High-dispersity superfine carbon-coated copper powder for photovoltaic cells and preparation method of high-dispersity superfine carbon-coated copper powder
By using thermally decomposed copper compounds for in situ carbon deposition coating under vacuum environment, combining volatile carbon sources and low-cost copper sources, the uniformity and cost control problems of carbon-covered copper powders in the preparation process are solved. , the ultrafine carbon coated copper powder with high dispersion and fine particle size is achieved, which is suitable for industrial large-scale production, and the performance of graphene coated copper powder is improved through graphitization treatment.
Patent Information
- Application Number
- CN202411142622.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-26
AI Technical Summary
The existing carbon-covered copper powders have problems such as uniformity, integrity, dispersion, particle size controllability and cost control during the preparation process, and the process is complex and not suitable for mass production, resulting in insufficient conductivity and oxidation resistance.
In a vacuum environment, the thermally decomposed copper compound is used as a copper source and immediately after decomposition. The carbon source is excited by a low-temperature excitation zone and transported to the reaction zone through carrier gas, simplifying the process flow and reducing energy To consume, select volatile carbon sources such as acetic acid and low-cost copper sources such as copper oxalate, and control reaction conditions such as temperature and vacuum to achieve high dispersion and fine-grained carbon coating.
Ultrafine carbon-coated copper powder with high dispersion, fine particle size, complete carbon coating and good oxidation resistance are obtained, which is suitable for industrial large-scale production, and the performance of graphene-coated copper powder is further improved through graphitization treatment.
Smart Images

Figure CN119016722A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a carbon-copper composite material, in particular to a carbon-coated copper powder and a preparation method thereof, and belongs to the technical field of electronic paste and photovoltaic cell industry. Background Art
[0002] As a renewable energy source, the photovoltaic cell industry is in a stage of sustained growth and has broad development prospects. The photovoltaic cell manufacturing process is inseparable from electronic paste with high conductivity. Traditional electronic paste uses pure silver. Silver has good conductivity, stability and thermal conductivity, but it is expensive and has high electrical mobility. The price of copper is relatively low, and its conductivity and thermal conductivity are second only to and close to silver. It is the most preferred metal as a low-cost substitute for silver. However, copper powder, especially ultrafine copper powder, is easily oxidized in the air, and its conductivity drops significantly after oxidation. In order to solve the problems of high cost of silver powder and easy oxidation of copper powder, the photovoltaic industry began to use silver-coated copper powder as raw material to prepare electronic paste. In addition, conductive, electromagnetic shielding and other products in the fields of electromechanical, communications, printing, aerospace, weapons, etc. also have a large demand for electronic paste.
[0003] Although silver-coated copper powder reduces the amount of silver used, it still uses silver as one of the raw materials. At present, the main processes for silver-coated copper powder include replacement method, chemical reduction method, ball milling method, chemical plating method, etc. Although each has its own advantages, they all face problems such as complex process flow, low output, unstable quality, and high cost. In short, silver-coated copper powder reduces the cost of electronic paste to a certain extent, but the degree of reduction is limited.
[0004] Carbon materials are stable, lightweight, and can be coated on the surface of copper powder in the form of an extremely thin shell, effectively isolating copper powder from oxygen in the air to prevent copper from being oxidized. In particular, graphene, as a new type of two-dimensional thin film carbon material, has performance far exceeding copper-based materials in terms of electrical conductivity, thermal conductivity, and mechanics, with high electrical conductivity (200mS / m) and high thermal conductivity at room temperature, and high strength. At present, there have also been some studies on carbon-coated copper or graphene-coated copper, such as Chinese patent CN110385432A discloses a method for preparing graphene / copper powder using fluidized bed as a reaction device and gas-phase carbon source as a reaction raw material, and this method requires expensive nano-scale copper powder as raw material powder to obtain a finer coating, which greatly increases the cost of graphene-coated copper powder. In order to prevent copper powder from bonding and growing together during carbon coating, equipment such as fluidized bed is needed, and equipment requirements are high and not suitable for mass production. Even in the dynamic environment of fluidized bed, it is still impossible to completely suppress the adhesion growth between copper powders, and the final coating powder is still micron-grade powder. In addition, this method uses a gas-phase carbon source, which, on the one hand, limits the types of carbon sources, and on the other hand, requires the cracking of the gas-phase carbon source at high temperature, resulting in high energy consumption for coating.
