White vehicle body front longitudinal beam welding method

Through laser wire fill welding technology and steep rise-constant slow-down-continuous slow-down waveform, the problems of low production efficiency and insufficient joint strength in automobile front longitudinal beam welding are solved, and the efficient and accurate welding process is achieved, which improves the Performance and production efficiency of welded joints.

CN119016871APending Publication Date: 2024-11-26LIAONING ZHONGWANG GROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411348196.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-26
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing automotive front longitudinal beam welding technology has problems such as low production efficiency, low joint connection strength, additional processing of keyholes and damage to profiles.

Method used

Laser wire fill welding technology is used to weld through steep rise-constant slow-down-continuous slow-down waveform, combined with online monitoring of welds and real-time rework, avoiding bevel opening and repair welding, and improving assembly accuracy and production efficiency.

Benefits of technology

It improves welding speed and joint strength, reduces production costs, ensures repeatability and aesthetics of weld quality, avoids subsequent machine-adding processes, and improves the tensile strength and bending performance of welded joints.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016871A_ABST
    Figure CN119016871A_ABST
Patent Text Reader

Abstract

The invention provides a body-in-white front longitudinal beam welding method. The body-in-white front longitudinal beam welding method comprises the following steps that a welding assembly tool is positioned; the workpiece is fixed to a welding assembly tool; a welding system is set, welding parameters and a welding waveform are determined, and the welding waveform is a steep rising-constant-speed slow descending-continuous-variable-speed slow descending waveform; one side of the workpiece is welded through laser filler wire welding, after one side of the workpiece is welded, the workpiece is taken down from the welding assembly tool, the workpiece is fixed to the welding assembly tool again after being turned over, the other side of the workpiece is welded through laser filler wires till the other side of the workpiece is welded, and the workpiece is taken down from the welding assembly tool; the appearance of a weld joint is detected through visual detection and penetration detection, and the performance of a welded joint is detected through tensile strength test and bending performance test. While the production efficiency is improved, the welding quality is ensured, the subsequent machining process is not needed, and the production cost is reduced while the production efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal processing, in particular to the technical field of metal welding, and specifically discloses a method for welding a front longitudinal beam of a body-in-white. Background Art

[0002] The front longitudinal beam of a car belongs to the front body part of the car. Its front end is connected to the anti-collision beam, and its rear end is connected to the driver's compartment. Studies have shown that when a car has a head-on collision, 70% of the energy is absorbed by the front longitudinal beam. The front longitudinal beam is usually designed with a front crushing section and a rear non-deformed section. In this way, when a collision occurs, the front section can not only absorb the collision energy, but also keep the rear section non-deformed to protect the safety of the driver's compartment. The two parts of the front longitudinal beam are connected in the form of tube-to-tube welding, usually using metal arc gas shielded welding (MIG), and the welding is carried out in sections. In order to ensure the penetration depth, a 60° groove is usually required. After welding, the arc starting and arc ending positions need to be ground, which increases the production process and reduces the production efficiency. In addition, the welding speed of MIG welding is slow and is greatly affected by human factors. The heat input of MIG welding is large, and the softening phenomenon of the welded joint is obvious, which will affect the overall connection strength of the joint. With the rise of friction stir welding technology, the front longitudinal beam tube-to-tube connection can also be connected by friction stir welding (FSW). After welding, the keyhole is repaired or a margin is left for machining. Removing the friction stir welding keyhole is not only time-consuming and labor-intensive, but also increases costs. In addition, the friction stir welding also requires high assembly accuracy. Since the tube wall of the automobile front longitudinal beam profile is relatively thin, the existing laser welding will cause damage to the profile. In view of the above-mentioned problems, it is necessary to study and design a new type of white body front longitudinal beam welding method to overcome the problems existing in the existing front longitudinal beam welding. Summary of the invention

[0003] The present invention proposes a method for welding a front longitudinal beam of a body in white to solve the problems of low production efficiency, low overall connection strength of joints, keyholes requiring additional processing and damage to profiles in the existing front longitudinal beam welding.

[0004] The present invention provides a method for welding a front longitudinal beam of a body in white, comprising the following steps:

[0005] S1. Position the welding assembly tooling;

[0006] S2. Fixing the workpiece on the welding assembly tooling;

[0007] S3. Setting the welding system, determining the welding parameters and welding waveform, wherein the welding waveform is a steep rise-constant speed slow fall-continuous-variable speed slow fall waveform;

[0008] S4. Weld one side of the workpiece by laser wire welding. After welding one side of the workpiece is completed, remove the workpiece from the welding assembly tooling, flip the workpiece and re-fix it on the welding assembly tooling, weld the other side of the workpiece by laser wire welding until the welding of the other side of the workpiece is completed, and remove the workpiece from the welding assembly tooling;

[0009] S5. Perform visual inspection and penetrant inspection on the appearance of welds, and perform performance inspection on weld joints through tensile strength test and bending performance test.

[0010] According to a method for welding a front longitudinal beam of a body-in-white in some embodiments of the present application, the welding assembly tool comprises a base, an end stopper, four pneumatic clamping devices and two pneumatic jacking devices;

[0011] The base is used to support the workpiece, the upper surface of the base is provided with a welding groove, the welding groove is used to reserve space for the excess height of the weld, and the upper surface of the base is provided with a baffle, and the baffle is in contact with one side of the workpiece;

[0012] The end limit block is arranged at the front side of the base, and is used to limit the workpiece in the X direction;

[0013] The four pneumatic clamping devices are respectively arranged on the left and right sides of the base, and the pneumatic clamping device includes a clamping plate, which is arranged above the workpiece and is used to cooperate with the base to limit the workpiece in the Y direction;

[0014] The two pneumatic jacking devices are arranged on the side of the base away from the baffle, and the pneumatic jacking device includes a jacking rod, which is in contact with the other side of the workpiece and is used to cooperate with the baffle to limit the workpiece in the Z direction.

[0015] According to a method for welding a front longitudinal beam of a body in white in some embodiments of the present application, in step S3, the welding parameters include wire feeding speed, welding speed, defocus, filament spacing, laser incident angle and shielding gas flow rate, the wire feeding speed is 4-6 m / min, the welding speed is 3-5 m / min, the defocus is 0-8 mm, the filament spacing is 0-2 mm, the laser incident angle is 5-10°, and the shielding gas flow rate is 20-35 L / min.

[0016] According to a method for welding a front longitudinal beam of a body in white in some embodiments of the present application, the steep rise-constant speed descent-continuous-variable speed descent waveform includes a steep rise stage, a uniform speed descent stage, a continuous stage and a variable speed descent stage. The welding in the steep rise stage, the uniform speed descent stage and the variable speed descent stage are all carried out by pulsed laser wire filling welding, and the welding in the continuous stage is carried out by continuous laser wire filling welding.

