Water washing method and device for sodium-reduced tantalum powder

By prioritizing the use of acidic wastewater and pure water to replace organic acids during the tantalum powder washing process, the problems of large consumption of pure water and waste of organic acids during the tantalum powder washing process are solved, and efficient tantalum powder yield and low impurity content are achieved, reducing the Production cost.

CN119016720APending Publication Date: 2024-11-26CONGHUA TANTALUM & NIOBIUM SMELTERY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411160951.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The pure water consumption during the washing of existing tantalum powder is large, and additional organic acids are required, resulting in low recovery rate, increasing environmental pressure and treatment cost. The tantalum powder settles for a long time, low yield, and too long production process.

Method used

A water washing method for sodium reducing tantalum powder is used. After crushing the sodium reducing product, it is first washed with acidic wastewater, and then gradually replaced with cold pure water and hot pure water. Finally, it is carried out to pickle and clean acid operations, and bake with pure water. Dry, collect and recycle acidic wastewater, reduce pure water consumption and improve tantalum powder yield.

Benefits of technology

It saves pure water consumption, improves tantalum powder yield and product quality, reduces impurity content and production costs, and simplifies production processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016720A_ABST
    Figure CN119016720A_ABST
Patent Text Reader

Abstract

The invention relates to a washing method for sodium-reduced tantalum powder. The washing method comprises the following steps: S1, crushing a sodium reduction product; S2, cleaning a material by using acidic wastewater; S3, cleaning the material by using cold pure water, S4, cleaning the material by using hot pure water, S6, carrying out acid washing on the material, S7, recovering the acidic wastewater, and S8, carrying out acid washing and drying. The washing method has the beneficial effects that the acid wastewater is preferentially used for washing the material, so that the consumption of pure water can be saved, and meanwhile, extra organic acid does not need to be consumed; in addition, waiting for sedimentation of the tantalum powder is not needed, the yield of the tantalum powder raw powder obtained through washing operation with the method is higher, the impurity content is lower, the product quality is improved, and meanwhile the cost is saved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of tantalum powder manufacturing, and in particular to a method and device for washing tantalum powder reduced with sodium. Background Art

[0002] Tantalum is a rare metal with a high melting point and a special functional material with excellent performance. It is widely used in high-end technology fields such as communications, computers, automotive electronics, missiles, aerospace, and automatic control devices.

[0003] The method for reducing potassium fluorotantalate has the following reaction equation: K 2 Tf 7 +5Na=Ta+5NaF+2KF. This reaction usually uses one or more metal halides such as NaCl, KCl, KF as diluent salts: one is to lower the melting point of the molten salt, balance the reaction heat, control the heating rate and reaction rate, and promote the reaction to improve the particle size, particle shape and other electrical properties of the tantalum powder; the other is to increase the solubility of metallic sodium in the molten salt system, which is conducive to the complete reduction of potassium fluorotantalate. In addition, in order to ensure that the reaction is thorough, an excess of metallic sodium needs to be added. The above reaction products are usually subjected to wet purification by crushing them, washing with water to remove residual metallic sodium, unreduced potassium fluorotantalate, reaction by-products potassium fluoride and sodium fluoride, and the added diluent. The impurities such as iron, nickel, and chromium that are corroded by the equipment and mechanically entrained are removed by acid washing, while reducing the oxygen content.

[0004] During the water washing process, metallic sodium reacts with water:

[0005] 2Na+2H 2 O=2NaOH+H 2 ↑, in a strong alkaline solution, tantalum powder reacts with sodium hydroxide as follows: 2Ta+2NaOH+4H 2 O=2NaTaO 3 ↓+5H 2 ↑. The following two methods are usually used to wash the sodium reduction product: one method is to directly use a stirring and washing machine to wash the reduction product at high speed; the other method is to filter and wash the reduction product without stirring. In the first method, the tantalum powder particles are stirred at high speed in the stirring and washing tank. The tantalum powder particles hit the container wall or baffle during high-speed movement and are strongly squeezed, which will cause loss of specific surface area. In addition, this method has a long sedimentation time and as the specific surface area of ​​tantalum powder increases, the particle size of tantalum powder becomes finer and the sedimentation time is longer or it is difficult to settle, resulting in serious loss of tantalum powder, reduced tantalum powder yield, and extended production cycle. In the second method, tantalum powder reacts with strong alkali to form tantalate, which is deposited on the surface of tantalum powder and filter cloth, making water washing difficult and the water washing efficiency low.

