from their respective outlets and mixed with each other; coal gas is introduced into the bottom of the fluidized bed 12, and the high-temperature powder ore is suspended under the action of the gas flow and is reduced and roasted at 500°C. The time that the high-temperature powder ore stays in the fluidized bed 12, i.e., the time of reduction roasting, is 30 minutes. Among them, the weakly magnetic Fe 2 O 3 Transformed into strong magnetic Fe 3 O 4 , Mn 2 O 3 The reduced calcined material is discharged from the outlet of the fluidized bed 12 as a reduced product.

[0050] The coal gas is producer gas, coke oven gas, blast furnace gas, converter gas or natural gas cracking gas. The main effective components of the coal gas are CO and H 2 , the volume concentration is 40-45%, and the rest is mainly N 2 , CO 2 With H 2 O, etc.; the amount of gas introduced is based on H2 / CO and Fe 2 O 3 / MnO 2 1.05 to 1.35 times the theoretical amount required for complete reaction, that is, the excess coefficient is 1.05 to 1.35. The reaction formula is as follows:

[0051] H 2 / CO+Fe 2 O 3 →H 2 O / CO 2 +Fe 3 O 4 1

[0052] H 2 / CO+MnO 2 →H 2 O / CO 2 +MnO 2

[0053] In this embodiment, CO and H 2 The volume concentration is 42% and the excess coefficient is 1.10.

[0054] S 6: Start the second induced draft fan 15, and the flue gas in the fluidized bed 12 enters the second cyclone separator 13 from above the discharge port for gas-solid separation. The flue gas contains reduced powder and excess reducing gas; the dust in the second cyclone separator 13 returns to the fluidized bed 12, and the gas in the second cyclone separator 13 is filtered by the second bag filter 14 and then returned to the rotary kiln 4 through the second induced draft fan 15 for combustion, thereby realizing efficient utilization of energy.

[0055] S7: The reduction product discharged from the fluidized bed 12 enters the stirring tank 17 through the third flow sealing valve 16 for cooling and slurrying. The slurry is transported to the first magnetic separator 18 by the slurry pump for magnetic separation. The magnetic field strength is 2000Oe. The concentrate separated by magnetic separation is a coarse iron concentrate, and the tailings is a manganese concentrate. The TMn grade of the manganese concentrate is 52.42%, and enters the manganese concentrate collector 21; the coarse iron concentrate of the first magnetic separator 18 is transported to the stirring mill 19, and is ground to a fineness of -0.074mm. The tailings are manganese middlings with TMn grade of 38.24% and TFe grade of 17.32% respectively, and then enter into the manganese middlings collector 22. According to the actual situation, they can be added into the manganese concentrate or sold separately, and also can be used as the raw material for smelting manganese-rich slag.

[0056] Example 3

[0057] A method for enhancing the separation of iron-manganese ore using an enhanced iron-manganese ore separation system provided in Example 1 specifically comprises the following steps:

[0058] S1: The crushed ferromanganese ore with a diameter of 0-15 mm, an iron grade of 31.14% TFe and a TMn grade of 28.51% is further pulverized by a high pressure roller mill 1 to obtain a powder ore with a diameter of -1.5 mm, which is stored in a silo 2.

[0059] S2: Start the rotary kiln 4 and continuously transport the powder ore in the silo 2 to the feed port of the rotary kiln 4 through the quantitative feeder 3.

[0060] S 3: Start the first induced draft fan 5 to generate negative pressure in the first bag filter 6 and the first cyclone separator 8; introduce high-temperature flue gas generated by natural gas combustion into the rotary kiln 4 to mix it with the powder ore, and heat it to remove adsorbed water and structural water in the powder ore;

[0061] The ore powder entering the rotary kiln 4 stays in the rotary kiln 4 for 36 minutes, and the material is heated; the heated material enters the first flow sealing valve 9 from the outlet of the rotary kiln 4;

[0062] In this step, the material temperature at the discharge port of the rotary kiln 4 is controlled to be 550°C.