[0017] According to a method for welding a front longitudinal beam of a body in white in some embodiments of the present application, the steep rise time t1 of the steep rise stage is 100ms~150ms, and the laser power P1 of the steep rise stage is 7000W~7500W; the uniform speed slow-down time t2 of the uniform speed slow-down stage is 300ms~500ms, the laser power P2 of the uniform speed slow-down starting point of the uniform speed slow-down stage is 7000W~7500W, and the laser power P2 of the uniform speed slow-down end point of the uniform speed slow-down stage is 7000W~7500W. The rate P2' is 5800W~6200W; the continuous time t3 of the continuous stage is ttotal-t1-t2-t4, and the laser power P3 of the continuous stage is 5800W~6200W; the variable speed slow down time t4 of the variable speed slow down stage is 500ms~750ms, and the variable speed slow down starting point laser power P4 of the variable speed slow down stage is 5800W~6200W, and the variable speed slow down end point laser power P4' of the variable speed slow down stage is 0W.

[0018] According to a method for welding a front longitudinal beam of a body-in-white in some embodiments of the present application, the ratio of the steep rise time t1, the uniform speed slow-down time t2 and the variable speed slow-down time t4 is 1:3:5.

[0019] According to a method for welding a front longitudinal beam of a body-in-white in some embodiments of the present application, the laser power P1 in the steep rise stage is 120% of the laser power P3 in the continuous stage.

[0020] According to a method for welding a front longitudinal beam of a body-in-white in some embodiments of the present application, in step S4, front wire feeding is used during welding, the shielding gas is located behind the welding point, and the wire is retracted 100ms before the end of welding.

[0021] According to a method for welding a front longitudinal beam of a body-in-white in some embodiments of the present application, the welding system includes a housing, an optical fiber coupling device, a laser head, a weld monitoring unit, a shielding gas pipeline, a first shielding gas connection plate, a second shielding gas connection plate, a wire feeding hose and a wire feeding tube connection plate;

[0022] The optical fiber coupling device is arranged at the upper end of the housing, and is used to receive laser light and transmit it to the laser head;

[0023] The laser head is arranged at the lower end of the shell, and the laser head is used to emit welding laser;

[0024] The weld monitoring unit is arranged on one side of the shell, and the weld monitoring unit is used to monitor the weld in real time;

[0025] The shielding gas pipeline is connected to the shell through the second shielding gas connection plate and the first shielding gas connection plate, the shielding gas pipeline is used to transport shielding gas, and the outlet of the shielding gas pipeline is arranged above the weld;

[0026] The wire feeding hose is connected to the shell through the wire feeding tube connecting plate, and the wire feeding hose is used to transport welding wire to the weld pool.

[0027] According to a method for welding a front longitudinal beam of a body-in-white in some embodiments of the present application, step S4 also includes online monitoring of the weld, and during the welding process, the weld forming quality and signal fluctuation are recorded in real time by the weld monitoring unit, the weld welding quality is detected and analyzed, and unqualified positions are repaired.

[0028] The present invention proposes a method for welding the front longitudinal beam of a body in white, which is less affected by human factors and can ensure the repeatability of the weld quality. In addition, no groove is required during welding, which improves production efficiency. The present invention also has lower assembly accuracy requirements than stir friction welding, and there is no keyhole after welding, so no need for repair welding and machining. In addition, real-time monitoring of the weld can be achieved during the welding process, and the abnormal welding points can be traced, so that accurate repair can be achieved to ensure welding quality. The present invention also designs a laser welding waveform that eliminates arc crater cracks after welding, which improves production efficiency while ensuring welding quality, reduces the heat input of the welding joint, thereby narrowing the heat-affected zone, reducing the softening degree of the joint, and greatly improving the performance of the weld. The weld joint has a high tensile strength. After welding is completed, the shape is beautiful, and no subsequent machining process is required. While improving production efficiency, it reduces production costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a schematic flow chart of a method for welding a front longitudinal beam of a body-in-white in the present invention;

[0030] Figure 2 The three-dimensional structural intention of the front longitudinal beam workpiece of the present invention;

[0031] Figure 3 The three-dimensional structural intention of the front longitudinal beam of the present invention;

[0032] Figure 4 It is a three-dimensional structural schematic diagram of the welding assembly tooling of the present invention;

[0033] Figure 5 It is a schematic diagram of the three-dimensional structure of the base of the present invention;

[0034] Figure 6 This is a schematic diagram of welding waveforms in Example 2 of the present invention;

[0035] Figure 7 It is a schematic diagram of the three-dimensional structure of the welding system of the present invention;

[0036] Figure 8 This is a schematic diagram of the three-dimensional structure of the welding process in Example 3 of the present invention;

[0037] Fig. 9This is a picture of the weld after welding in Example 3 of the present invention;

[0038] Fig.10 This is a schematic diagram of welding waveforms of Comparative Example 1 of the present invention;

[0039] Fig.11 This is a picture of the weld after welding in Comparative Example 1 of the present invention;

[0040] Fig.12 This is a schematic diagram of welding waveforms of Comparative Example 4 of the present invention;

[0041] Fig.13 This is a schematic diagram of welding waveforms of Comparative Example 5 of the present invention;

[0042] Fig.14 This is a schematic diagram of the welding waveform of comparative example 5 of the present invention.

[0043] In the figure: 1. base, 1-1. welding groove, 1-2. baffle, 2. end limit block, 3. pneumatic clamping device, 3-1. clamping plate, 4. pneumatic jacking device, 4-1. jacking rod, 5. shell, 6. optical fiber coupling device, 7. laser head, 8. weld monitoring unit, 9. shielding gas pipeline, 10. first shielding gas connecting plate, 11. second shielding gas connecting plate, 12. wire feeding hose, 13. wire feeding tube connecting plate, 14. first workpiece, 15. second workpiece. DETAILED DESCRIPTION

[0044] The following embodiments of the present invention are described in further detail in conjunction with the accompanying drawings and examples. The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention.

[0045] Embodiment 1, this embodiment provides a method for welding the front longitudinal beam of a body in white, such as Figure 1 As shown, the following steps are included:

[0046] S1. Position the welding assembly tooling;

[0047] S2. Fix the workpiece on the welding assembly tool;

[0048] S3. Set the welding system to determine the welding parameters and welding waveform. The welding waveform is a steep rise-constant speed slow drop-continuous-variable speed slow drop waveform;

[0049] S4. Weld one side of the workpiece by laser wire welding. After welding one side of the workpiece is completed, remove the workpiece from the welding assembly tooling, flip the workpiece and re-fix it on the welding assembly tooling, and weld the other side of the workpiece by laser wire welding until the welding of the other side of the workpiece is completed, and remove the workpiece from the welding assembly tooling;

[0050] S5. Perform visual inspection and penetrant inspection on the appearance of welds, and perform performance inspection on weld joints through tensile strength test and bending performance test.

