Method for preparing nickel-based superalloy standard sample for spectral analysis through powder metallurgy
Through powder metallurgy technology, including vacuum induction furnace smelting, argon atomization and hot press sintering, standard samples of nickel-based high-temperature alloys with uniform composition were prepared, which solved the problem of insufficient sample composition uniformity in the prior art and improved the Accuracy of spectral analysis.
Patent Information
- Application Number
- CN202310584487.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-11-26
AI Technical Summary
The prior art is difficult to ensure the composition uniformity of high-temperature alloy standard samples, resulting in insufficient accuracy of spectrometer detection.
Standard samples of nickel-based high-temperature alloys are prepared by powder metallurgy technology, and the uniformity and density of components are ensured through vacuum induction furnace smelting, argon atomization, high-energy ball milling, electrostatic separation and hot press sintering.
It improves the composition uniformity and detection accuracy of the sample, reduces composition segregation, and provides a reliable basis for high-temperature alloy composition analysis.
Smart Images

Figure CN119016732A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgical analysis, and in particular relates to a method for preparing a nickel-based high-temperature alloy standard sample for spectral analysis by powder metallurgy. Background Art
[0002] High-temperature alloy materials have many advantages such as good corrosion resistance, heat resistance, high fatigue strength, etc. They are widely used in aircraft engines, gas turbine turbines, turbine blades and machine parts used under corrosive conditions. The element content of high-temperature alloy materials has a great influence on their performance, so the element content needs to be strictly controlled in production. The detection of high-temperature alloy element content mainly uses spectrometers for analysis, such as: inductively coupled plasma emission spectrometer, direct reading spectrometer, X-ray fluorescence spectrometer, atomic absorption spectrometry, etc. Among them, the most widely used spectrometers are X-ray fluorescence spectrometers and direct reading spectrometers. When using a spectrometer for analysis, the first thing to get is the relative content of the elements. A reference to a standard sample is needed for reference and comparison to obtain the content of the elements in the sample. The role of the standard sample: 1. Establish a "standard curve"; 2. As a known substance, it is used to evaluate the measurement method; 3. As an internal control substance, it is analyzed at the same time as the substance to be tested to calibrate the results. When the spectrometer analyzes the sample, the analytical data obtained will be different from the true value. These differences come from the drift of the standard working curve, the spectral interference between elements, the state of the surface of the sample to be tested, and the physical state of the sample. Using standard samples with similar composition to establish the working curve can reduce the analysis error. Therefore, when analyzing samples with a spectrometer, it is very dependent on standard samples, especially high-temperature alloys with a high degree of alloying. Requirements for standard samples: very close to the type and content of elements in the sample to be tested, uniform composition, and no obvious defects.
[0003] At present, most of the methods for preparing standard samples for high-temperature alloy spectra are: directly cutting and processing at the appropriate position of the master alloy ingot, and directly using it as a standard sample after surface treatment. Although this method is simple and easy to operate, it is difficult to control the uniformity of the sample, the qualified rate of the product is low, and the accuracy of the spectrometer detection cannot be guaranteed. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing a nickel-based high-temperature alloy standard sample for spectral analysis by powder metallurgy, which can ensure the uniformity of each element composition of the prepared standard sample.
[0005] In order to achieve the above object, the technical solution of the present invention is:
[0006] A method for preparing a nickel-based high-temperature alloy standard sample for spectral analysis by powder metallurgy, comprising the following steps:
[0007] (1) Using a 50 kg vacuum induction furnace to smelt the required master alloy raw materials at a smelting temperature of 1350°C to 1550°C, casting into master alloy ingots, and preparing for remelting and powder spraying after treatment;
[0008] (2) placing the master alloy ingot into a 10 kg argon-protected vacuum furnace for remelting, using an argon atomizing device to atomize the molten metal flowing down the nozzle of the vacuum furnace into powder under high-pressure argon gas, with a casting temperature of 1400° C. to 1520° C. and an argon gas injection pressure of 1.2 to 1.8 MPa;
[0009] (3) sieving under argon atmosphere to obtain nickel-based high-temperature alloy powder with a particle size of ≤200 mesh, and crushing the powder using a high-energy ball mill;
[0010] (4) Using electrostatic separation to remove ceramic inclusions from the powder, at a pressure less than or equal to 8×10 -3 Pa vacuum and heated to 200-500°C to remove the gas adsorbed on the powder surface; taking powders from different parts, and using inductively coupled plasma mass spectrometry to detect the content of major elements in the powder;
[0011] (5) Under argon protection, the powder is fully shaken and loaded into a hot pressing sintering mold;
[0012] (6) hot pressing and sintering the powder loaded into the mold in step (5), with a holding temperature of 1000-1200° C., a pressure of 20 MPa-30 MPa, a holding time of 1-3 h, a heating rate of 10-15° C. / min, and cooling to room temperature with the furnace;
[0013] (7) The samples obtained by hot pressing sintering are subjected to hot isostatic pressing treatment, with a holding temperature of 1000-1200°C, a pressure of 110MPa-120MPa, a holding time of 1-3h, a heating rate of 10-15°C / min, and the temperature is cooled to room temperature along with the furnace; each sample is divided into three equal parts by wire cutting, and the upper and lower surfaces of each sample are ground and polished.