[0063] S 4: The dust-containing flue gas discharged from the rotary kiln 4 is separated into gas and solid by the first cyclone separator 8, and the dust enters the second flow sealing valve 10. The flue gas is discharged from the top of the first cyclone separator 8, filtered by the first bag filter 6, and discharged by the first induced draft fan 5; the dust produced by the first bag filter 6 is transported to the ash hopper 11 through the pipe chain conveyor 7, and then enters the first flow sealing valve 9 to mix with the high-temperature material discharged from the rotary kiln 4.

[0064] S 5: The materials of the first flow sealing valve 9 and the second flow sealing valve 10 are fed into the fluidized bed 12 from their respective outlets and mixed with each other; coal gas is introduced into the bottom of the fluidized bed 12, and the high-temperature powder ore is suspended under the action of the airflow and is reduced and roasted at 520°C. The time that the high-temperature powder ore stays in the fluidized bed 12, i.e., the time of reduction roasting, is 40 minutes. Among them, the weakly magnetic Fe 2 O 3 Transformed into strong magnetic Fe 3 O 4 , Mn 2 O 3 The reduced calcined material is discharged from the outlet of the fluidized bed 12 as a reduced product.

[0065] In this embodiment, CO and H 2 The volume concentration is 40% and the excess coefficient is 1.20.

[0066] S 6: Start the second induced draft fan 15, and the flue gas in the fluidized bed 12 enters the second cyclone separator 13 from above the discharge port for gas-solid separation. The flue gas contains reduced powder and excess reducing gas; the dust in the second cyclone separator 13 returns to the fluidized bed 12, and the gas in the second cyclone separator 13 is filtered by the second bag filter 14 and then returned to the rotary kiln 4 through the second induced draft fan 15 for combustion, thereby realizing efficient utilization of energy.

[0067] S7: The reduction product discharged from the fluidized bed 12 enters the stirring tank 17 through the third flow sealing valve 16 for cooling and slurrying. The slurry is transported to the first magnetic separator 18 by the slurry pump for magnetic separation. The magnetic field strength is 2200Oe. The concentrate separated by magnetic separation is a coarse iron concentrate, and the tailings are a manganese concentrate. The TMn grade of the manganese concentrate is 57.33%, and enters the manganese concentrate collector 21; the coarse iron concentrate of the first magnetic separator 18 is transported to the stirring mill 19, and is ground to a fineness of -0.074 mm. The tailings are manganese middlings with a TMn grade of 48.26% and a TFe grade of 12.55%. The tailings enter the manganese middling collector 22 and can be added to the manganese concentrate or sold separately according to actual conditions. They can also be used as raw materials for smelting manganese-rich slag.

[0068] Example 4

[0069] A method for enhancing the separation of iron-manganese ore using an enhanced iron-manganese ore separation system provided in Example 1 specifically comprises the following steps:

[0070] S1: The crushed ferromanganese ore with a diameter of 0-15 mm, an iron grade of 42.54% TFe and a TMn grade of 12.29% is further pulverized by a high pressure roller mill 1 to obtain a powder ore with a diameter of -1.5 mm, which is stored in a silo 2.

[0071] S2: Start the rotary kiln 4 and continuously transport the powder ore in the silo 2 to the feed port of the rotary kiln 4 through the quantitative feeder 3.

[0072] S 3: Start the first induced draft fan 5 to generate negative pressure in the first bag filter 6 and the first cyclone separator 8; introduce high-temperature flue gas generated by natural gas combustion into the rotary kiln 4 to mix it with the powder ore, and heat it to remove adsorbed water and structural water in the powder ore;

[0073] The ore powder entering the rotary kiln 4 stays in the rotary kiln 4 for 23 minutes, and the material is heated; the heated material enters the first flow sealing valve 9 from the outlet of the rotary kiln 4;

[0074] In this step, the material temperature at the discharge port of the rotary kiln 4 is controlled to be 580°C.