[0051] Embodiment 2: This embodiment provides a method for welding a front longitudinal beam of a body-in-white, comprising the following steps:

[0052] S1. Position the welding assembly tooling;

[0053] Among them, the welding assembly tooling used in this embodiment is as follows Figure 4 As shown, it includes a base 1, an end stopper 2, four pneumatic clamping devices 3 and two pneumatic jacking devices 4; the base 1 is used to support the workpiece, such as Figure 5 As shown, a welding groove 1-1 is provided on the upper surface of the base 1, and the welding groove 1-1 is used to reserve space for the excess height of the weld. A baffle 1-2 is provided on the upper surface of the base 1, and the baffle 1-2 is in contact with one side of the workpiece; an end limit block 2 is arranged on the front side of the base 1, and is used to limit the workpiece in the X direction; four pneumatic clamping devices 3 are respectively arranged on the left and right sides of the base 1, and the pneumatic clamping device 3 includes a clamping plate 3-1, which is arranged above the workpiece, and the clamping plate 3-1 is used to cooperate with the base 1 to limit the workpiece in the Y direction; two pneumatic jacking devices 4 are arranged on the side of the base 1 away from the baffle 1-2, and the pneumatic jacking device 4 includes a jacking rod 4-1, which is in contact with the other side of the workpiece, and the jacking rod 4-1 is used to cooperate with the baffle 1-2 to limit the workpiece in the Z direction;

[0054] S2. Fix the workpiece on the welding assembly tool. Figure 2 and Figure 3 As shown;

[0055] S3. Set up the welding system and determine the welding parameters and welding waveform, such as Figure 6 As shown, the welding waveform is a steep rise-constant speed slow decline-continuous-variable speed slow decline waveform;

[0056] Among them, the welding parameters include wire feeding speed, welding speed, defocus, filament spacing, laser incident angle and shielding gas flow rate. The wire feeding speed is 4-6m / min, the welding speed is 3-5m / min, the defocus is 0-8mm, the filament spacing is 0-2mm, the laser incident angle is 5-10°, and the shielding gas flow rate is 20-35L / min.

[0057] The steep rise-uniform speed slow down-continuous-variable speed slow down waveform includes a steep rise stage, a uniform speed slow down stage, a continuous stage and a variable speed slow down stage. The welding in the steep rise stage, the uniform speed slow down stage and the variable speed slow down stage all adopts pulsed laser wire welding, and the welding in the continuous stage adopts continuous laser wire welding. The steep rise time t1 of the steep rise stage is 100ms~150ms, and the laser power P1 of the steep rise stage is 7000W~7500W; the uniform speed slow down time t2 of the uniform speed slow down stage is 300ms~500ms, and the uniform speed slow down starting point laser of the uniform speed slow down stage is 200ms~500ms. The optical power P2 is 7000W to 7500W, and the laser power P2' at the end point of the uniform speed reduction stage is 5800W to 6200W; the continuous time t3 of the continuous stage is ttotal-t1-t2-t4, and the laser power P3 of the continuous stage is 5800W to 6200W; the variable speed reduction time t4 of the variable speed reduction stage is 500ms to 750ms, and the laser power P4 at the starting point of the variable speed reduction stage is 5800W to 6200W, and the laser power P4' at the end point of the variable speed reduction stage is 0W;

[0058] More preferably, the ratio of the steep rise time t1, the uniform speed slow-down time t2 and the variable speed slow-down time t4 is 1:3:5.

[0059] The steep rise stage can be set to solve the problem of insufficient heat in the plate at the start of the weld, which is not conducive to the absorption of laser energy. The power is increased to melt the material and form a more stable laser keyhole. As the welding time increases, the temperature of the test plate gradually increases, and the absorption of laser power gradually increases. In order to avoid excessive melting of the parent material, the steep rise stage is set to ensure the stability of welding. The purpose of the variable speed slow down stage is to fill the arc pit and avoid the generation of arc pit cracks. The variable speed slow down stage is to slowly reduce the power first and then quickly reduce the power.

[0060] The laser power P1 in the steep rise stage is 120% of the laser power P3 in the continuous stage;

[0061] S4. Weld one side of the workpiece by laser wire welding. After welding one side of the workpiece is completed, remove the workpiece from the welding assembly tooling, flip the workpiece and re-fix it on the welding assembly tooling, and weld the other side of the workpiece by laser wire welding until the welding of the other side of the workpiece is completed, and remove the workpiece from the welding assembly tooling;

[0062] Among them, the front wire feeding is adopted in the welding process, the shielding gas is located behind the welding point, and the wire is collected 100ms before the end of welding, which can avoid the unmelted welding wire in the weld and ensure that the welding wire at the end of the weld is completely melted at the end of welding;

[0063] The welding system used in this embodiment is as follows Figure 7As shown, it includes a shell 5, an optical fiber coupling device 6, a laser head 7, a weld monitoring unit 8, a shielding gas pipeline 9, a first shielding gas connecting plate 10, a second shielding gas connecting plate 11, a wire feeding hose 12 and a wire feeding tube connecting plate 13; the optical fiber coupling device 6 is arranged at the upper end of the shell 5, and is used to receive laser and transmit it to the laser head 7; the laser head 7 is arranged at the lower end of the shell 5, and the laser head 7 is used to emit welding laser; the weld monitoring unit 8 is arranged on one side of the shell 5, and the weld monitoring unit 8 is used to monitor the weld in real time; the shielding gas pipeline 9 is connected to the shell 5 through the second shielding gas connecting plate 11 and the first shielding gas connecting plate 10, and the shielding gas pipeline 9 is used to transport shielding gas, and the outlet of the shielding gas pipeline 9 is arranged above the weld; the wire feeding hose 12 is connected to the shell 5 through the wire feeding tube connecting plate 13, and the wire feeding hose 12 is used to transport welding wire to the weld molten pool;

[0064] This step also includes online monitoring of the weld. During the welding process, the weld monitoring unit 8 records the weld forming quality and signal fluctuation in real time, detects and analyzes the weld quality, and repairs unqualified positions.

[0065] S5. Perform visual inspection and penetrant inspection on the appearance of welds, and perform performance inspection on weld joints through tensile strength test and bending performance test.