[0014] In the method for preparing nickel-based high-temperature alloy standard samples for spectral analysis by powder metallurgy, in step (4), the content of major elements in powders from different parts of the same batch is detected by an inductively coupled plasma mass spectrometer.
[0015] In the method for preparing a nickel-based high-temperature alloy standard sample for spectral analysis by powder metallurgy, in step (5), the mold size is Φ38mm in diameter and 30mm to 35mm in height.
[0016] The method for preparing a nickel-based high-temperature alloy standard sample for spectral analysis by powder metallurgy comprises the following steps: in step (5), the powder is fully shaken under argon protection, and mixed by multi-directional vibration at a frequency of 10 to 80 times / min for a mixing time of 0.5 to 1 hour.
[0017] The design concept of the present invention is:
[0018] The present invention prepares a high-temperature alloy master alloy ingot through vacuum induction melting, and then obtains alloy powder through surface cleaning, grinding and cutting. Then, a vacuum smelting argon atomization method is used to obtain alloy powder, and powder with a particle size of ≤200 mesh is screened out. The powder is further crushed by a high-energy ball mill to improve the activity and uniformity of the alloy powder, so that the powder can be better bonded during hot isostatic pressing, the density of the alloy sample is improved, and a nickel-based high-temperature alloy standard sample with uniform composition and no surface defects can be obtained.
[0019] The advantages and beneficial effects of the present invention are:
[0020] 1. The present invention uses powder metallurgy technology to prepare a nickel-based high-temperature alloy standard sample for spectral analysis. The standard sample is prepared using nickel-based high-temperature alloy powder with uniform composition. After hot pressing sintering and hot isostatic pressing, a standard sample with uniform composition and small segregation is obtained. The standard sample prepared by this method provides a reliable basis for high-temperature alloy composition analysis and guarantees the accuracy of high-temperature alloy furnace detection.
[0021] 2. The method for preparing the nickel-based high-temperature alloy spectral analysis standard sample in the present invention is applicable to all nickel-based high-temperature alloys.
[0022] 3. The present invention adopts metallurgical powder technology to prepare standard samples. Compared with the method of directly cutting raw materials from the master alloy ingot and simply processing them as standard samples, it can improve the uniformity of the samples, reduce component segregation, and improve the accuracy of sample detection. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is the surface morphology of the sample. DETAILED DESCRIPTION
[0024] In the specific implementation process, the present invention proposes a method for preparing a nickel-based high-temperature alloy standard sample for spectral analysis by powder metallurgy, which specifically includes the following steps: ① preparing a high-temperature alloy master alloy; ② putting the alloy ingot into an argon-protected vacuum furnace for remelting, using an argon atomization device to prepare the master alloy into powder, and finally obtaining a high-temperature alloy powder with a particle size of ≤200 mesh by selection and screening; ③ using a high-energy ball mill to grind and reduce its sphericity; ④ placing the evenly mixed high-temperature alloy powder in a grinding mold for hot pressing and sintering; ⑤ hot isostatic pressing treatment.
[0025] The present invention will be further described below in conjunction with specific embodiments.
[0026] Example
[0027] The nickel-based high-temperature alloy K465 is selected in this embodiment. Its specific composition, by weight percentage, is: C 0.15, Cr 9.32, Co 10.16, Mo 1.91, Zr 0.026, Al 5.12, Ti 2.71, Nb 1.03, B 0.018, W 10.14, and Ni is the balance.
[0028] The method for preparing the nickel-based high-temperature alloy standard sample comprises the following steps:
[0029] (1) Alloy raw materials are prepared according to the composition range of the high-temperature alloy, added into a vacuum induction furnace in a certain order, and melted and cast to obtain a Φ80×1000mm round rod-shaped master alloy ingot.