[0075] S 4: The dust-containing flue gas discharged from the rotary kiln 4 is separated into gas and solid by the first cyclone separator 8, and the dust enters the second flow sealing valve 10. The flue gas is discharged from the top of the first cyclone separator 8, filtered by the first bag filter 6, and discharged by the first induced draft fan 5; the dust produced by the first bag filter 6 is transported to the ash hopper 11 through the pipe chain conveyor 7, and then enters the first flow sealing valve 9 to mix with the high-temperature material discharged from the rotary kiln 4.

[0076] S 5: The materials of the first flow sealing valve 9 and the second flow sealing valve 10 are fed into the fluidized bed 12 from their respective outlets and mixed with each other; coal gas is introduced into the bottom of the fluidized bed 12, and the high-temperature powder ore is suspended under the action of the airflow and is reduced and roasted at 520°C. The time that the high-temperature powder ore stays in the fluidized bed 12, i.e., the time of reduction roasting, is 27 minutes. Among them, the weakly magnetic Fe 2 O 3 Transformed into strong magnetic Fe 3 O 4 , Mn 2 O 3 The reduced calcined material is discharged from the outlet of the fluidized bed 12 as a reduced product.

[0077] In this embodiment, CO and H 2 The volume concentration is 40% and the excess coefficient is 1.25.

[0078] S 6: Start the second induced draft fan 15, and the flue gas in the fluidized bed 12 enters the second cyclone separator 13 from above the discharge port for gas-solid separation. The flue gas contains reduced powder and excess reducing gas; the dust in the second cyclone separator 13 returns to the fluidized bed 12, and the gas in the second cyclone separator 13 is filtered by the second bag filter 14 and then returned to the rotary kiln 4 through the second induced draft fan 15 for combustion, thereby realizing efficient utilization of energy.

[0079] S7: The reduction product discharged from the fluidized bed 12 enters the stirring tank 17 through the third flow sealing valve 16 for cooling and slurrying. The slurry is transported to the first magnetic separator 18 by the slurry pump for magnetic separation. The magnetic field strength is 1600Oe. The concentrate separated by magnetic separation is a coarse iron concentrate, and the tailings are a manganese concentrate. The TMn grade of the manganese concentrate is 50.84%, and enters the manganese concentrate collector 21; the coarse iron concentrate of the first magnetic separator 18 is transported to the stirring mill 19, and is ground to a fineness of -0.074 mm. The tailings are manganese middlings with a TMn grade of 36.49% and a TFe grade of 16.32%. The tailings enter the manganese middling collector 22 and can be added to the manganese concentrate or sold separately according to actual conditions. They can also be used as raw materials for smelting manganese-rich slag.

[0080] Example 5

[0081] A method for enhancing the separation of iron-manganese ore using an enhanced iron-manganese ore separation system provided in Example 1 specifically comprises the following steps:

[0082] S1: The crushed ferromanganese ore with a diameter of 0-15 mm, an iron grade of 24.33% TFe and a TMn grade of 30.65% is further pulverized by a high pressure roller mill 1 to obtain a powder ore with a diameter of -1.5 mm, which is stored in a silo 2.

[0083] S2: Start the rotary kiln 4 and continuously transport the powder ore in the silo 2 to the feed port of the rotary kiln 4 through the quantitative feeder 3.

[0084] S 3: Start the first induced draft fan 5 to generate negative pressure in the first bag filter 6 and the first cyclone separator 8; introduce high-temperature flue gas generated by natural gas combustion into the rotary kiln 4 to mix it with the powder ore, and heat it to remove adsorbed water and structural water in the powder ore;

[0085] The ore powder entering the rotary kiln 4 stays in the rotary kiln 4 for 40 minutes, and the material is heated; the heated material enters the first flow sealing valve 9 from the outlet of the rotary kiln 4;

[0086] In this step, the material temperature at the discharge port of the rotary kiln 4 is controlled to be 575°C.