[0006] Chinese patent CN102990076 B introduces a stirring water washing method and device for producing tantalum powder by reducing potassium fluorotantalate with metallic sodium, and Chinese patent CN 102191389 B introduces a water washing method for a product of potassium fluorotantalate reduced with sodium. Both require the addition of inorganic acid during water washing, which causes waste of inorganic acid and the acidic wastewater generated cannot be reused, increasing environmental pressure and processing costs. Tantalum powder has a long sedimentation time. As the specific surface area of ​​tantalum powder increases, the particle size of tantalum powder becomes finer and finer, and the sedimentation time is longer or it is difficult to settle. The yield is low and the production process is too long, which is not conducive to reducing production costs. Summary of the invention

[0007] The purpose of the present invention is to overcome the problems of large pure water consumption, the need for additional addition of organic acid and low recovery rate in the water washing process in the prior art, and to provide a sodium reduced tantalum powder water washing method and a sodium reduced tantalum powder water washing device.

[0008] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:

[0009] A method for washing sodium-reduced tantalum powder, comprising the following steps:

[0010] S1. Crushing the sodium reduction product: crushing the sodium reduction product into materials with a particle size of less than 2 cm using a jaw crusher, and then adding the materials into a water washing tank;

[0011] S2. Wash the material with acidic wastewater: add the acidic wastewater in the high-level return water tank into the water washing tank. When the material in the water washing tank is completely submerged by the acidic wastewater, blow compressed air into the water washing tank to agitate and stir the material. After the compressed air is passed for T minutes, filter the water washing tank to separate the cleaning liquid from the material.

[0012] S3, washing the material with cold pure water: repeat step S2 until the pH of the cleaning liquid filtered out of the washing tank is 8±0.2, stop using acidic wastewater to wash the material, add cold pure water to the washing tank to wash the material, and stop washing with cold pure water when the pH of the cleaning liquid is 7±0.2;

[0013] S4. Wash the material with hot pure water: Add hot pure water into the water washing tank to wash the material until the conductivity of the cleaning liquid discharged from the water washing tank is ≤20us / cm, and stop washing with hot pure water;

[0014] S6. Pickling the material: transfer the material from the water washing tank to the pickling barrel, and pickle the material with mixed acid;

[0015] S7. Recycling acidic wastewater: After the pickling is completed, the material is transferred from the pickling barrel to the water washing tank, and the material is washed with pure water twice, and the acidic wastewater generated by the two acid washings is collected in the recovery tank;

[0016] S8, acid washing and drying: continue to use pure water to wash the material with acid until the conductivity of the acid washing solution discharged from the water washing tank is ≤5us / cm, then stop acid washing, transfer the material from the water washing tank to a vacuum drying box for drying, and sieve the dried material to obtain tantalum powder.

[0017] Wherein, the weight ratio of the material in S2 to the acidic wastewater is 1:5-50.

[0018] The time T for introducing compressed air in S2 is 2-15 minutes.

[0019] Wherein, the mass ratio of the material to the mixed acid during pickling in S6 is 1:0.5-5.

[0020] The mixed acid in S6 is prepared by mixing nitric acid with a concentration of 10-15% and hydrofluoric acid with a concentration of 0.1-1% in a volume ratio of 1:1.

[0021] A sodium-reduced tantalum powder washing device is provided for use in the sodium-reduced tantalum powder washing method, comprising a washing tank for washing materials and acid washing, a recovery tank for collecting acid washing wastewater, a high-level return water tank for storing acid wastewater, a high-level cold pure water tank for storing cold pure water, and a high-level hot pure water tank for storing hot pure water. The recovery tank is connected to the high-level return water tank through a conveying pipeline equipped with a lift pump. A compressed air pipe, a suction filter pipe, and a liquid adding main pipe are arranged at the bottom of the washing tank. The high-level return water tank, the high-level cold pure water tank, and the high-level hot pure water tank are respectively connected to the liquid adding main pipe through liquid adding branches equipped with electric valves.

[0022] Wherein, the compressed air pipe is connected to an air compressor, the suction filter pipe is connected to a suction filter, and the discharge port of the suction filter is connected to the recovery tank through a pipeline.

[0023] The water washing tank is made of stainless steel, and a filter plate is arranged in the water washing tank, and the filter plate separates the water washing tank into a cleaning area and a drainage area.