[0030] (2) The mother alloy ingot is polished and cut into suitable sizes, and put into a 25Kg furnace for remelting. After the alloy ingots of suitable sizes are obtained, the different alloy ingots are put into a 10Kg argon-protected vacuum furnace for remelting. The molten liquid flowing down the nozzle of the vacuum furnace is atomized into powder under high-pressure argon using an argon atomizing device. The casting temperature is 1400°C to 1520°C (Examples 1-3 are 1420°C, 1460°C, and 1500°C, respectively), and the pressure of the argon injection is 1.2 to 1.8 MPa (Examples 1-3 are 1.3 MPa, 1.5 MPa, and 1.7 MPa, respectively).
[0031] (3) Preparation of high-temperature alloy spectral analysis standard samples by powder metallurgy has very strict requirements on powder quality. High-temperature alloy powder with a particle size of ≤200 mesh is screened under the protection of argon atmosphere. The powder is crushed by a high-energy ball mill to break the sphericity. This method can also reduce the powder particle size, which is conducive to the agglomeration of the powder during the sintering process and improve the density of the sample.
[0032] (4) Using electrostatic separation to remove ceramic inclusions from the powder, at a pressure less than or equal to 8×10 -3 Pa (Examples 1-3 are 8×10 -3 Pa, 6×10 -3 Pa, 4×10 -3 Pa) to 200-500°C (300°C, 400°C, and 500°C in Examples 1-3, respectively) to remove the gas adsorbed on the powder surface, which can improve the purity of the powder. Under argon protection, the powder is fully shaken and mixed in multiple directions at a frequency of 10-80 times / min (20 times / min, 40 times / min, and 60 times / min in Examples 1-3, respectively) for 0.5-1h (0.6h, 0.8h, and 1h in Examples 1-3, respectively). The ceramic inclusions in the powder are removed by electrostatic separation. When the pressure is less than or equal to 8×10 -3Pa (Examples 1-3 are 8×10 -3 Pa, 6×10 -3 Pa, 4×10 -3 The powder was heated to 200-500°C (300°C, 400°C, and 500°C in Examples 1-3, respectively) under a vacuum of 1.5 Pa to remove the gas adsorbed on the powder surface. Three portions of powder from different parts were taken and the contents of the major elements in the powder were detected by inductively coupled plasma mass spectrometry (ICP-MS). The contents of each element are shown in Table 1.
[0033] Table 1. Content of each element in the powder detected by inductively coupled plasma mass spectrometry (wt%)
[0034] Powder No. Al Ti Cr Nb Mo W Co 1# 5.12 2.71 9.31 1.02 1.9 10.14 10.16 2# 5.1 2.72 9.33 1.03 1.91 10.15 10.17 3# 5.13 2.7 9.32 1.04 1.92 10.12 10.16 average value 5.12 2.71 9.32 1.03 1.91 10.14 10.16
[0035] (5) Under argon protection, the powder was fully shaken and then loaded into a hot pressing sintering mold for hot pressing sintering. The holding temperature was 1000-1200°C (1050°C, 1100°C, and 1150°C for Examples 1-3, respectively), the pressure was 20MPa-30MPa (20MPa, 25MPa, and 30MPa for Examples 1-3, respectively), the holding time was 1-3h (1h, 2h, and 3h for Examples 1-3, respectively), the heating rate was 10-15°C / min (10°C / min, 12°C / min, and 15°C / min for Examples 1-3, respectively), and the temperature was cooled to room temperature with the furnace. The sample size after sintering was Φ38mm in diameter and 30mm-35mm in height.
[0036] (6) The samples obtained by hot pressing sintering were subjected to hot isostatic pressing treatment, with a holding temperature of 1000-1200°C (1050°C, 1100°C, and 1150°C for Examples 1-3, respectively), a pressure of 110MPa-120MPa (110MPa, 115MPa, and 120MPa for Examples 1-3, respectively), a holding time of 1-3h (1h, 2h, and 3h for Examples 1-3, respectively), a heating rate of 10-15°C / min (10°C / min, 12°C / min, and 15°C / min for Examples 1-3, respectively), and the temperature was cooled to room temperature along with the furnace.
[0037] After the powder is sintered by hot pressing, hot isostatic pressing is performed to improve the uniformity and density of the sample. Each sample is divided into three equal parts by wire cutting, and three samples with a diameter of Φ38mm and a height of about 10mm are obtained. The upper and lower surfaces of each sample are polished.
