High-precision manufacturing method of large-size ternary blade
By controlling the preheating and installation time, combined with the press-type tire tool and cooling treatment, the problem of insufficient processing accuracy of large-scale ternary blades is solved, efficient impeller finished product manufacturing is achieved, and the technical requirements of impeller operation efficiency is met.
Patent Information
- Application Number
- CN202411144423.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-26
AI Technical Summary
During the press-forming manufacturing process, large ternary blades have insufficient precision in the finished product line and cannot meet the technical requirements of impeller operation efficiency.
By controlling the preheating and installation time of the initial blades, it is ensured that it is fully heated and uniformly cooled during the processing of the press-type tires. The press-type tires are used for press-type tires, combined with air-cooling and water-cooling cooling treatments, ensuring that the blades are in Shaping at high temperatures limits preheating and pressing time to avoid uneven temperature and uneven deformation.
The machining accuracy of large-size ternary blades is improved, the operation efficiency of the impeller is ensured, and the uneven pressure response and deformation caused by temperature drop and uneven cooling are avoided, which improves the accuracy of finished blades.
Smart Images

Figure CN119016676A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of compressor manufacturing, and in particular to a high-precision manufacturing method for large-sized three-dimensional blades. Background Art
[0002] The impeller in a centrifugal compressor is usually composed of a wheel disc, blades, and a wheel cover, wherein the blades are located between the wheel disc and the wheel cover. In order to reduce the cost of raw materials for impeller forgings, the prior art usually adopts the method of welding the wheel disc, blades, and wheel cover to form an impeller.
[0003] Since large three-dimensional blades are thick, usually more than 30 mm, and are in a three-dimensional distorted state, they need to be pressed using a mold. The existing pressing method is to preheat the raw material and then transfer it to the mold for pressing, but there is no operating specification for the preheating time and transfer time, resulting in insufficient precision of the finished product line of the three-dimensional blade, causing the impeller operation efficiency to fail to meet the technical requirements. Summary of the invention
[0004] In view of this, an embodiment of the present invention provides a high-precision manufacturing method for large-sized three-dimensional blades, the main purpose of which is to ensure the pressing accuracy by controlling the preheating and installation time.
[0005] In order to achieve the above object, the present invention mainly provides the following technical solutions:
[0006] The embodiment of the present invention provides a high-precision manufacturing method for a large-sized three-dimensional blade, comprising:
[0007] Obtaining raw materials, and processing the raw materials using a leaf unfolding template to obtain an initial leaf;
[0008] Performing a preheating treatment on the initial blade for a first preset time;
[0009] Within a second preset time, the initial blade after preheating is mounted on a molding die;
[0010] The initial blades are pressed using a pressing jig to obtain finished blades.
[0011] The step of preheating the initial blades for a first preset time is specifically as follows:
[0012] Using a heating furnace to heat the initial blade to a temperature not lower than a preset minimum temperature, and heating the initial blade for a first preset time starting from when the temperature of the heating furnace reaches the preset minimum temperature;
[0013] The first preset time is not less than 90 minutes and not more than 120 minutes, and the preset minimum temperature is not less than 1050°C.
[0014] The second preset time is no more than 90 seconds.
[0015] The step of installing the initial blade after preheating treatment on the pressing mold within the second preset time is specifically as follows:
[0016] Perform the following operations within the second preset time:
[0017] Place the initial blade on the profiling jig, and adjust the blade inlet end and the blade-to-shaft disc welding end of the initial blade to ensure there is no gap between the positioning pins of the profiling jig.
[0018] The manufacturing method according to claim 1 is characterized in that between the step of using a molding die to mold the initial blade to obtain a finished blade, the method further comprises:
[0019] If the time for installing the preheated initial blade on the molding jig exceeds 180 seconds, the initial blade is preheated again for the first preset time.
[0020] The step of using a molding die to mold the initial blade to obtain a finished blade specifically includes:
[0021] The initial blades are pressed using a pressing jig, and the tonnage of the press connected to the pressing jig is not less than 600 tons;
[0022] During the profiling process, a feeler gauge is used to try to enter between the initial blade and the positioning pin at a preset time interval. If a feeler gauge larger than the preset size can enter, the initial blade is preheated again for the first preset time, and the preset size is not greater than 1 mm.