[0066] Embodiment 3, this embodiment provides a method for welding a front longitudinal beam of a body-in-white, and welding is performed based on the welding assembly tooling and welding system mentioned in Embodiment 2, and specifically includes the following steps:

[0067] S1. Tool positioning: Fix the end stopper 2 and the base 1 of the welding assembly tool to the welding platform with bolts, use three-coordinate to check the positioning accuracy of the end stopper 2 and the base 1, fix the pneumatic clamping device 3 and the pneumatic clamping device 4 in the corresponding position, and ensure that there is enough space on both sides of the welding position, and leave at least 10mm margin from the edge of the clamping plate 3-1 to the weld to avoid interference and collision with the protective gas pipeline 9 and the wire feeding hose 12 of the welding system;

[0068] S2 loading: The first workpiece 14 and the second workpiece 15 of the front longitudinal beam workpiece are fitted with the end stopper 2 and the baffle 1-2, and the workpiece is fixed by the pneumatic clamping device 3 and the pneumatic clamping device 4;

[0069] S3. Welding: The welding method adopts laser wire welding, such as Figure 8 As shown, the welding direction is the direction pointed by the arrow. During the welding process, the front wire is fed and the shielding gas is located behind the welding point. At this time, the position of the shielding gas pipeline 9 needs to be adjusted through the second shielding gas connecting plate 11 to ensure that the central axis of the shielding gas pipeline 9 is coaxial with the center line of the weld.

[0070] In this embodiment, the front longitudinal beam workpiece is 3mm thick 6082 aluminum alloy, the weld length is 600mm, and the laser power P3 in the continuous stage is set to 6000W, the defocus is set to 4mm, the filament spacing is set to 2mm, the wire feeding speed is set to 4.5m / min, the welding speed is set to 3m / min, and the shielding gas flow rate is set to 20-35L / min;

[0071] The steep rise time t1 of the steep rise stage is set to 100ms, and the laser power P1 of the steep rise stage is set to 7200W; the uniform speed slow-down time t2 of the uniform speed slow-down stage is set to 300ms, the laser power P2 at the starting point of the uniform speed slow-down stage is set to 7200W, and the laser power P2' at the end point of the uniform speed slow-down stage is set to 6000W; the laser power P3 of the continuous stage is 6000W, and the continuous time t3 of the continuous stage is 11100ms; the variable speed slow-down time t4 at the end position of the weld is set to 500ms, the laser power P4 at the starting point of the variable speed slow-down stage is 6000W, and the laser power P4' at the end point of the variable speed slow-down stage is 0W;

[0072] The steep rise stage can be set to solve the problem of insufficient heat in the plate at the start of the weld, which is not conducive to the absorption of laser energy. The power is increased to melt the material and form a more stable laser keyhole. As the welding time increases, the temperature of the test plate gradually increases, and the absorption of laser power gradually increases. In order to avoid excessive melting of the parent material, the steep rise stage is set to ensure the stability of welding. The purpose of the variable speed slow down stage is to fill the arc pit and avoid the generation of arc pit cracks. The variable speed slow down stage is to slowly reduce the power first and then quickly reduce the power.

[0073] In order to avoid unmelted wire in the weld, a trigger signal is added to the wire feeding program to shut down the wire feeding 100ms in advance;

[0074] S4. Turn over the test piece: weld one side of the workpiece by laser wire welding. After the welding of one side of the workpiece is completed, loosen the pneumatic clamping device 3 and the pneumatic clamping device 4, turn the workpiece over, clamp and clamp it again, and then weld it. After the welding is completed, the entire workpiece production is completed, and the workpiece is removed from the welding assembly tooling;

[0075] During the welding process, the weld monitoring unit 8 will record the weld forming quality and signal fluctuation in real time, detect and analyze the weld quality, and repair the unqualified positions;

[0076] S5. Performance test: 3mm 6082-T6 aluminum alloy welded joint tensile strength test: base material tensile strength 315MPa, welded joint tensile strength 240MPa, welded joint strength reaches 76% of base material strength; bending performance test: select the bending angle of 180°, after positive bending and back bending tests, there is no opening defect on the weld surface. Fig. 9 As shown, the weld has good fusion at the starting position and no crater defect at the arc ending position.

[0077] Embodiment 4: This embodiment provides a method for welding a front longitudinal beam of a body-in-white, and welding is performed based on the welding assembly tooling and welding system mentioned in Embodiment 2, and specifically includes the following steps:

[0078] S1. Tool positioning: Fix the end stopper 2 and the base 1 of the welding assembly tool to the welding platform with bolts, use three-coordinate to check the positioning accuracy of the end stopper 2 and the base 1, fix the pneumatic clamping device 3 and the pneumatic clamping device 4 in the corresponding position, and ensure that there is enough space on both sides of the welding position, and leave at least 10mm margin from the edge of the clamping plate 3-1 to the weld to avoid interference and collision with the protective gas pipeline 9 and the wire feeding hose 12 of the welding system;

[0079] S2 loading: The first workpiece 14 and the second workpiece 15 of the front longitudinal beam workpiece are fitted with the end stopper 2 and the baffle 1-2, and the workpiece is fixed by the pneumatic clamping device 3 and the pneumatic clamping device 4;

[0080] S3. Welding: The welding method adopts laser wire welding, such as Figure 8 As shown, the welding direction is the direction pointed by the arrow. During the welding process, the front wire is fed and the shielding gas is located behind the welding point. At this time, the position of the shielding gas pipeline 9 needs to be adjusted through the second shielding gas connecting plate 11 to ensure that the central axis of the shielding gas pipeline 9 is coaxial with the center line of the weld.

[0081] In this embodiment, the front longitudinal beam workpiece is 3mm thick 6082 aluminum alloy, the weld length is 600mm, and the laser power P3 in the continuous stage is set to 5800W, the defocus is set to 4mm, the filament spacing is set to 2mm, the wire feeding speed is set to 4.5m / min, the welding speed is set to 3m / min, and the shielding gas flow rate is set to 20-35L / min;

[0082] The steep rise time t1 of the steep rise stage is set to 100ms, and the laser power P1 of the steep rise stage is set to 7000W; the uniform speed slowing down time t2 of the uniform speed slowing down stage is set to 300ms, the laser power P2 of the uniform speed slowing down starting point of the uniform speed slowing down stage is set to 6960W, and the laser power P2' of the uniform speed slowing down end point of the uniform speed slowing down stage is set to 5800W; the laser power P3 of the continuous stage is 5800W, and the continuous time t3 of the continuous stage is 11100ms; the variable speed slowing down time t4 of the end position of the weld is set to 500ms, the laser power P4 of the variable speed slowing down starting point of the variable speed slowing down stage is 5800W, and the laser power P4' of the variable speed slowing down end point of the variable speed slowing down stage is 0W;

[0083] The steep rise stage can be set to solve the problem of insufficient heat in the plate at the start of the weld, which is not conducive to the absorption of laser energy. The power is increased to melt the material and form a more stable laser keyhole. As the welding time increases, the temperature of the test plate gradually increases, and the absorption of laser power gradually increases. In order to avoid excessive melting of the parent material, the steep rise stage is set to ensure the stability of welding. The purpose of the variable speed slow down stage is to fill the arc pit and avoid the generation of arc pit cracks. The variable speed slow down stage is to slowly reduce the power first and then quickly reduce the power.