[0087] S 4: The dust-containing flue gas discharged from the rotary kiln 4 is separated into gas and solid by the first cyclone separator 8, and the dust enters the second flow sealing valve 10. The flue gas is discharged from the top of the first cyclone separator 8, filtered by the first bag filter 6, and discharged by the first induced draft fan 5; the dust produced by the first bag filter 6 is transported to the ash hopper 11 through the pipe chain conveyor 7, and then enters the first flow sealing valve 9 to mix with the high-temperature material discharged from the rotary kiln 4.

[0088] S5: The materials of the first flow sealing valve 9 and the second flow sealing valve 10 are fed into the fluidized bed 12 from their respective outlets and mixed with each other; coal gas is introduced into the bottom of the fluidized bed 12, and the high-temperature powder ore is suspended under the action of the airflow and is reduced and roasted at 540°C. The time that the high-temperature powder ore stays in the fluidized bed 12, i.e., the time of reduction roasting, is 30 minutes. Among them, the weakly magnetic Fe 2 O 3 Transformed into strong magnetic Fe 3 O 4 , Mn 2 O 3 The reduced calcined material is discharged from the outlet of the fluidized bed 12 as a reduced product.

[0089] In this embodiment, CO and H 2 The volume concentration is 45% and the excess coefficient is 1.15.

[0090] S 6: Start the second induced draft fan 15, and the flue gas in the fluidized bed 12 enters the second cyclone separator 13 from above the discharge port for gas-solid separation. The flue gas contains reduced powder and excess reducing gas; the dust in the second cyclone separator 13 returns to the fluidized bed 12, and the gas in the second cyclone separator 13 is filtered by the second bag filter 14 and then returned to the rotary kiln 4 through the second induced draft fan 15 for combustion, thereby realizing efficient utilization of energy.

[0091] S7: The reduction product discharged from the fluidized bed 12 enters the stirring tank 17 through the third flow sealing valve 16 for cooling and slurrying. The slurry is transported to the first magnetic separator 18 by the slurry pump for magnetic separation. The magnetic field strength is 1700Oe. The concentrate separated by magnetic separation is a coarse iron concentrate, and the tailings are a manganese concentrate. The TMn grade of the manganese concentrate is 58.62%, and enters the manganese concentrate collector 21; the coarse iron concentrate of the first magnetic separator 18 is transported to the stirring mill 19, and is ground to a fineness of -0.074 mm. The tailings are manganese middlings with a TMn grade of 45.31% and a TFe grade of 11.23%. The tailings enter the manganese middling collector 22 and can be added to the manganese concentrate or sold separately according to actual conditions. They can also be used as raw materials for smelting manganese-rich slag.

Claims

1. A system for strengthening the separation of iron and manganese ore, characterized in that: The invention comprises a high-pressure roller mill (1). The powder ore crushed by the high-pressure roller mill (1) is heated and dehydrated by a rotary kiln (4) and then fed into a fluidized bed (12). The high-temperature powder ore is suspended under the action of airflow and subjected to reduction roasting. The reduction product discharged from the fluidized bed (12) enters a stirring tank (17) for cooling and slurrying. The slurry is sequentially transported by a slurry pump to a plurality of magnetic separators for sorting and collection.

2. A system for strengthening the separation of iron and manganese ore according to claim 1, characterized in that: A quantitative feeder (3) is arranged between the high-pressure roller mill (1) and the rotary kiln (4); the discharge end of the high-pressure roller mill (1) is connected to the inlet of the silo (2); a quantitative feeder (3) is arranged below the bottom outlet of the silo (2); and the discharge port of the quantitative feeder (3) matches the feed port of the rotary kiln (4).

3. A system for strengthening the separation of iron-manganese ore according to claim 2, characterized in that: A multi-channel multi-stage dust removal system is arranged between the rotary kiln (4) and the fluidized bed (12).