[0005] Therefore, the uniformity and integrity of carbon-coated copper powder, the dispersibility and particle size controllability of carbon-coated copper powder, the controllability of carbon layer thickness, the feasibility of mass production of carbon-coated copper process, process complexity and cost controllability are the problems that need to be urgently solved in carbon-coated copper powder. Summary of the invention
[0006] In view of the shortcomings of the prior art, the first object of the present invention is to provide a highly dispersible ultrafine carbon-coated copper powder. The carbon-coated copper powder has the advantages of good dispersibility, uniform particle size distribution, complete carbon coating, good oxidation resistance, high carbon order and good conductivity.
[0007] The second object of the present invention is to provide a method for preparing highly dispersed ultrafine carbon-coated copper powder using low-cost carbon source and copper source as raw materials. The method is simple, has a short process flow, low equipment requirements, low cost, and is suitable for industrial-scale production.
[0008] The third object of the present invention is to provide a graphene-coated copper powder, which has a high degree of graphitization and a small particle size.
[0009] In order to achieve the above technical objectives, the present invention provides a method for preparing highly dispersed ultrafine carbon-coated copper powder, which is obtained by exciting a carbon source in an excitation zone under a vacuum environment and then transporting it to a reaction zone via a carrier gas and depositing and coating it on copper powder; the copper powder is obtained by decomposing a thermally decomposable copper source in a reaction zone or reducing it after decomposition.
[0010] The key to the technical solution of the present invention is to select a thermally decomposable copper compound as the copper source, so that once the copper compound is decomposed or decomposed and reduced to copper in the reaction zone, in-situ carbon deposition and coating can be immediately carried out, so that the deposited carbon isolation between the copper powders is obtained, the bonding and growth between the powders are avoided, and the high dispersibility and fine particle size of the powders can be guaranteed without the need for complex equipment requirements. At the same time, the gaps between the highly dispersible and unbonded powders are sufficient, so that the atmosphere containing the carbon source can be fully in contact with the powders, and the uniformity and integrity of the carbon coating can be guaranteed. In addition, the method of using a thermally decomposable copper source to decompose in the reaction zone has no strict requirements on the particle size of the copper source, which simplifies the process and reduces the production cost. Finally, the carbon source of the present invention is excited in the excitation zone of the lower temperature zone and then transported to the reaction zone by a carrier gas, which can realize carbon deposition on the highly active copper surface at a lower deposition temperature and a shorter deposition time, greatly reducing energy consumption. The carbon deposition coating process is carried out under low vacuum and flowing atmosphere, and only a first-stage rotary vane pump is used for vacuuming. The experimental equipment is simple, which ensures the activity of the copper surface during the carbon deposition process and the full contact between the carbon-containing atmosphere and the powder.
[0011] As a preferred solution, the carbon source includes at least one of acetic acid, polymethyl methacrylate and sucrose. The preferred carbon source of the present invention is a volatile carbon source or a more traditional low-temperature carbon source. Volatile acetic acid is further preferred because acetic acid itself has low cost, and the volatility of acetic acid allows it to be excited at a relatively fast speed in a flowing gas under low vacuum at room temperature (0-35°C), and is carried to the reaction zone by the airflow for carbon deposition, thereby reducing the energy consumption required to excite the carbon source and reducing costs.
[0012] As a preferred solution, the copper source includes at least one of copper oxide, copper oxalate, copper carbonate, basic copper carbonate and copper acetate. The preferred copper source of the present invention can not only achieve thermal decomposition relative to the prior art, but also has a lower cost. It is further preferred to be copper oxalate because copper oxalate is cheap and has a high copper content. And its decomposition temperature is low, and it starts to decompose at about 300°C. At a lower decomposition temperature, the adhesion growth rate between the nano-scale copper powders obtained after decomposition is slow, and sufficient carbon coating can be performed before the powder adhesion growth. Once the carbon coating is performed, the powders are isolated by the coated carbon and will not continue to adhere and grow, and finally obtain an extremely fine carbon-coated copper powder; while at a higher decomposition temperature, the adhesion growth rate between the nano-scale copper powders obtained after decomposition is fast, and the powders can adhere and grow to a certain extent before sufficient carbon coating, and finally obtain a carbon-coated powder with a larger particle size. Therefore, the copper source of the present invention can be decomposed in an inert atmosphere to directly obtain nano-scale copper powder. At the same time, the particle size of the generated copper powder can be regulated by controlling the decomposition temperature, and the particle size of the carbon-coated copper powder can be further controlled.