[0023] During the profiling process, the initial blades are cooled;
[0024] When the initial temperature around the blade is not greater than 100° C. and the pressing time is not less than 60 minutes, the pressing operation is completed to obtain a finished blade.
[0025] Among them, during the profiling process, the step of cooling the initial blade is specifically as follows:
[0026] The initial blades are air-cooled and the molds are water-cooled.
[0027] Wherein, after the step of using a molding die to mold the initial blade to obtain a finished blade, the method further comprises:
[0028] After a third preset time, testing the finished blades;
[0029] The third preset time is not less than 24 hours.
[0030] The steps of testing the finished blades specifically include:
[0031] Perform three-dimensional scanning on the finished blade to obtain actual three-dimensional image information of the finished blade;
[0032] Obtain theoretical three-dimensional image information corresponding to the finished blade;
[0033] The actual 3D image information is compared with the theoretical 3D image information, and the accuracy of the finished blade is determined based on the image deviation results.
[0034] The steps of testing the finished blades specifically include:
[0035] Place the finished blade on the lower mold of the molding jig, and adjust the blade inlet end of the finished blade and the welding end of the blade and the shaft disc to ensure that there is no gap between the positioning pin of the molding jig;
[0036] Use a feeler gauge to measure the gap between each test point on the finished blade and the lower mold, record the data, and form data 1;
[0037] The finished blade is placed back on the upper mold of the molding jig, and the blade inlet end of the finished blade and the welding end of the blade and the shaft disc are adjusted to have no gap between the positioning pin of the molding jig;
[0038] Use a feeler gauge to measure the gap between each test point on the finished blade and the upper mold, record the data, and form data 2;
[0039] Determine the accuracy of the finished blade based on Data 2 and Data 1.
[0040] By means of the above technical solution, the present invention has at least the following beneficial effects:
[0041] The high-precision manufacturing method for large-size three-dimensional blades provided by the embodiment of the present invention limits the time of preheating treatment to a first preset time, and limits the time from the initial blade after preheating treatment to the start of pressing of the pressing mold to a second preset time, thereby ensuring that the initial blade is fully and evenly heated, avoiding the problem of temperature drop and uneven cooling caused by the blade being placed for a long time before pressing, thereby making the blade temperature high and easy to shape, ensuring the pressing effect, avoiding uneven pressing response caused by uneven initial blade temperature, and avoiding uneven deformation of the blade after pressing. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 A flow chart of a high-precision manufacturing method for a large-sized three-dimensional blade provided by an embodiment of the present invention;
[0043] Figure 2 A flow chart of another method for high-precision manufacturing of large-sized three-dimensional blades provided by an embodiment of the present invention;
[0044] Figure 3 A flow chart of another method for high-precision manufacturing of large-sized three-dimensional blades provided by an embodiment of the present invention;
[0045] Figure 4 A schematic diagram of the structure of a large-sized three-dimensional blade provided in an embodiment of the present invention;
[0046] Figure 5 A schematic diagram of the structure of a blade deployment template provided by an embodiment of the present invention;
[0047] Figure 6 A schematic structural diagram of a mold press provided by an embodiment of the present invention;
[0048] Figure 7 A schematic diagram of the structure of an initial blade, a molding jig and a positioning pin provided in an embodiment of the present invention;
[0049] Figure 8 A schematic diagram of the position of the blade inlet end provided in an embodiment of the present invention;
[0050] Fig. 9 A schematic diagram of the position of the welding end of the blade and the shaft disc provided in an embodiment of the present invention;
[0051] Fig.10 A schematic diagram of the positions of the blade inlet end, the blade and the shaft disc welding end, and the positioning pin provided in an embodiment of the present invention;
[0052] Fig.11 A schematic diagram of the detection position of a finished blade provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0053] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme in the embodiment of the present invention will be described in more detail below in conjunction with the drawings in the preferred embodiments of the present invention. In the drawings, the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The described embodiments are part of the embodiments of the present invention, not all of them. The embodiments described below with reference to the drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limitations on the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. The embodiments of the present invention are described in detail below in conjunction with the drawings.