4. A system for strengthening the separation of iron and manganese ore according to claim 3, characterized in that: The multi-channel multi-stage dust removal system comprises a first cyclone separator (8), a material discharge port of a rotary kiln (4) is connected to a material feed port of a first flow sealing valve (9), an air outlet of the rotary kiln (4) is connected to an inlet of the first cyclone separator (8), an outlet at the bottom end of the first cyclone separator (8) is connected to an inlet of a second flow sealing valve (10), and an air hole at the top of the first cyclone separator (8) is connected to an inlet of a first bag filter (6); the outlet of the first bag filter (6) is connected to an air inlet of a first induced draft fan (5), and the bottom ash discharge port of the first bag filter (6) is matched with an inlet of a tube chain conveyor (7); the outlet of the tube chain conveyor (7) is connected to an inlet of an ash hopper (11), and the bottom material discharge port of the ash hopper (11) is connected to the material feed port of the first flow sealing valve (9); the material discharge ports of the first flow sealing valve (9) and the second flow sealing valve (10) are both connected to a material feed port of a fluidized bed (12).

5. A system for strengthening the separation of iron and manganese ore according to claim 4, characterized in that: The bottom end of the fluidized bed (12) discharge port is connected to the inlet of the second cyclone separator (13), the bottom outlet of the second cyclone separator (13) is connected to the feed port in the middle of the top end of the fluidized bed (12), and the top outlet of the second cyclone separator (13) is matched with the inlet of the second bag dust collector (14); the air outlet of the second bag dust collector (14) is connected to the air inlet of the second induced draft fan (15), the ash outlet of the second bag dust collector (14) is matched with the inlet of the ash hopper (11), and the air outlet of the second induced draft fan (15) is matched with the air inlet of the rotary kiln (4).

6. A system for strengthening the separation of iron and manganese ore according to claim 1, characterized in that: The discharge port of the fluidized bed (12) is connected to the feed port of the third flow sealing valve (16), the discharge port of the third flow sealing valve (16) is matched with the stirring tank (17), the slurry in the stirring tank (17) is connected to the inlet of the first magnetic separator (18) through the slurry pump, the tailings outlet of the first magnetic separator (18) is matched with the inlet of the manganese concentrate collector (21), the concentrate outlet of the first magnetic separator (18) is matched with the inlet of the stirring mill (19), the outlet of the stirring mill (19) is connected to the outlet of the second magnetic separator (20), the tailings outlet of the second magnetic separator (20) is matched with the inlet of the manganese medium ore collector (22), and the concentrate outlet of the second magnetic separator (20) is matched with the inlet of the iron concentrate collector (23).

7. A method for strengthening the separation of iron-manganese ore, using the system for strengthening the separation of iron-manganese ore according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1: The crushed iron-manganese ore is further pulverized by a high pressure roller mill (1) to obtain -1.5 mm powder ore, which is stored in a silo (2); S2: starting the rotary kiln (4) and continuously conveying the powder ore in the silo (2) to the feed inlet of the rotary kiln (4) through the quantitative feeder (3); S3: starting the first induced draft fan (5) to generate negative pressure in the first bag filter (6) and the first cyclone separator (8); introducing high-temperature flue gas generated by the combustion of natural gas into the rotary kiln (4) to mix it with the powdered ore, and heating to remove adsorbed water and structural water in the powdered ore; The heated material enters the first flow sealing valve (9) from the outlet of the rotary kiln (4); S4: The dust-containing flue gas discharged from the rotary kiln (4) is separated into gas and solid by the first cyclone separator (8), and the dust enters the second flow sealing valve (10). The flue gas is discharged from the top of the first cyclone separator (8), filtered by the first bag filter (6), and discharged by the first induced draft fan (5); the dust produced by the first bag filter (6) is transported to the ash hopper (11) by the pipe chain conveyor (7), and then enters the first flow sealing valve (9) to mix with the high-temperature material discharged from the rotary kiln (4); S5: the materials of the first flow sealing valve (9) and the second flow sealing valve (10) are fed into the fluidized bed (12) from their respective discharge ports and mixed with each other; coal gas is introduced into the bottom of the fluidized bed (12), and the high-temperature powder ore is suspended under the action of the gas flow and subjected to reduction roasting, wherein the weakly magnetic Fe2O3 is converted into the strongly magnetic Fe3O4, and the Mn2O3 is converted into MnO; the materials after reduction roasting are discharged from the outlet of the fluidized bed (12) as reduction products; S6: Start the second induced draft fan (15), and the flue gas in the fluidized bed (12) enters the second cyclone separator (13) from above the discharge port for gas-solid separation. The flue gas contains reduced powder and excess reducing gas; the dust in the second cyclone separator (13) returns to the fluidized bed (12), and the gas in the second cyclone separator (13) is filtered by the second bag filter (14) and then returned to the rotary kiln (4) for combustion through the second induced draft fan (15); S7: The reduction product discharged from the fluidized bed (12) enters the stirring tank (17) through the third flow sealing valve (16) for cooling and slurrying. The slurry is transported by the slurry pump to the first magnetic separator (18) for magnetic separation. The concentrate separated by magnetic separation is a coarse iron concentrate, and the tailings are a manganese concentrate, which enter the manganese concentrate collector (21). The coarse iron concentrate from the first magnetic separator (18) is transported to the stirring mill (19) and then enters the second magnetic separator (20) for magnetic separation. The concentrate separated by magnetic separation is an iron concentrate, and the tailings are a manganese medium ore, which enter the manganese medium ore collector (22). According to actual conditions, the concentrate can be added to the manganese concentrate or sold separately, and can also be used as a raw material for smelting manganese-rich slag.