[0013] As a preferred solution, the temperature of the excitation zone is higher than the volatilization or decomposition temperature of the carbon source. When acetic acid is used as the carbon source, the temperature of the excitation zone can be room temperature, which is 0 to 35°C.
[0014] As a preferred solution, the vacuum degree of the vacuum environment is controlled to be an absolute pressure of <40 kPa. Improving the vacuum degree is beneficial to improving the surface activity of copper decomposition or reduction after decomposition of the copper source, increasing the contact probability between the carbon source and the active sites of the copper source, and promoting the deposition and coating of copper by carbon. In a further preferred solution, the vacuum degree is an absolute pressure of <10 kPa.
[0015] As a preferred solution, the conditions of the reaction zone are: temperature of 350-600°C and time of 0.5-3h. When the temperature of the reaction zone is too low, the copper source cannot be decomposed and the carbon source cannot be deposited on the surface of the copper powder in the form of carbon. When the temperature of the reaction zone is too high, the prepared carbon-coated copper powder has too large a particle size and the possibility of bonding between powders increases. At the same time, energy consumption is high and the process cost is high.
[0016] As a preferred solution, the heating rate of the reaction zone is 3-10°C / min, and the reaction zone is cooled along with the furnace. If the reaction zone is cooled quickly, the carbon coating layer will be damaged due to the inconsistent shrinkage between the carbon layer and the central copper.
[0017] As a preferred solution, the carrier gas is at least one of hydrogen, nitrogen and argon. Hydrogen is further preferred because under low vacuum, residual oxygen will preferentially react with the highly active surface, while inhibiting carbon deposition, resulting in more defects in the coated carbon layer. Hydrogen, as a reducing gas, can effectively prevent the influence of residual oxygen on highly active copper.
[0018] As a preferred solution, the flow rate of the carrier gas is 0.5 to 15 cm / min. If the carrier gas flow rate is too small, the carbon source participating in the reaction is insufficient, and sufficient carbon cannot be deposited on the surface of the high-activity copper for coating, resulting in a prolonged carbon coating time, and the high-activity copper powders are bonded due to lack of carbon isolation; and when the carrier gas flow rate is too large, the order of the carbon coated on the copper surface decreases, and the defects increase.
[0019] The present invention also provides a highly dispersible ultrafine carbon-coated copper powder obtained by the above preparation method. The carbon-coated copper powder has micro-nano particle size, good dispersibility, uniform particle size distribution, complete carbon coating, good oxidation resistance, high carbon order, and good conductivity.
[0020] Finally, the present invention provides a graphene-coated copper powder, which is obtained by graphitizing the highly dispersed ultrafine carbon-coated copper powder prepared as described above. After the low-temperature carbon deposition and coating of the copper powder, the carbon-coated copper powder is further subjected to high-temperature graphitization to convert the carbon-coated copper powder into graphene-coated copper powder. During the high-temperature graphitization process of the ultrafine copper powder after carbon coating, the carbon coated on the surface of the copper powder can isolate the copper powders from each other, thereby preventing the copper powders from adhering to each other and growing at high temperature, thereby obtaining extremely fine graphene-coated copper powder.
[0021] As a preferred solution, the graphitization treatment conditions are: under vacuum conditions, the temperature is 700-1000° C. and the temperature is maintained for 0.5-3 hours.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] (1) The present invention selects a decomposable or decomposable and reducible copper compound as a copper source. When the copper source is decomposed or reduced to expose highly active copper, the carbon source simultaneously deposits and coats the surface of the highly active copper, thereby preventing the adhesion and growth of copper powder. Thus, ultrafine carbon-coated copper powder with high dispersibility and complete and uniform carbon coating is obtained.
[0024] (2) The present invention can adjust the particle size of the carbon-coated copper powder and the thickness and orderliness of the carbon layer according to different carbon coating temperatures and times, gas flow rates, etc.
[0025] (3) The preparation method is simple, the raw material and process costs are low, and it is suitable for industrial-scale production.
[0026] (4) The present invention uses a variety of carbon sources and copper sources, and there is no need to strictly control the particle size of the raw materials. Carbon deposition can be performed at a lower deposition temperature and a shorter deposition time, thereby reducing the cost of the carbon-copper coating process. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is a SEM image of the microscopic morphology of the ultrafine carbon-coated copper powder prepared in Example 1 of the present invention.