[0054] In the description of this embodiment, it should be understood that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship, are based on the orientation or position relationship shown in the accompanying drawings, and are only for the convenience of describing this embodiment and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the scope of protection of this embodiment.
[0055] The embodiment of the present invention provides a high-precision manufacturing method for a large-sized three-dimensional blade, which is used to manufacture a large-sized three-dimensional blade, such as Figure 4 Taking the blade shown as an example, the blade features are: the blade material is FV520B stainless steel, the unfolded template corresponding to the blade size is between 800mm×400mm and 1000mm×800mm, the blade thickness is between 35mm-50mm, the blade thickness is equal at all locations, and the blade as a whole is in a three-dimensional space twisted shape.
[0056] In one embodiment, if Figure 1 As shown, the method includes:
[0057] S1-1, obtaining raw materials, and processing the raw materials using a blade expansion template to obtain an initial blade 100.
[0058] After the blade design is completed, the software is used to perform two-dimensional lofting on the blade's three-dimensional shape to obtain a two-dimensional plane shape. The blade unfolding template tool is cut on the template according to the two-dimensional plane shape, such as Figure 5 As shown, the thickness of the blade expansion template is usually about 2mm. The blade base material is selected as needed, and the base material surface is required to be flat. The blade material can be FV520B stainless steel plate. Then the blade expansion template is placed on the surface of the base material and fixed, such as by a clamp or temporary welding. Use CNC cutting equipment such as wire cutting to cut around the edge of the blade expansion template to obtain a cut rough material, and then grind or mill the upper and lower surface planes of the rough material to obtain a flat initial blade 100.
[0059] S1-2, performing a preheating treatment on the initial blade 100 for a first preset time.
[0060] The preheating treatment is carried out in an additional heating furnace that is different from the molding mold. The preheating treatment should ensure that the initial blade 100 reaches a sufficient temperature and heating time. For example, the step of preheating the initial blade 100 for a first preset time is specifically: using a heating furnace to heat the initial blade 100 to a temperature not lower than a preset minimum temperature, and continuing for a first preset time from the time when the furnace temperature of the heating furnace reaches the preset minimum temperature. Then, on the one hand, it ensures that the initial blade 100 can have a high enough temperature for smooth molding, and on the other hand, it avoids uneven internal temperature caused by short heating time, resulting in different plasticity of various areas of the blade during molding, and avoiding affecting the molding accuracy. In some embodiments, the first preset time is not less than 90 minutes, and not more than 120 minutes, and the preset minimum temperature is not less than 1050°C. For example, the initial blade 100 may be heated to 1050° C. in a heating furnace, and the preheating time may be started when the furnace temperature reaches 1050° C. When the preheating time reaches 90 minutes, the preheating is completed, or when the preheating time reaches 100 minutes, 105 minutes, or 120 minutes, the preheating is completed.
[0061] S1-3, within a second preset time, the initial blade 100 after preheating is mounted on a molding jig.
[0062] Use Figure 6 The molding jig shown is used to mold the initial blade 100. The molding jig includes an upper jig 602 and a lower jig 601. The initial blade 100 needs to be placed on the lower jig 601 and the position is adjusted. A plurality of positioning pins 701 are provided on the lower jig 601. Figure 7 The solid line in the middle corresponds to the edge shape of the lower mold 601, the dotted line corresponds to the edge shape of the initial blade 100, and the circles scattered around the outer circumference of the initial blade 100 are the positions of the positioning pins 701. The installation of the initial blade 100 requires that both sides of the initial blade 100 (the blade inlet end 101 and the blade-to-shaft disc welding end 102) be in close contact with the positioning pins 701 as the positioning position, and there must be no gap at the close contact position. Among them, ensuring that there is no gap means that the gap is smaller than the preset gap. More specifically, it may be a step of installing the initial blade 100 after the preheat treatment on the molding mold within the second preset time, specifically: perform the following operations within the second preset time: place the initial blade 100 on the molding mold, and adjust the blade inlet end 101 and the blade-to-shaft disc welding end 102 of the initial blade 100 to have no gap with the positioning pins 701 of the molding mold. Figure 8 As shown, the black and bold line along the edge of the initial blade 100 is the blade inlet end 101 of the initial blade 100. Fig. 9 As shown in FIG. 1 , the black and thick line at the edge of the initial blade 100 is the welding end 102 between the blade and the shaft disk. Fig.10As shown, the bold lines are the blade inlet end 101 and the blade and shaft disc welding end 102 of the initial blade 100, and there is no gap between the two and the positioning pin 701. A 0.1 mm feeler gauge can be used to try to enter between the blade inlet end 101 and the blade and shaft disc welding end 102 and the positioning pin 701. If it cannot enter, it can be considered that there is no gap.