[0084] In order to avoid unmelted wire in the weld, a trigger signal is added to the wire feeding program to shut down the wire feeding 100ms in advance;

[0085] S4. Turn over the test piece: weld one side of the workpiece by laser wire welding. After the welding of one side of the workpiece is completed, loosen the pneumatic clamping device 3 and the pneumatic clamping device 4, turn the workpiece over, clamp and clamp it again, and then weld it. After the welding is completed, the entire workpiece production is completed, and the workpiece is removed from the welding assembly tooling;

[0086] During the welding process, the weld monitoring unit 8 will record the weld forming quality and signal fluctuation in real time, detect and analyze the weld quality, and repair the unqualified positions;

[0087] S5. Performance test: 3mm 6082-T6 aluminum alloy welded joint tensile strength test: base material tensile strength 315MPa, welded joint tensile strength 238MPa, welded joint strength reaches 75.5% of base material strength; Bending performance test: The bending angle is 180°, and after forward and backward bending tests, there are no opening defects on the weld surface.

[0088] Embodiment 5, this embodiment provides a method for welding a front longitudinal beam of a body-in-white, and welding is performed based on the welding assembly tooling and welding system mentioned in Embodiment 2, and specifically includes the following steps:

[0089] S1. Tool positioning: Fix the end stopper 2 and the base 1 of the welding assembly tool to the welding platform with bolts, use three-coordinate to check the positioning accuracy of the end stopper 2 and the base 1, fix the pneumatic clamping device 3 and the pneumatic clamping device 4 in the corresponding position, and ensure that there is enough space on both sides of the welding position, and leave at least 10mm margin from the edge of the clamping plate 3-1 to the weld to avoid interference and collision with the protective gas pipeline 9 and the wire feeding hose 12 of the welding system;

[0090] S2 loading: The first workpiece 14 and the second workpiece 15 of the front longitudinal beam workpiece are fitted with the end stopper 2 and the baffle 1-2, and the workpiece is fixed by the pneumatic clamping device 3 and the pneumatic clamping device 4;

[0091] S3. Welding: The welding method adopts laser wire welding, such as Figure 8 As shown, the welding direction is the direction pointed by the arrow. During the welding process, the front wire is fed and the shielding gas is located behind the welding point. At this time, the position of the shielding gas pipeline 9 needs to be adjusted through the second shielding gas connecting plate 11 to ensure that the central axis of the shielding gas pipeline 9 is coaxial with the center line of the weld.

[0092] In this embodiment, the front longitudinal beam workpiece is 3mm thick 6082 aluminum alloy, the weld length is 600mm, and the laser power P3 in the continuous stage is set to 6200W, the defocus is set to 4mm, the filament spacing is set to 2mm, the wire feeding speed is set to 4.5m / min, the welding speed is set to 3m / min, and the shielding gas flow rate is set to 20-35L / min;

[0093] The steep rise time t1 of the steep rise stage is set to 100ms, and the laser power P1 of the steep rise stage is set to 7440W; the uniform speed slow-down time t2 of the uniform speed slow-down stage is set to 300ms, the laser power P2 of the uniform speed slow-down starting point of the uniform speed slow-down stage is set to 7440W, and the laser power P2' of the uniform speed slow-down end point of the uniform speed slow-down stage is set to 6200W; the laser power P3 of the continuous stage is 6200W, and the continuous time t3 of the continuous stage is 11100ms; the variable speed slow-down time t4 of the end position of the weld is set to 500ms, the laser power P4 of the variable speed slow-down starting point of the variable speed slow-down stage is 6200W, and the laser power P4' of the variable speed slow-down end point of the variable speed slow-down stage is 0W;

[0094] The steep rise stage can be set to solve the problem of insufficient heat in the plate at the start of the weld, which is not conducive to the absorption of laser energy. The power is increased to melt the material and form a more stable laser keyhole. As the welding time increases, the temperature of the test plate gradually increases, and the absorption of laser power gradually increases. In order to avoid excessive melting of the parent material, the steep rise stage is set to ensure the stability of welding. The purpose of the variable speed slow down stage is to fill the arc pit and avoid the generation of arc pit cracks. The variable speed slow down stage is to slowly reduce the power first and then quickly reduce the power.

[0095] In order to avoid unmelted wire in the weld, a trigger signal is added to the wire feeding program to shut down the wire feeding 100ms in advance;

[0096] S4. Turn over the test piece: weld one side of the workpiece by laser wire welding. After the welding of one side of the workpiece is completed, loosen the pneumatic clamping device 3 and the pneumatic clamping device 4, turn the workpiece over, clamp and clamp it again, and then weld it. After the welding is completed, the entire workpiece production is completed, and the workpiece is removed from the welding assembly tooling;

[0097] During the welding process, the weld monitoring unit 8 will record the weld forming quality and signal fluctuation in real time, detect and analyze the weld quality, and repair the unqualified positions;

[0098] S5. Performance test: 3mm 6082-T6 aluminum alloy welded joint tensile strength test: base material tensile strength 315MPa, welded joint tensile strength 242MPa, welded joint strength reaches 75.2% of base material strength; Bending performance test: The bending angle is 180°, and after forward and backward bending tests, there are no opening defects on the weld surface.

[0099] Comparative Example 1: This comparative example uses the welding assembly tooling and welding system used in Example 3 for welding. The difference from Example 3 is that the welding waveform of this comparative example adopts continuous laser welding without steep rise, uniform speed slow fall, or variable speed slow fall waveform. The welding waveform is as follows: Fig.10 As shown, the specific steps include:

[0100] S1. Tool positioning: Fix the end stopper 2 and the base 1 of the welding assembly tool to the welding platform with bolts, use three-coordinate to check the positioning accuracy of the end stopper 2 and the base 1, fix the pneumatic clamping device 3 and the pneumatic clamping device 4 in the corresponding position, and ensure that there is enough space on both sides of the welding position, and leave at least 10mm margin from the edge of the clamping plate 3-1 to the weld to avoid interference and collision with the protective gas pipeline 9 and the wire feeding hose 12 of the welding system;

[0101] S2 loading: The first workpiece 14 and the second workpiece 15 of the front longitudinal beam workpiece are fitted with the end stopper 2 and the baffle 1-2, and the workpiece is fixed by the pneumatic clamping device 3 and the pneumatic clamping device 4;

[0102] S3. Welding: The welding method adopts laser wire welding, and the front wire feeding is adopted during the welding process. The shielding gas is located behind the welding point. At this time, the position of the shielding gas pipeline 9 needs to be adjusted through the second shielding gas connecting plate 11 to ensure that the central axis of the shielding gas pipeline 9 is coaxial with the center line of the weld;

[0103] In this comparative example, the front longitudinal beam workpiece is 6082 aluminum alloy with a wall thickness of 3mm and a weld length of 600mm. At this time, the continuous welding laser power is set to 6000W, the defocus amount is set to 4mm, the light wire spacing is set to 2mm, the wire feeding speed is set to 4.5m / min, the welding speed is set to 3m / min, and the shielding gas flow rate is set to 20-35L / min.