[0028] Figure 2 This is a TEM image of the ultrafine carbon-coated copper powder prepared in Example 1 of the present invention.
[0029] Figure 3 This is a Raman graph of the ultrafine carbon-coated copper powder prepared in Example 1 of the present invention.
[0030] Figure 4 It is a SEM image of the microscopic morphology of the ultrafine carbon-coated copper powder prepared in Comparative Example 1 of the present invention.
[0031] Figure 5 It is a microscopic SEM image of the ultrafine carbon-coated copper powder prepared in Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0032] The technical solution of the present invention will be further described below in conjunction with specific embodiments of the present invention. It should be noted that the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments; these embodiments are only for a better understanding of the present invention, rather than limiting the scope of protection of the present invention.
[0033] Unless otherwise specified, all reagents and raw materials used in the present invention are commercially available products or products that can be prepared by known methods.
[0034] Example 1
[0035] Acetic acid was used as the carbon source and copper oxalate as the copper source. The carrier gas was hydrogen, the gas flow rate was 2.5 cm / min, and the vacuum degree was 1 kPa. The temperature of the carbon source excitation zone was 25°C, and the temperature of the high temperature reaction zone was 400°C (heating rate was 5°C / min) for 1.5 hours. After the program was completed, the furnace was cooled to obtain ultrafine carbon-coated copper powder.
[0036] Depend on Figure 1The microscopic morphology SEM image of the ultrafine carbon-coated copper powder prepared in this embodiment shows that the particle size of the carbon-coated copper powder is between 100 and 300 nm, the particle size distribution is uniform, and the powder dispersion is high.
[0037] from Figure 2 It can be seen from the TEM image of the ultrafine carbon-coated copper powder prepared in this embodiment that there are about 5 to 7 relatively complete coating layers on the edge of the copper particles. The interlayer spacing is 0.34 nm, which is consistent with the interlayer spacing of graphite crystals. This shows that the carbon on the surface of the carbon-coated copper powder has a certain degree of order and contains more graphene. The conductivity of the carbon-coated copper powder is 4.7×10 4 S / cm.
[0038] Figure 3 is the Raman graph of the ultrafine carbon-coated copper powder prepared in this embodiment, wherein I D / I G The ratio is 0.68.
[0039] Example 2
[0040] Compared with Example 1, the carbon source was changed to polymethyl methacrylate, the copper source was changed to basic copper carbonate, the temperature of the excitation zone was raised to 160°C, at which polymethyl methacrylate can volatilize under a vacuum environment, the temperature of the reaction zone was 400°C, the insulation time was 2.5h, and the others remained the same.
[0041] The particle size of the obtained carbon-coated copper powder is slightly larger than that of Example 1, ranging from 100 to 400 nm, but the particle size distribution is uniform, the powder dispersion is high, the carbon layer thickness is about 3 to 6 layers, and the conductivity of the carbon-coated copper powder is 5.6×10 4 S / cm, the graphene coating is relatively complete, and the Raman results show that I D / I G The ratio is 0.60.
[0042] Example 3
[0043] Compared with Example 1, only the temperature of the reaction zone was increased to 600° C., and the others remained the same.
[0044] The particle size of the carbon-coated copper powder obtained in Example 1 is larger, ranging from 0.5 to 2 μm, but the particle size distribution is uniform, the powder dispersion is high, the carbon layer thickness is about 5 to 9 layers, and the conductivity of the carbon-coated copper powder is 5.1×10 4 S / cm, graphene is fully coated, and the Raman results show that I D / I G The ratio is 0.55.
[0045] Example 4
[0046] Compared with Example 1, only the carbon deposition holding time in the reaction zone was increased to 2.5 h, and the others remained the same.
[0047] The particle size of the obtained carbon-coated copper powder is basically the same as that of Example 1, between 100 and 300 nm, the particle size distribution is uniform, the powder dispersion is high, and the conductivity of the carbon-coated copper powder is 4.2×10 4 S / cm, but the number of graphene layers on the surface increases to 7-10 layers, and the Raman results show that I D / I G The ratio is 0.70.
[0048] Example 5
[0049] Compared with Example 1, only the gas flow rate was changed to 7.5 cm / min, and the others remained the same.