[0063] The initial blade 100 at high temperature is conducive to deformation during the profiling operation, so the time from picking up the initial blade 100 from the heating furnace to placing the initial blade 100 on the profiling jig should be shortened as much as possible. Usually, the time from picking up and transporting the initial blade 100 to the completion of the position adjustment of the initial blade 100 on the profiling jig, or the time from picking up the initial blade 100 to the start of profiling of the initial blade 100 by the profiling jig, should not exceed 90 seconds (at this time, the ambient temperature is 15-35°C. If the ambient temperature is too low, the interval time should be further reduced). Once the time from picking up and transporting the initial blade 100 to the completion of the position adjustment of the initial blade 100 on the profiling jig exceeds 180 seconds, it is necessary to re-execute step S1-2 to preheat the initial blade 100.
[0064] S1-4, using a molding die to mold the initial blade 100 to obtain a finished blade.
[0065] The upper mold 602 and the lower mold 601 are used to cooperate with a press to extrude the initial blade 100 from both sides, and then the high-temperature initial blade 100 is compression-molded. The tonnage of the press used during the compression molding needs to be as large as possible to ensure the compression molding effect. For example, when the initial blade 100 is compressed by the compression molding mold, the tonnage of the press connected to the compression molding mold is not less than 600 tons.
[0066] The high-precision manufacturing method for large-size three-dimensional blades provided by the embodiment of the present invention limits the time of preheating treatment to a first preset time, and limits the time from the initial blade after preheating treatment to the start of pressing of the pressing mold to a second preset time, thereby ensuring that the initial blade is fully and evenly heated, avoiding the problem of temperature drop and uneven cooling caused by the blade being placed for a long time before pressing, thereby making the blade temperature high and easy to shape, ensuring the pressing effect, avoiding uneven pressing response caused by uneven initial blade temperature, and avoiding uneven deformation of the blade after pressing.
[0067] like Figure 2 As shown, the embodiment of the present invention also provides another method, including:
[0068] S2-1, obtaining raw materials, and processing the raw materials using a blade expansion template to obtain an initial blade 100.
[0069] S2-2, performing a preheating treatment on the initial blade 100 for a first preset time.
[0070] S2-3, within a second preset time, the initial blade 100 after the preheating treatment is installed on a molding jig.
[0071] S2-4, the initial blade 100 is pressed by a pressing jig. During the pressing process, a feeler gauge is used to try to enter between the initial blade 100 and the positioning pin 701 at preset intervals. If a feeler gauge larger than the preset size can enter, step S2-2 is performed again on the initial blade 100 to perform a preheating treatment for a first preset time.
[0072] The preset size is not greater than 1 mm. The preset interval time can be 3 minutes, 5 minutes, 8 minutes, etc., and the interval time needs to be as short as possible. The feeler gauge can be used to try to enter between the initial blade 100 and the positioning pin 701, which can be between the blade inlet end 101 of the initial blade 100 and the positioning pin 701 and between the blade and the shaft disc welding end 102 and the positioning pin 701. During the profiling process of the initial blade 100, the close positioning position is frequently measured with a feeler gauge to ensure that a 1mm feeler gauge cannot enter. If there is a gap of more than 1mm between the blade inlet end 101 of the initial blade 100 and the positioning pin 701 and / or between the blade and the shaft disc welding end 102 and the positioning pin 701 during the profiling process, that is, a 1mm feeler gauge can enter, then the initial blade 100 needs to be re-performed with step S2-2 and preheated for the first preset time.