[0104] In order to avoid unmelted wire in the weld, a trigger signal is added to the wire feeding program to turn off the wire feeding signal 100ms in advance;

[0105] S4. Turn over the test piece: weld one side of the workpiece by laser wire welding. After the welding of one side of the workpiece is completed, loosen the pneumatic clamping device 3 and the pneumatic clamping device 4, turn the workpiece over, clamp and clamp it again, and then weld it. After the welding is completed, the entire workpiece production is completed, and the workpiece is removed from the welding assembly tooling;

[0106] During the welding process, the weld monitoring unit 8 will record the weld forming quality and signal fluctuation in real time, detect and analyze the weld quality, and repair the unqualified positions;

[0107] S5. Performance test: 3mm 6082-T6 aluminum alloy welded joint tensile strength test: the base material tensile strength is 315MPa, the welded joint tensile strength is 225.5MPa, and the welded joint strength reaches 71.5% of the base material strength; Fig.11 As shown, the weld is not melted at the beginning and has arc crater cracks, which affects its performance.

[0108] Comparative Example 2: This comparative example uses the welding assembly tooling used in Example 3 for welding. The difference from Example 3 is that this comparative example uses stir friction welding for welding, which specifically includes the following steps:

[0109] S1. Tool positioning: Fix the end stopper 2 and base 1 of the welding assembly tool on the welding platform with bolts, use three-coordinate to check the positioning accuracy of the end stopper 2 and base 1, fix the pneumatic clamping device 3 and the pneumatic jacking device 4 in the corresponding positions, and ensure that there is enough space on both sides of the welding position, and leave at least 10mm margin from the edge of the clamping plate 3-1 to the weld to avoid interference and collision with the stirring welding device;

[0110] S2 loading: The first workpiece 14 and the second workpiece 15 of the front longitudinal beam workpiece are fitted with the end stopper 2 and the baffle 1-2, and the workpiece is fixed by the pneumatic clamping device 3 and the pneumatic clamping device 4;

[0111] S3. Welding: The welding method adopts friction stir welding. In this comparative example, the front longitudinal beam workpiece is a 3mm thick 6082 aluminum alloy, the weld length is 600mm, and the welding speed is 0.7m / min;

[0112] S4. Turn over the test piece: weld one side of the workpiece by laser wire welding. After the welding of one side of the workpiece is completed, loosen the pneumatic clamping device 3 and the pneumatic clamping device 4, turn the workpiece over, clamp and clamp it again, and then weld it. After the welding is completed, the entire workpiece production is completed, and the workpiece is removed from the welding assembly tooling;

[0113] During the welding process, the weld monitoring unit 8 will record the weld forming quality and signal fluctuation in real time, detect and analyze the weld quality, and repair the unqualified positions;

[0114] S5. Performance test: 3mm 6082-T6 aluminum alloy welded joint tensile strength test: the base material tensile strength is 315MPa, the welded joint tensile strength is 223.65MPa, the welded joint strength reaches 71% of the base material strength, but there is a stir friction welding keyhole, the keyhole needs to be repaired, and the welded joint strength is lower than the welded joint strength that can be achieved by the technical solution of the present invention.

[0115] Comparative Example 3: This comparative example uses the welding assembly tooling used in Example 3 for welding. The difference from Example 3 is that this comparative example uses MIG welding for welding, and specifically includes the following steps:

[0116] S1. Tool positioning: Fix the end stopper 2 and base 1 of the welding assembly tool on the welding platform with bolts, use three-coordinate to check the positioning accuracy of the end stopper 2 and base 1, fix the pneumatic clamping device 3 and the pneumatic jacking device 4 in the corresponding position, and ensure that there is enough space on both sides of the welding position, and leave at least 10mm margin from the edge of the clamping plate 3-1 to the weld to avoid interference and collision with the MIG welding device;

[0117] S2 loading: The first workpiece 14 and the second workpiece 15 of the front longitudinal beam workpiece are fitted with the end stopper 2 and the baffle 1-2, and the workpiece is fixed by the pneumatic clamping device 3 and the pneumatic clamping device 4;

[0118] S3. Welding: The welding method is MIG welding. In this comparative example, the front longitudinal beam workpiece is 3mm thick 6082 aluminum alloy, the weld length is 600mm, and the welding speed is 0.35m / min;

[0119] S4. Turn over the test piece: weld one side of the workpiece by laser wire welding. After the welding of one side of the workpiece is completed, loosen the pneumatic clamping device 3 and the pneumatic clamping device 4, turn the workpiece over, clamp and clamp it again, and then weld it. After the welding is completed, the entire workpiece production is completed, and the workpiece is removed from the welding assembly tooling;

[0120] During the welding process, the weld monitoring unit 8 will record the weld forming quality and signal fluctuation in real time, detect and analyze the weld quality, and repair the unqualified positions;

[0121] S5. Performance test: 3mm 6082-T6 aluminum alloy welded joint tensile strength test: the base material tensile strength is 315MPa, the welded joint tensile strength is 198.45MPa, and the welded joint strength reaches 63% of the base material strength. It can be seen that the strength of the welded joint using MIG welding is much lower than the welding strength that can be obtained by the present invention.

[0122] Comparative Example 4: This comparative example uses the welding assembly tooling and welding system used in Example 3 for welding. The difference from Example 3 is that the welding waveform of this comparative example adopts welding without a steep rise stage, without a uniform slow-down stage, and a uniform slow-down waveform is used at the arc closing position. The welding waveform is as follows: Fig.12 As shown, the specific steps include:

[0123] S1. Tool positioning: Fix the end stopper 2 and the base 1 of the welding assembly tool to the welding platform with bolts, use three-coordinate to check the positioning accuracy of the end stopper 2 and the base 1, fix the pneumatic clamping device 3 and the pneumatic clamping device 4 in the corresponding position, and ensure that there is enough space on both sides of the welding position, and leave at least 10mm margin from the edge of the clamping plate 3-1 to the weld to avoid interference and collision with the protective gas pipeline 9 and the wire feeding hose 12 of the welding system;

[0124] S2 loading: The first workpiece 14 and the second workpiece 15 of the front longitudinal beam workpiece are fitted with the end stopper 2 and the baffle 1-2, and the workpiece is fixed by the pneumatic clamping device 3 and the pneumatic clamping device 4;

[0125] S3. Welding: The welding method adopts laser wire welding, and the front wire feeding is adopted during the welding process. The shielding gas is located behind the welding point. At this time, the position of the shielding gas pipeline 9 needs to be adjusted through the second shielding gas connecting plate 11 to ensure that the central axis of the shielding gas pipeline 9 is coaxial with the center line of the weld;