[0024] Wherein, the recovery tank, the high-position return water tank, the high-position cold pure water tank and the high-position hot pure water tank are all made of PVC material.

[0025] The beneficial effects of the present invention are:

[0026] The sodium reduction tantalum powder washing method uses acidic wastewater to wash the material, which can save the consumption of pure water. At the same time, no additional organic acid needs to be added during washing. There is no need to wait for the tantalum powder to settle. The tantalum powder obtained by the washing operation using this method has a higher yield and a lower impurity content, which improves product quality while saving costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of this application. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0028] Figure 1 It is a schematic structural diagram of a sodium-reduced tantalum powder washing device in the present invention;

[0029] Description of the numbers in the figure:

[0030] Water washing tank 1, compressed air pipe 101, suction filter pipe 102, liquid adding main pipe 103, recovery tank 2, high-level return water tank 3, high-level cold pure water tank 4, high-level hot pure water tank 5, lift pump 6, liquid adding branch pipe 7, air compressor 8, suction filter 9. DETAILED DESCRIPTION

[0031] The present invention will be described in detail below with reference to the accompanying drawings and in combination with embodiments.

[0032] like Figure 1 As shown, a sodium reduced tantalum powder washing device for a sodium reduced tantalum powder washing method comprises a washing tank 1 for washing materials and acid washing operations, a recovery tank 2 for collecting acid washing waste water, a high-level return water tank 3 for storing acid waste water, a high-level cold pure water tank 4 for storing cold pure water, and a high-level hot pure water tank 5 for storing hot pure water. The recovery tank 2 is connected to the high-level return water tank 3 through a conveying pipeline equipped with a lift pump 6, and a compressed air pipe 101, a suction filter pipe 102, and a liquid adding main pipe 103 are arranged at the bottom of the washing tank 1. The high-level return water tank 3, the high-level cold pure water tank 4, and the high-level hot pure water tank 5 are respectively connected to the liquid adding main pipe 13 through a liquid adding branch pipe 7 equipped with an electric valve. The compressed air pipe 101 is connected to an air compressor 8, and the suction filter pipe is connected to a suction filter 9. The discharge port of the suction filter 9 is connected to the recovery tank 2 through a pipeline.

[0033] The water washing tank 1 is made of stainless steel. A filter plate is arranged in the water washing tank 1. The filter plate separates the water washing tank into a washing area and a drainage area.

[0034] The recovery tank 2, the high-level return water tank 3, the high-level cold pure water tank 4 and the high-level hot pure water tank 5 are all made of PVC material.

[0035] A method for washing sodium-reduced tantalum powder, comprising the following steps:

[0036] S1. Crushing the sodium reduction product: crush the sodium reduction product into materials with a particle size less than 2 cm using a jaw crusher, and then add the materials into a water washing tank.

[0037] S2. Wash the material with acidic wastewater: add the acidic wastewater in the high-level return water tank into the water washing tank. When the material in the water washing tank is completely submerged by the acidic wastewater, the weight ratio of the material to the acidic wastewater is 1:5-50. Blow compressed air into the water washing tank to agitate and stir the material. After the compressed air is introduced for 2-15 minutes, the water washing tank is filtered to separate the cleaning liquid from the material.

[0038] S3. Wash the material with cold pure water: Repeat step S2 until the pH of the cleaning liquid filtered out of the washing tank is 8±0.2, stop using acidic waste water to wash the material, add cold pure water to the washing tank to wash the material, and stop washing with cold pure water until the pH of the cleaning liquid is 7±0.2.

[0039] S4. Wash the material with hot pure water: Add hot pure water into the water washing tank to wash the material until the conductivity of the cleaning liquid discharged from the water washing tank is ≤20us / cm, then stop washing with hot pure water.

[0040] S6. Pickling the material: transfer the material from the water washing tank to the pickling barrel, and use mixed acid to pickle the material. The mass ratio of the material to the mixed acid during pickling is 1:0.5-5; wherein the mixed acid is a mixture of nitric acid with a concentration of 10-15% and hydrofluoric acid with a concentration of 0.1-1% in a volume ratio of 1:1.

[0041] S7. Recycling of acidic wastewater: After the pickling is completed, the material is transferred from the pickling barrel to the water washing tank, and the material is washed with pure water twice, and the acidic wastewater generated by the two acid washings is collected in the recovery tank.