[0073] S2-5. During the pressing process, the initial blade 100 is subjected to a cooling treatment. When the temperature around the initial blade 100 is not greater than 100° C. and the pressing time is not less than 60 minutes, the pressing operation is completed to obtain a finished blade.
[0074] During the molding process, the pressure holding time is required to be no less than 60 minutes to ensure that the initial blade 100 can be fully shaped. The molding operation can only be completed when the temperature around the initial blade 100 drops to 100°C to avoid large deformation of the initial blade 100 after high temperature and pressure loss. During the molding process, the initial blade 100 is cooled by air, and / or the molding jig is cooled by water. During the pressure holding process, the initial blade 100 can be cooled by air, such as using air conditioning, electric fans, etc. to cool the initial blade 100 and the molding jig; at the same time, the molding jig can be cooled by water, including using circulating water to cool the molding jig, and spraying water mist on the molding jig to achieve cooling of the molding jig, thereby achieving rapid cooling of the initial blade 100, so as to achieve rapid shaping of the initial blade 100.
[0075] It is worth noting that the present application adopts the method of heating in a heating furnace and then transferring to the mold. Compared with the solution of heating in the mold, firstly, it reduces the complexity of the mold and avoids the problem of difficult heating; secondly, it avoids the problem of uneven heating in the mold; thirdly, excessive heating temperature on the mold may cause deformation of the mold line; finally, heating on the mold causes the temperature of the mold to rise, resulting in energy waste and is not conducive to cooling during the molding process.
[0076] In addition, the profiling steps of the above two methods can be performed multiple times. For example, in the first method, steps S1-2 to S1-4 can be repeated, and in the second method, steps S2-2 to S2-5 can be repeated to achieve multiple profiling of the blades, but the number of profiling times should not exceed three times.
[0077] like Figure 3 As shown, the embodiment of the present invention also provides another method, including:
[0078] S3-1, obtaining raw materials, and processing the raw materials using a blade expansion template to obtain an initial blade 100.
[0079] S3-2, performing a preheating treatment on the initial blade 100 for a first preset time.
[0080] S3-3, within the second preset time, the initial blade 100 after the preheating treatment is installed on the molding jig.
[0081] S3-4, using a molding die to mold the initial blade 100 to obtain a finished blade.
[0082] S3-5. After the third preset time, the finished blades are inspected.
[0083] The third preset time is not less than 24 hours. The inspection of the finished blades should be carried out 24 hours after the blades are pressed to ensure that the blades are fully deformed after pressing.
[0084] There may be many ways to inspect the finished blades. For example, in one embodiment, the steps of inspecting the finished blades specifically include:
[0085] S3-5-1. Perform a three-dimensional scan on the finished blade to obtain actual three-dimensional image information of the finished blade.
[0086] It can be realized by using any existing equipment and software with three-dimensional scanning function, such as using a three-dimensional scanner to detect and analyze the blades and perform three-dimensional reconstruction calculations to create a digital model of the actual blade in the virtual world.
[0087] S3-5-2. Obtain theoretical three-dimensional image information corresponding to the finished blade.
[0088] That is, the three-dimensional digital information of the design data corresponding to the finished blade.
[0089] S3-5-3. Compare the actual three-dimensional image information with the theoretical three-dimensional image information, and determine the accuracy of the finished blade according to the image deviation result.
[0090] Point-by-point comparison and surface analysis can be performed to detect molding deviations. In the case of free comparison, the actual 3D image information is compared with the theoretical 3D image information. If the maximum deviation is less than or equal to 1mm, it is excellent; if the maximum deviation is less than or equal to 1.5mm, it is good; if the maximum deviation is less than or equal to 2mm, it is qualified; if the maximum deviation is less than or equal to 2mm, it needs to be eliminated.
[0091] In another embodiment, when there is no three-dimensional scanning measurement of the blade, the blade accuracy can be measured using a feeler gauge. The steps of testing the finished blade specifically include:
[0092] S3-5-4, re-place the finished blade on the lower mold 601 of the molding mold, and adjust the finished blade so that there is no gap between the blade inlet end 101 and the blade-shaft disc welding end 102 and the positioning pin 701 of the molding mold. Use a 0.1 mm feeler gauge to try to enter between the blade inlet end 101 and the blade-shaft disc welding end 102 and the positioning pin 701. If it cannot enter, it can be considered as no gap.