[0038] (7) The upper and lower surfaces of the three samples in Example 1 were marked as 1S, 1X, 2S, 2X, 3S, and 3X, respectively, by a direct reading spectrometer. The contents of Al, Ti, Cr, Mo, Nb, W, and Co on the upper and lower surfaces of the samples were detected by a direct reading spectrometer. The results were statistically analyzed, and the single-factor variance method was used to verify whether the samples prepared by this method met the uniformity requirements of the standard samples. The results are shown in Tables 2 to 8.
[0039] Table 2. Homogeneity test results of Al element in samples
[0040]
[0041] Table 3. Homogeneity test results of Ti element in samples
[0042]
[0043]
[0044] Table 4. Homogeneity test results of Cr element in samples
[0045]
[0046] Table 5. Homogeneity test results of Nb element in samples
[0047]
[0048]
[0049] Table 6. Homogeneity test results of Mo element in samples
[0050]
[0051] Table 7. Homogeneity test results of W element in samples
[0052]
[0053]
[0054] Table 8. Homogeneity test results of Co element in samples
[0055]
[0056] (7) Observe the sample surface under a microscope and there is no obvious defect such as looseness. Figure 1 .
[0057] The implementation results show that the present invention uses a uniformly mixed high-temperature alloy powder to prepare a high-temperature alloy standard sample for a spectrometer by a powder metallurgy method. The powder is hot pressed and sintered and then hot isostatic pressed to improve the density of the sample, reduce looseness, heat-induced voids, inclusions, etc., and can solve the problem of uneven standard samples. According to the method described in the present invention, a standard sample with uniform composition can be obtained, and the reproducibility of each element is very good, which solves the problem of difficulty in obtaining standard samples for industrial production of high-temperature alloys.
Claims
1. A method for preparing a nickel-based high-temperature alloy standard sample for spectral analysis by powder metallurgy, characterized in that: The following steps are involved: (1) Using a 50 kg vacuum induction furnace to smelt the required master alloy raw materials at a smelting temperature of 1350°C to 1550°C, casting into master alloy ingots, and preparing for remelting and powder spraying after treatment; (2) placing the master alloy ingot into a 10 kg argon-protected vacuum furnace for remelting, using an argon atomizing device to atomize the molten metal flowing down the nozzle of the vacuum furnace into powder under high-pressure argon gas, with a casting temperature of 1400° C. to 1520° C. and an argon gas injection pressure of 1.2 to 1.8 MPa; (3) sieving under argon atmosphere to obtain nickel-based high-temperature alloy powder with a particle size of ≤200 mesh, and crushing the powder using a high-energy ball mill; (4) Using electrostatic separation to remove ceramic inclusions from the powder, at a pressure less than or equal to 8×10 -3 Pa vacuum and heated to 200-500°C to remove the gas adsorbed on the powder surface; taking powders from different parts, and using inductively coupled plasma mass spectrometry to detect the content of major elements in the powder; (5) Under argon protection, the powder is fully shaken and loaded into a hot pressing sintering mold; (6) hot pressing and sintering the powder loaded into the mold in step (5), with a holding temperature of 1000-1200° C., a pressure of 20 MPa-30 MPa, a holding time of 1-3 h, a heating rate of 10-15° C. / min, and cooling to room temperature with the furnace; (7) The samples obtained by hot pressing sintering are subjected to hot isostatic pressing treatment, with a holding temperature of 1000-1200°C, a pressure of 110MPa-120MPa, a holding time of 1-3h, a heating rate of 10-15°C / min, and the temperature is cooled to room temperature along with the furnace; each sample is divided into three equal parts by wire cutting, and the upper and lower surfaces of each sample are ground and polished.
2. The method for preparing a nickel-based high-temperature alloy standard sample for spectral analysis by powder metallurgy according to claim 1, characterized in that: In step (4), the contents of major elements in powders from different parts of the same batch are detected using an inductively coupled plasma mass spectrometer.
3. The method for preparing a nickel-based high-temperature alloy standard sample for spectral analysis by powder metallurgy according to claim 1, characterized in that: In step (5), the mold size is Φ38mm in diameter and 30mm to 35mm in height.
4. The method for preparing a nickel-based high-temperature alloy standard sample for spectral analysis by powder metallurgy according to claim 1, characterized in that: In step (5), the powder is fully shaken under argon protection, and mixed by multi-directional vibration at a frequency of 10 to 80 times / min for a mixing time of 0.5 to 1 h.