[0126] In this comparative example, the front longitudinal beam workpiece is 3mm thick 6082 aluminum alloy, the weld length is 600mm, and the continuous welding laser power is set to 6000W, the defocus is set to 4mm, the wire spacing is set to 2mm, the wire feeding speed is set to 4.5m / min, the welding speed is set to 3m / min, and the shielding gas flow is set to 20-35L / min;

[0127] In order to avoid unmelted wire in the weld, a trigger signal is added to the wire feeding program to turn off the wire feeding signal 100ms in advance;

[0128] S4. Turn over the test piece: weld one side of the workpiece by laser wire welding. After the welding of one side of the workpiece is completed, loosen the pneumatic clamping device 3 and the pneumatic clamping device 4, turn the workpiece over, clamp and clamp it again, and then weld it. After the welding is completed, the entire workpiece production is completed, and the workpiece is removed from the welding assembly tooling;

[0129] During the welding process, the weld monitoring unit 8 will record the weld forming quality and signal fluctuation in real time, detect and analyze the weld quality, and repair the unqualified positions;

[0130] S5. Performance test: 3mm 6082-T6 aluminum alloy welded joint tensile strength test: base material tensile strength is 315MPa, welded joint tensile strength is 228MPa, welded joint strength reaches 72.3% of base material strength, when arc ending position is a uniform speed slow-down waveform, welded joint strength is lower than arc ending position variable speed slow-down waveform stage welded joint strength.

[0131] Comparative Example 5: This comparative example uses the welding assembly tooling and welding system used in Example 3 for welding. The difference from Example 3 is that the welding waveform of this comparative example uses a waveform with a steep rise stage, no uniform speed slow-down stage, and a variable speed slow-down stage for welding. The welding waveform is as follows: Fig.13 As shown, the specific steps include:

[0132] S1. Tool positioning: Fix the end stopper 2 and the base 1 of the welding assembly tool to the welding platform with bolts, use three-coordinate to check the positioning accuracy of the end stopper 2 and the base 1, fix the pneumatic clamping device 3 and the pneumatic clamping device 4 in the corresponding position, and ensure that there is enough space on both sides of the welding position, and leave at least 10mm margin from the edge of the clamping plate 3-1 to the weld to avoid interference and collision with the protective gas pipeline 9 and the wire feeding hose 12 of the welding system;

[0133] S2 loading: The first workpiece 14 and the second workpiece 15 of the front longitudinal beam workpiece are fitted with the end stopper 2 and the baffle 1-2, and the workpiece is fixed by the pneumatic clamping device 3 and the pneumatic clamping device 4;

[0134] S3. Welding: The welding method adopts laser wire welding, and the front wire feeding is adopted during the welding process. The shielding gas is located behind the welding point. At this time, the position of the shielding gas pipeline 9 needs to be adjusted through the second shielding gas connecting plate 11 to ensure that the central axis of the shielding gas pipeline 9 is coaxial with the center line of the weld;

[0135] In this comparative example, the front longitudinal beam workpiece is 6082 aluminum alloy with a wall thickness of 3mm and a weld length of 600mm. At this time, the continuous welding laser power is set to 6000W, the defocus amount is set to 4mm, the light wire spacing is set to 2mm, the wire feeding speed is set to 4.5m / min, the welding speed is set to 3m / min, and the shielding gas flow rate is set to 20-35L / min.

[0136] In order to avoid unmelted wire in the weld, a trigger signal is added to the wire feeding program to turn off the wire feeding signal 100ms in advance;

[0137] S4. Turn over the test piece: weld one side of the workpiece by laser wire welding. After the welding of one side of the workpiece is completed, loosen the pneumatic clamping device 3 and the pneumatic clamping device 4, turn the workpiece over, clamp and clamp it again, and then weld it. After the welding is completed, the entire workpiece production is completed, and the workpiece is removed from the welding assembly tooling;

[0138] During the welding process, the weld monitoring unit 8 will record the weld forming quality and signal fluctuation in real time, detect and analyze the weld quality, and repair the unqualified positions;

[0139] S5. Performance test: 3mm 6082-T6 aluminum alloy welded joint tensile strength test: the base material tensile strength is 315MPa, the welded joint tensile strength is 225MPa, the welded joint strength reaches 71.4% of the base material strength, and the strength of the welded joint welded without the uniform slow-down stage waveform is lower than the strength of the welded joint with the uniform slow-down stage waveform.

[0140] Comparative Example 6: This comparative example uses the welding assembly tooling and welding system used in Example 3 for welding. The difference from Example 3 is that the welding waveform of this comparative example uses a steep rise phase, a uniform speed slow fall phase, but no variable speed slow fall phase steep rise waveform for welding. The welding waveform is as follows: Fig.14 As shown, the specific steps include:

[0141] S1. Tool positioning: Fix the end stopper 2 and the base 1 of the welding assembly tool to the welding platform with bolts, use three-coordinate to check the positioning accuracy of the end stopper 2 and the base 1, fix the pneumatic clamping device 3 and the pneumatic clamping device 4 in the corresponding position, and ensure that there is enough space on both sides of the welding position, and leave at least 10mm margin from the edge of the clamping plate 3-1 to the weld to avoid interference and collision with the protective gas pipeline 9 and the wire feeding hose 12 of the welding system;

[0142] S2 loading: The first workpiece 14 and the second workpiece 15 of the front longitudinal beam workpiece are fitted with the end stopper 2 and the baffle 1-2, and the workpiece is fixed by the pneumatic clamping device 3 and the pneumatic clamping device 4;

[0143] S3. Welding: The welding method adopts laser wire welding, and the front wire feeding is adopted during the welding process. The shielding gas is located behind the welding point. At this time, the position of the shielding gas pipeline 9 needs to be adjusted through the second shielding gas connecting plate 11 to ensure that the central axis of the shielding gas pipeline 9 is coaxial with the center line of the weld;

[0144] In this embodiment, the front longitudinal beam workpiece is 3mm thick 6082 aluminum alloy and the weld length is 600mm. At this time, the continuous welding laser power is set to 6000W, the defocus amount is set to 4mm, the light wire spacing is set to 2mm, the wire feeding speed is set to 4.5m / min, the welding speed is set to 3m / min, and the shielding gas flow rate is set to 20-35L / min.

[0145] In order to avoid unmelted wire in the weld, a trigger signal is added to the wire feeding program to turn off the wire feeding signal 100ms in advance;

[0146] S4. Turn over the test piece: weld one side of the workpiece by laser wire welding. After the welding of one side of the workpiece is completed, loosen the pneumatic clamping device 3 and the pneumatic clamping device 4, turn the workpiece over, clamp and clamp it again, and then weld it. After the welding is completed, the entire workpiece production is completed, and the workpiece is removed from the welding assembly tooling;

[0147] During the welding process, the weld monitoring unit 8 will record the weld forming quality and signal fluctuation in real time, detect and analyze the weld quality, and repair the unqualified positions;

[0148] S5. Performance test: 3mm 6082-T6 aluminum alloy welded joint tensile strength test: the base material tensile strength is 315MPa, the welded joint tensile strength is 230.5MPa, the welded joint strength reaches 73% of the base material strength, and the welded joint strength is lower than the welded joint strength obtained by the technical solution provided by the present invention.