[0093] S3-5-5. Use a feeler gauge to measure the gap between each test point on the finished blade and the lower mold 601, and record the data to form data one.
[0094] Use a feeler gauge to measure the gap between the finished blade and the lower mold 601, such as Fig.11 As shown, as many test points as possible are selected in the test area 103, such as 50 points, 80 points, etc. evenly distributed in the test area 103. The data refers to the thickness of the largest feeler gauge that can be inserted into the test points.
[0095] S3-5-6, re-place the finished blade on the upper mold 602 of the molding mold, and adjust the finished blade so that there is no gap between the blade inlet end 101 and the blade-shaft disc welding end 102 and the positioning pin 701 of the molding mold. Use a 0.1 mm feeler gauge to try to enter between the blade inlet end 101 and the blade-shaft disc welding end 102 and the positioning pin 701. If it cannot enter, it can be considered as no gap.
[0096] S3-5-7. Use a feeler gauge to measure the gap between each test point on the finished blade and the upper mold 602, and record the data to form data 2.
[0097] It can be understood that the test point in this step and the test point in step S3-5-5 are located at the same position in the finished blade test area 103.
[0098] S3-5-8. Determine the accuracy of the finished blade based on data 2 and data 1.
[0099] For data 1 and data 2 corresponding to all test points, if they are all less than or equal to 1mm, they are excellent; if they are all less than or equal to 1.5mm, they are good; if they are all less than or equal to 2mm, they are qualified. If they are greater than 2mm, they are considered to be discarded.
[0100] In addition, before S3-5-8, the step of determining the accuracy of the finished blade according to data 2 and data 1, it also includes judging whether data 2 and data 1 have opposite trends. If so, it proves that the measured data is accurate data, otherwise, re-measure. When data 1 and data 2, when the finished blade rebounds, their shape errors relative to the upper mold and the lower mold should be exactly opposite. If one of the detection points is used as the current detection point, data 1 includes an increasing trend in the direction close to the current detection point, and for data 2, it should be that data 2 includes a decreasing trend in the direction close to the current detection point. The data change trend can be analyzed for any detection point, and then it can be determined whether the measurement data is reliable. For example, the detection data corresponding to the detection points numbered 1 to 6 in data one are 0.1mm, 0.5mm, 0.8mm, 1.2mm, 0.8mm, and 0mm, and the detection data corresponding to the detection points numbered 1 to 6 in data two are 1.2mm, 0.5mm, 0.1mm, 0mm, 0.2mm, and 1.4mm. It can be seen that if the detection point numbered 4 is taken as the current detection point, data one includes an increasing trend in the direction close to the current detection point, and data two includes a decreasing trend in the direction close to the current detection point, which meets the characteristics of opposite trends and the data is reliable.
[0101] Before the step of S3-5-8, determining the accuracy of the finished blade according to data 2 and data 1, it also includes judging whether the sum of data 2 and data 1 of each detection point is consistent. If so, it proves that the measured data is accurate data, otherwise, re-measure. At the same point measurement of the finished blade, the sum of data 2 and data 1 should be the same. If the finished blade rebounds elastically, data 2 will increase while data 1 will decrease, or data 2 will decrease while data 1 will increase. Then, it can be determined whether the measured data is reliable by judging whether the sum of data 2 and data 1 of each detection point is consistent or tends to be consistent. As in the embodiment of the detection data of the detection points numbered 1 to 6 above, the sum of data 1 and data 2 is 1.3mm, 1mm, 0.9mm, 1.2mm, 1mm, 1.4mm, and the error difference is 0.5mm. The error is large, and this group of data can be regarded as unreliable and needs to be re-measured.
[0102] The above two methods for testing finished blades can be used simultaneously, such as combining three-dimensional testing with feeler gauge measurement. The above two methods for verifying whether the data is reliable can be used in a superimposed manner.