[0042] S8, acid washing and drying: continue to use pure water to wash the material with acid until the conductivity of the acid washing solution discharged from the water washing tank is ≤5us / cm, then stop acid washing, transfer the material from the water washing tank to a vacuum drying box for drying, and sieve the dried material to obtain tantalum powder.

[0043] Embodiment 1

[0044] A method for washing sodium-reduced tantalum powder, comprising the following steps:

[0045] S1. Crushing the sodium reduction product: crush the sodium reduction product into materials with a particle size of 1±0.2 cm using a jaw crusher, and then add the materials into a water washing tank.

[0046] S2. Wash the material with acidic wastewater: add the acidic wastewater in the high-level return water tank into the water washing tank. When the material in the water washing tank is completely submerged by the acidic wastewater, the weight ratio of the material to the acidic wastewater is 1:20. Blow compressed air into the water washing tank to agitate and stir the material. After the compressed air is introduced for 2-15 minutes, filter the water washing tank to separate the cleaning liquid from the material.

[0047] S3. Wash the material with cold pure water: Repeat step S2 until the pH of the cleaning liquid filtered out of the washing tank is 8±0.2, stop using acidic waste water to wash the material, add cold pure water to the washing tank to wash the material, and stop washing with cold pure water until the pH of the cleaning liquid is 7±0.2.

[0048] S4. Wash the material with hot pure water: Add hot pure water into the water washing tank to wash the material until the conductivity of the cleaning liquid discharged from the water washing tank is ≤20us / cm, then stop washing with hot pure water.

[0049] S6. Pickling the material: transfer the material from the washing tank to the pickling barrel, and use mixed acid to pickle the material. The mass ratio of the material to the mixed acid during pickling is 1:1; wherein the mixed acid is a mixture of nitric acid with a concentration of 10-15% and hydrofluoric acid with a concentration of 0.1-1% in a volume ratio of 1:1.

[0050] S7. Recycling of acidic wastewater: After the pickling is completed, the material is transferred from the pickling barrel to the water washing tank, and the material is washed with pure water twice, and the acidic wastewater generated by the two acid washings is collected in the recovery tank.

[0051] S8, acid washing and drying: continue to use pure water to wash the material with acid until the conductivity of the acid washing solution discharged from the water washing tank is ≤5us / cm, then stop acid washing, transfer the material from the water washing tank to a vacuum drying box for drying, and sieve the dried material to obtain tantalum powder 1.

[0052] Comparative Example 1

[0053] A method for washing sodium-reduced tantalum powder, comprising the following steps:

[0054] S1. Crushing the sodium reduction product: crush the sodium reduction product into materials with a particle size less than 2 cm using a jaw crusher, and then add the materials into a water washing tank.

[0055] S2. Wash the material with cold pure water: Add cold pure water into the water washing tank to wash the material until the pH of the washing liquid is 7±0.2, then stop washing with cold pure water.

[0056] S3. Wash the material with hot pure water: Add hot pure water into the water washing tank to wash the material until the conductivity of the cleaning liquid discharged from the water washing tank is ≤20us / cm, then stop washing with hot pure water.

[0057] S4. Pickling the material: transfer the material from the washing tank to the pickling barrel, and use mixed acid to pickle the material. The mass ratio of the material to the mixed acid during pickling is 1:1; wherein the mixed acid is a mixture of nitric acid with a concentration of 10-15% and hydrofluoric acid with a concentration of 0.1-1% in a volume ratio of 1:1.

[0058] S5. Acid washing and drying: After the acid washing is completed, the material is transferred from the acid washing barrel to the water washing tank, and the material is washed with pure water until the conductivity of the acid washing solution discharged from the water washing tank is ≤5us / cm. The acid washing is stopped, and the material is transferred from the water washing tank to a vacuum drying box for drying. The dried material is sieved to obtain tantalum powder II.

[0059] The tantalum powder yield and pure water consumption in Example 1 and Example 2 were calculated, and the impurity content of the tantalum powder 1 obtained in Example 1 and the tantalum powder 2 obtained in Comparative Example 1 was tested. The results are shown in Table 1 below.