8. A method for strengthening the separation of iron-manganese ore according to claim 7, characterized in that: In the step S1, the crushed ferromanganese ore is 0-15 mm, with an iron grade of TFe of 20-50 and a manganese grade of TMn of 10-35%.

9. A method for strengthening the separation of iron-manganese ore according to claim 7, characterized in that: In the step S3, the ore powder entering the rotary kiln (4) stays in the rotary kiln (4) for 20 to 40 minutes, the material is heated, and the material temperature at the outlet of the rotary kiln (4) is controlled to be 500 to 650° C.; In step S5, the temperature of reduction roasting is 450-600°C; The time that the high-temperature powder ore stays in the fluidized bed (12), i.e., the time for reduction roasting, is 25 to 45 minutes; The coal gas is producer gas, coke oven gas, blast furnace gas, converter gas or natural gas cracking gas, the main effective components of the coal gas are CO and H2, the volume concentration is 40-45%, and the rest includes N2, CO2 and H2O; the amount of coal gas introduced is 1.05-1.35 times the theoretical amount required for the complete reaction of H2 / CO and Fe2O3 / MnO2, that is, the excess coefficient is 1.05-1.35, and the reaction formula is as follows: H2 / CO+Fe2O3→H2O / CO2+Fe3O4 (1) H2 / CO+MnO2→H2O / CO2+MnO (2).

10. A method for strengthening the separation of iron-manganese ore according to claim 7, characterized in that: In the step S7, the portion ground to -0.074 mm accounts for 70-85% of the total mass; the magnetic field strength of the first magnetic separator (18) is 1500-2500 Oe, and the magnetic field strength of the second magnetic separator (20) is 1000-1500 Oe; the TFe grade of the iron concentrate is 57-66%, and the TMn grade of the manganese concentrate is 50-60%. The manganese middlings can be added to the manganese concentrate or sold separately according to actual conditions, and can also be used as a raw material for smelting manganese-rich slag.

Citation Information

Patent Citations

  • Reducing roasting process for low-grade high-iron manganese ore

    CN105331800A

  • Suspension roasting manganese and iron treatment method of iron-contained manganese ore

    CN107523684A

  • Suspension roasting comprehensive utilization system and method for iron containing manganese ore

    CN107523685A

  • Complex iron ore reinforced separation system capable of precisely regulating and controlling mineral phases in sections

    CN111482269A

  • Suspension roasting system and method for industrially processing ferromanganese ore

    CN111500854A