[0103] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A high-precision manufacturing method for large-sized three-dimensional blades, characterized in that: include: Obtaining raw materials, and processing the raw materials using a blade development template to obtain initial blades; Performing a preheating treatment on the initial blade for a first preset time; Within a second preset time, the initial blade after preheating is mounted on a molding die; The initial blade is pressed by the pressing mold to obtain a finished blade.
2. The manufacturing method according to claim 1, characterized in that: The step of preheating the initial blade for a first preset time is specifically: Using a heating furnace to heat the initial blade to a temperature not lower than a preset minimum temperature, and heating the initial blade for a first preset time starting from when the furnace temperature of the heating furnace reaches the preset minimum temperature; The first preset time is not less than 90 minutes and not more than 120 minutes, and the preset minimum temperature is not less than 1050°C.
3. The manufacturing method according to claim 1, characterized in that: The second preset time is no more than 90 seconds.
4. The manufacturing method according to claim 1, characterized in that: The step of installing the preheated initial blade on the molding die within the second preset time is specifically as follows: Perform the following operations within the second preset time: The initial blade is placed on the molding jig, and the blade inlet end of the initial blade and the welding end of the blade and the shaft disc are adjusted to have no gap with the positioning pin of the molding jig.
5. The manufacturing method according to claim 1, characterized in that: Between the step of using the profiling jig to profil the initial blade to obtain a finished blade, the method further comprises: If the time for installing the preheated initial blade on the molding jig exceeds 180 seconds, the initial blade is preheated again for a first preset time.
6. The manufacturing method according to claim 1, characterized in that: The step of using the profiling jig to profil the initial blade to obtain a finished blade specifically includes: The initial blade is pressed by using the pressing jig, wherein the tonnage of the press connected to the pressing jig is not less than 600 tons; During the profiling process, a feeler gauge is used to try to enter between the initial blade and the positioning pin at a preset time interval. If the feeler gauge larger than the preset size can enter, the initial blade is preheated again for a first preset time, and the preset size is not greater than 1 mm. During the profiling process, the initial blade is subjected to a cooling treatment; When the temperature around the initial blade is not higher than 100° C. and the pressing time is not less than 60 minutes, the pressing operation is completed to obtain the finished blade.
7. The manufacturing method according to claim 6, characterized in that: The step of cooling the initial blade during the profiling process is specifically as follows: The initial blades are subjected to air cooling, and / or the molding mold is subjected to water cooling.
8. The manufacturing method according to any one of claims 1 to 7, characterized in that: After the step of using the profiling jig to profile the initial blade to obtain a finished blade, the method further comprises: After a third preset time, inspecting the finished blade; The third preset time is not less than 24 hours.
9. The manufacturing method according to any one of claims 8, characterized in that: The step of testing the finished blades specifically includes: Performing a three-dimensional scan on the finished blade to obtain actual three-dimensional image information of the finished blade; Acquiring theoretical three-dimensional image information corresponding to the finished blade; The actual three-dimensional image information is compared with the theoretical three-dimensional image information, and the accuracy of the finished blade is determined according to the image deviation result.
10. The manufacturing method according to any one of claims 8, characterized in that: The step of testing the finished blades specifically includes: Placing the finished blade on the lower mold of the molding jig, and adjusting the blade inlet end of the finished blade and the welding end of the blade and the shaft disc to have no gap with the positioning pin of the molding jig; Use a feeler gauge to measure the gap between each test point on the finished blade and the lower mold, and record the data to form data 1; Placing the finished blade on the upper mold of the molding jig, and adjusting the blade inlet end of the finished blade and the welding end of the blade and the shaft disc to have no gap with the positioning pin of the molding jig; Using the feeler gauge to measure the gap between each test point on the finished blade and the upper mold, and recording the data to form data 2; The accuracy of the finished blade is determined based on the data 2 and the data 1.
Citation Information
Patent Citations
Compressor impeller three-dimensional flow large blade profiling tool with guide blade structure and method
CN114939622A
Method and device for forming blades in three-body welded impeller
CN116809745A
Hot-pressing machining method for marine propeller
CN117920830A
Sintering fan three -dimensional flow blade die mould frock
CN208680336U