[0060] Table 1. Tantalum powder yield, pure water consumption and impurity content test results

[0061]

[0062] It can be seen from Table 1 that the tantalum powder yield of Example 1 is higher than that of Comparative Example 1, the pure water consumption of Example 1 is less than that of Comparative Example 1, and the impurity content of the tantalum powder 1 obtained in Example 1 is lower than that of the tantalum powder 2 obtained in Comparative Example 1. Therefore, the method of Example 1 is used to preferentially use acidic waste water to wash the material, which can save the consumption of pure water and does not require the consumption of additional organic acid. The tantalum powder obtained by the washing operation using this method has a higher yield and a lower impurity content, which improves product quality while saving costs and has good economic benefits.

[0063] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.

Claims

1. A method for washing sodium-reduced tantalum powder, characterized in that: The following steps are involved: S1. Crushing the sodium reduction product: crushing the sodium reduction product into materials with a particle size of less than 2 cm using a jaw crusher, and then adding the materials into a water washing tank; S2. Wash the material with acidic wastewater: add the acidic wastewater in the high-level return water tank into the water washing tank. When the material in the water washing tank is completely submerged by the acidic wastewater, blow compressed air into the water washing tank to agitate and stir the material. After the compressed air is passed for T minutes, filter the water washing tank to separate the cleaning liquid from the material. S3, washing the material with cold pure water: repeat step S2 until the pH of the cleaning liquid filtered out of the washing tank is 8±0.2, stop using acidic wastewater to wash the material, add cold pure water to the washing tank to wash the material, and stop washing with cold pure water when the pH of the cleaning liquid is 7±0.2; S4. Wash the material with hot pure water: Add hot pure water into the water washing tank to wash the material until the conductivity of the cleaning liquid discharged from the water washing tank is ≤20us / cm, and stop washing with hot pure water; S6. Pickling the material: transfer the material from the water washing tank to the pickling barrel, and pickle the material with mixed acid; S7. Recycling acidic wastewater: After the pickling is completed, the material is transferred from the pickling barrel to the water washing tank, and the material is washed with pure water twice, and the acidic wastewater generated by the two acid washings is collected in the recovery tank; S8, acid washing and drying: continue to use pure water to wash the material with acid until the conductivity of the acid washing solution discharged from the water washing tank is ≤5us / cm, then stop acid washing, transfer the material from the water washing tank to a vacuum drying box for drying, and sieve the dried material to obtain tantalum powder.

2. The method for washing tantalum powder reduced with sodium according to claim 1, characterized in that: The weight ratio of the material in S2 to the acidic wastewater is 1:5-50.

3. The method for washing tantalum powder reduced with sodium according to claim 1, characterized in that: The time T for introducing compressed air in S2 is 2-15 minutes.

4. The method for washing tantalum powder reduced with sodium according to claim 1, characterized in that: The mass ratio of the material to the mixed acid during pickling in S6 is 1:0.5-5.

5. The method for washing sodium-reduced tantalum powder according to claim 1, characterized in that: The mixed acid in S6 is prepared by mixing nitric acid with a concentration of 10-15% and hydrofluoric acid with a concentration of 0.1-1% in a volume ratio of 1:

1.

6. A sodium-reduced tantalum powder washing device for use in the sodium-reduced tantalum powder washing method according to any one of claims 1 to 5, characterized in that: It includes a water washing tank for material washing and acid washing, a recovery tank for collecting acid washing wastewater, a high-level return water tank for storing acidic wastewater, a high-level cold pure water tank for storing cold pure water, and a high-level hot pure water tank for storing hot pure water. The recovery tank is connected to the high-level return water tank through a conveying pipeline equipped with a lift pump. A compressed air pipe, a suction filter pipe, and a liquid adding main pipe are arranged at the bottom of the water washing tank. The high-level return water tank, the high-level cold pure water tank, and the high-level hot pure water tank are respectively connected to the liquid adding main pipe through liquid adding branches equipped with electric valves.

7. The sodium-reduced tantalum powder washing device according to claim 6, characterized in that: The compressed air pipe is connected to an air compressor, the suction filter pipe is connected to a suction filter, and the discharge port of the suction filter is connected to the recovery tank through a pipeline.

8. The sodium-reduced tantalum powder washing device according to claim 6, characterized in that: The water washing tank is made of stainless steel and is provided with a filter plate in the water washing tank. The filter plate separates the water washing tank into a cleaning area and a drainage area.

9. The sodium-reduced tantalum powder washing device according to claim 6, characterized in that: The recovery tank, the high-level return water tank, the high-level cold pure water tank and the high-level hot pure water tank are all made of PVC material.