[0149] The welding waveform designed by the present invention has a good surface forming after welding and no arc pit defects. The strength of the welded joint is greatly improved compared with stir friction welding and MIG welding, and the welding speed is also greatly improved. The present invention has greatly improved production efficiency while improving product quality.

[0150] The embodiments of the present invention are given for the purpose of illustration and description, and are not intended to be exhaustive or to limit the invention to the disclosed forms. Many modifications and variations will be apparent to those of ordinary skill in the art. The embodiments are selected and described in order to better illustrate the principles and practical applications of the present invention and to enable those of ordinary skill in the art to understand the present invention and thereby design various embodiments with various modifications suitable for specific uses.

Claims

1. A method for welding a front longitudinal beam of a body in white, characterized in that: The steps include: S1. Position the welding assembly tooling; S2. Fixing the workpiece on the welding assembly tooling; S3. Setting the welding system, determining the welding parameters and welding waveform, wherein the welding waveform is a steep rise-constant speed slow fall-continuous-variable speed slow fall waveform; S4. Weld one side of the workpiece by laser wire welding. After welding one side of the workpiece is completed, remove the workpiece from the welding assembly tooling, flip the workpiece and re-fix it on the welding assembly tooling, weld the other side of the workpiece by laser wire welding until the welding of the other side of the workpiece is completed, and remove the workpiece from the welding assembly tooling; S5. Perform visual inspection and penetration testing on the welds, and perform performance testing on the welded joints by tensile strength testing and bending performance testing.

2. A method for welding a front longitudinal beam of a body-in-white according to claim 1, characterized in that: The welding assembly tool comprises a base (1), an end stop block (2), four pneumatic clamping devices (3) and two pneumatic jacking devices (4); The base (1) is used to support a workpiece, a welding groove (1-1) is provided on the upper surface of the base (1), the welding groove (1-1) is used to reserve space for the excess height of the weld, and a baffle (1-2) is provided on the upper surface of the base (1), the baffle (1-2) is in contact with one side of the workpiece; The end limit block (2) is arranged on the front side of the base (1) and is used to limit the workpiece in the X direction; The four pneumatic clamping devices (3) are respectively arranged on the left and right sides of the base (1), and the pneumatic clamping device (3) comprises a clamping plate (3-1). The clamping plate (3-1) is arranged above the workpiece, and the clamping plate (3-1) is used to cooperate with the base (1) to limit the workpiece in the Y direction; The two pneumatic jacking devices (4) are arranged on a side of the base (1) away from the baffle (1-2), and the pneumatic jacking device (4) comprises a jacking rod (4-1), the jacking rod (4-1) is in contact with the other side of the workpiece, and the jacking rod (4-1) is used to cooperate with the baffle (1-2) to limit the workpiece in the Z direction.

3. A method for welding a front longitudinal beam of a body-in-white according to claim 1, characterized in that: In the step S3, the welding parameters include wire feeding speed, welding speed, defocus, filament spacing, laser incident angle and shielding gas flow rate, the wire feeding speed is 4-6 m / min, the welding speed is 3-5 m / min, the defocus is 0-8 mm, the filament spacing is 0-2 mm, the laser incident angle is 5-10°, and the shielding gas flow rate is 20-35 L / min.

4. A method for welding a front longitudinal beam of a body-in-white according to claim 1, characterized in that: The steep rise-uniform speed descent-continuous-variable speed descent waveform includes a steep rise stage, a uniform speed descent stage, a continuous stage and a variable speed descent stage. The welding in the steep rise stage, the uniform speed descent stage and the variable speed descent stage all adopts pulsed laser wire welding, and the welding in the continuous stage adopts continuous laser wire welding.

5. The method for welding a front longitudinal beam of a body-in-white according to claim 1, characterized in that: The steep rise time t1 of the steep rise stage is 100ms~150ms, and the laser power P1 of the steep rise stage is 7000W~7500W; the uniform speed slowing down time t2 of the uniform speed slowing down stage is 300ms~500ms, the laser power P2 at the starting point of the uniform speed slowing down stage is 7000W~7500W, and the laser power P2' at the end point of the uniform speed slowing down stage is 5800W~6200W; the continuous time t3 of the continuous stage is ttotal-t1-t2-t4, and the laser power P3 of the continuous stage is 5800W~6200W; the variable speed slowing down time t4 of the variable speed slowing down stage is 500ms~750ms, the laser power P4 at the starting point of the variable speed slowing down stage is 5800W~6200W, and the laser power P4' at the end point of the variable speed slowing down stage is 0W.

6. A method for welding a front longitudinal beam of a body-in-white according to claim 5, characterized in that: The ratio of the steep rise time t1, the uniform speed slow-down time t2 and the variable speed slow-down time t4 is 1:3:

5.

7. A method for welding a front longitudinal beam of a body-in-white according to claim 5, characterized in that: The laser power P1 in the steep rise stage is 120% of the laser power P3 in the continuous stage.

8. The method for welding a front longitudinal beam of a body-in-white according to claim 1, characterized in that: In step S4, the wire is fed in advance during welding, the shielding gas is located behind the welding point, and the wire is collected 100ms before the end of welding.

9. A method for welding a front longitudinal beam of a body-in-white according to claim 1, characterized in that: The welding system comprises a housing (5), an optical fiber coupling device (6), a laser head (7), a weld monitoring unit (8), a shielding gas pipeline (9), a first shielding gas connection plate (10), a second shielding gas connection plate (11), a wire feeding hose (12) and a wire feeding tube connection plate (13); The optical fiber coupling device (6) is arranged at the upper end of the housing (5) and is used to receive laser light and transmit it to the laser head (7); The laser head (7) is arranged at the lower end of the housing (5), and the laser head (7) is used to emit welding laser; The weld monitoring unit (8) is arranged on one side of the shell (5), and the weld monitoring unit (8) is used to monitor the weld in real time; The shielding gas pipeline (9) is connected to the housing (5) via the second shielding gas connection plate (11) and the first shielding gas connection plate (10), the shielding gas pipeline (9) is used to transport shielding gas, and the outlet of the shielding gas pipeline (9) is arranged above the weld; The wire feeding hose (12) is connected to the housing (5) via the wire feeding tube connecting plate (13), and the wire feeding hose (12) is used to feed welding wire to the weld pool.

10. A method for welding a front longitudinal beam of a body-in-white according to claim 9, characterized in that: The step S4 also includes online monitoring of the weld, in which the weld forming quality and signal fluctuation are recorded in real time by the weld monitoring unit (8) during the welding process, the weld quality is detected and analyzed, and unqualified positions are repaired.