[0050] The particle size of the obtained carbon-coated copper powder is almost the same as that of Example 1, between 100 and 300 nm, the particle size distribution is uniform, the powder dispersion is high, the carbon layer thickness is about 7 to 10 layers, and the conductivity of the carbon-coated copper powder is 9.8×10 3 S / cm. Raman results D / I G The ratio is 0.78, the order of the surface-coated graphene decreases, the G peak remains basically unchanged, but the D peak increases, indicating that the graphene defects increase.
[0051] Example 6
[0052] Compared with Example 1, the graphitization degree is improved only by adding a heat preservation temperature of 800° C. for 0.5 h in the subsequent process to obtain graphene-coated copper powder.
[0053] The particle size of the obtained graphene-coated copper powder is basically the same as that in Example 1, between 100 and 400 nm, with uniform particle size distribution and high powder dispersion. The conductivity of the carbon-coated copper powder is 9.6×10 4 S / cm, the number of graphene layers on the surface is about 5 to 8 layers, and the Raman results show that I D / I G The ratio is 0.31, and the order of the carbon layer is significantly improved.
[0054] Comparative Example 1
[0055] Compared with Example 1, only the carbon source was removed, and the others remained the same.
[0056] Depend on Figure 4 It can be seen that most of the powder particle sizes are still between 100 and 300 nm. However, due to the lack of carbon layer isolation between the powders, there is a lot of adhesion between the copper powders even at a temperature of 400 °C, and more coarse particles of 1 to 3 μm appear. The particle size uniformity and particle dispersion are reduced, and the carbon-coated copper structure powder is not obtained. The conductivity is 1.3×103 S / cm.
[0057] Comparative Example 2
[0058] Compared with Example 2, only the copper source is changed to 3-5 μm pure copper powder, and the rest remains the same.
[0059] Depend on Figure 5 It can be seen that although the surface of the copper powder particles is coated with a lot of graphene, the adhesion between the particles is serious, the copper powder particles grow large, the dispersion is poor, and the conductivity is 8.7×10 2 S / cm, Raman results I D / I G The ratio is 0.81.
Claims
1. A method for preparing highly dispersible ultrafine carbon-coated copper powder, characterized in that: In a vacuum environment, the carbon source is excited in the excitation zone and then transported to the reaction zone by a carrier gas to be deposited and coated on the copper powder to obtain; The copper powder is obtained by decomposing a thermally decomposable copper source in a reaction zone or reducing the decomposition thereof.
2. The method for preparing a highly dispersible ultrafine carbon-coated copper powder according to claim 1, characterized in that: The carbon source includes at least one of acetic acid, polymethyl methacrylate and sucrose.
3. The method for preparing a highly dispersible ultrafine carbon-coated copper powder according to claim 2, characterized in that: The copper source includes at least one of copper oxide, copper oxalate, copper carbonate, basic copper carbonate and copper acetate.
4. The method for preparing a highly dispersible ultrafine carbon-coated copper powder according to claim 1, characterized in that: The temperature of the excitation zone is higher than the volatilization or decomposition temperature of the carbon source.
5. The method for preparing a highly dispersible ultrafine carbon-coated copper powder according to claim 4, characterized in that: The conditions of the reaction zone are: temperature of 350-600° C. and time of 0.5-3 h.
6. The method for preparing a highly dispersible ultrafine carbon-coated copper powder according to claim 5, characterized in that: The heating rate of the reaction zone is 3-10°C / min, and the reaction zone is cooled along with the furnace during cooling.
7. The method for preparing highly dispersible ultrafine carbon-coated copper powder according to any one of claims 1 to 6, characterized in that: The carrier gas is at least one of hydrogen, nitrogen and argon.
8. The method for preparing highly dispersible ultrafine carbon-coated copper powder according to claim 7, characterized in that: The flow rate of the carrier gas is 0.5-15 cm / min.
9. A highly dispersible ultrafine carbon-coated copper powder, characterized in that: The method is obtained by the preparation method according to any one of claims 1 to 8.
10. A graphene-coated copper powder, characterized in that: The highly dispersed ultrafine carbon-coated copper powder according to claim 9 is obtained by graphitization treatment; the graphitization treatment conditions are: under vacuum conditions, the temperature is 700-1000° C. and the temperature is maintained for 0.5-3 hours.
Citation Information
Patent Citations
Graphene / copper powder material and preparation method thereof
CN110385432A