Repair process for active diffusion brazing of cobalt-based high-temperature alloy nozzle

Through the active diffusion brazing process of cobalt-based high-temperature alloy nozzles, the problems of the expansion of heat-affected zones and corrosion resistance damage when repairing cobalt-based high-temperature alloy components are solved, achieving a more efficient and accurate repair effect, and extending the Equipment lifespan and reduce maintenance costs.

CN119017005APending Publication Date: 2024-11-26HUARUI (JIANGSU) GAS TURBINE SERVICE CO LTD

Patent Information

Application Number
CN202411204542.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Traditional argon arc welding and brazing methods are difficult to accurately control the welding process, resulting in the expansion of the heat-affected zone, which damages the mechanical properties and corrosion resistance of cobalt-based high-temperature alloy components, and cannot meet the stability and durability requirements in harsh environments, especially in The strength requirements cannot be met when repairing large areas of cracks.

Method used

Adopt active diffusion brazing process of cobalt-based high-temperature alloy nozzles, including removal of accessories, cleaning of surfaces, sandblasting, brazing injection and heating treatment, and achieve more efficient and accurate repair through specific steps and material preparation, including the use of oxidation Aluminum cleaning, hydrogen fluoride flushing, nickel sandblasting, brazing spraying and temperature control ensure uniform heat treatment and vacuum environment.

Benefits of technology

The strength of the repaired parts reaches more than 92% of the raw material, effectively extending the service life of the equipment, reducing maintenance costs, and improving repair efficiency. It overcomes the shortcomings of traditional welding methods and achieves a more efficient repair effect.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a cobalt-based high-temperature alloy nozzle active diffusion brazing repair process, which comprises the following steps of: firstly, cutting off a connecting weld joint by using a cutting blade, then mounting an inner edge plate, an outer edge plate, an inner edge plate and an outer edge plate on a shape correcting tool, and cleaning the nozzle by using aluminum oxide to remove surface oxides; continuously flushing with hydrogen fluoride, and annealing in a furnace; the nozzle is taken out of the furnace, and nickel sand is used for conducting nickel sand blasting on the to-be-brazed surface; then the nozzle is transferred to a brazing room, a needle tube is used for injecting a solder resist into all cooling holes of the nozzle, injection is conducted from the holes to the brazing face, and injection is stopped at the position 0.3-0.5 mm away from the surface; the prepared brazing material is evenly sprayed to the to-be-brazed surface of the nozzle, the sprayed nozzle is loaded into a brazing furnace, vacuumizing is carried out, then heating and cooling are carried out for multiple times, and finally cooling is carried out to achieve repairing. According to the technology, the heat channel component of the gas turbine can be repaired more efficiently and more accurately, and the defects in the prior art, such as heat affected zone expansion, mechanical property and corrosion resistance damage, residual stress and deformation, are overcome.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a repair process of active diffusion brazing of a cobalt-based high-temperature alloy nozzle, belonging to the technical field of heavy-duty gas turbine maintenance. Background Art

[0002] As a material for gas turbine hot channel, cobalt-based superalloys work in extremely harsh environments, and components must withstand multiple effects such as high temperature, thermal cycle fatigue, impact, and thermal fatigue. Although this cobalt-based superalloy has excellent high-temperature performance, long-term operation under such harsh conditions will inevitably lead to performance degradation, among which cracking and large-area cracking caused by thermal fatigue are particularly common.

[0003] The traditional argon arc welding repair method is only suitable for repairing a small number of cracks and defects. It is difficult to accurately control the heat input during a large number of welding processes, which can easily lead to the expansion of the heat-affected zone, thereby damaging the mechanical properties and corrosion resistance of the turbine components. In addition, the ordinary brazing method is only suitable for repairing local microcracks. The repair of large-area cracks cannot meet the strength requirements after repair, and cannot ensure the stability and durability of the components in harsh working environments. Summary of the invention

[0004] In view of the problems existing in the above-mentioned prior art, the present invention provides a repair process for active diffusion brazing of cobalt-based high-temperature alloy nozzles, so that the hot channel components of gas turbines can be repaired more efficiently and accurately.

[0005] In order to achieve the above-mentioned object, the technical solution adopted by the present invention is: a repair process of active diffusion brazing of a cobalt-based high-temperature alloy nozzle, characterized in that it comprises the following steps;

[0006] Step S1: Use a cutting blade with a thickness of ≤1mm to cut off the connecting welds between the cooling cover plate, cooling core and other accessories and the outer edge plate of the nozzle, and remove all accessories; calibrate the floating sealing grooves of the inner and outer edge plates, install the inner and outer edge plates to the calibration tooling in a specific posture, and adjust the inner and outer edge plates respectively; use aluminum oxide to clean the entire nozzle to remove surface oxides;

[0007] Step S2: Load the nozzle into the reactor of the FIC equipment, fix the front edge of the nozzle toward the gas purge direction using a tool, continuously flush with hydrogen fluoride, and then anneal in the furnace; then take out the nozzle from the furnace, use 80 mesh nickel sand to nickel blast the surface to be brazed, and the spray gun is at an angle of 60 degrees to the sandblasted surface to obtain a clean and rough surface;

[0008] Step S3: After completing the previous operation, within 4 hours, transfer the nozzle to the brazing room, use a 0.8mm needle to inject solder resist into all cooling holes of the nozzle, inject from the inside of the hole to the brazing surface, and stop at 0.3-0.5mm away from the surface; the solder resist at the edge of the hole is full, and no gaps should be left;

[0009] Step S4: prepare the solder, add an appropriate amount of acetone and mix thoroughly;

[0010] Step S5: Spray the prepared brazing solder uniformly onto the surface of the nozzle to be brazed at a distance of 15 to 20 cm from the nozzle surface. For areas with more cracks, spray repeatedly after the surface is dried and solidified each time. Load the sprayed nozzle into the brazing furnace, evacuate it, and then heat it to a certain temperature to react and fully decompose the S glue.

[0011] Step S6: then heating to 1100°C at a heating rate of 8-14°C and maintaining at 1100°C for 40 minutes, the overall temperature of the nozzle is uniform at this temperature, then heating to 1180°C at a heating rate of 8-14°C and maintaining at this temperature for 30 minutes; then cooling to 1150°C in the furnace and maintaining at this temperature for 4 hours; then heating to 1180°C at a heating rate of 8-14°C and maintaining for 4 hours, then heating to 1200°C at a heating rate of 8-14°C and maintaining for 4 hours;

[0012] Step S7: After the temperature adjustment reaction, argon gas is introduced to cool to room temperature, and a 200-mesh sand belt is used to polish from the leading edge to the trailing edge of the nozzle blade to remove excess brazing material and restore the original profile;

[0013] Step S8: EDM to open the cooling holes blocked by brazing, using 0.8 mm, 1.2 mm, and 1.5 mm wire diameter electrodes;

[0014] Step S9: Perform fluorescent penetrant inspection and visual inspection on the parts after diffusion brazing. If cracks or surface defects are found during the visual inspection, repeat steps S2-S7 to repair the defects.

[0015] Furthermore, in step S1, the surface oxide is removed, and the entire nozzle is cleaned using 220 mesh alumina with a purity greater than 98% at a pressure of 6 Bar.

[0016] Furthermore, in step S2, hydrogen fluoride is used for continuous flushing at 1020° C. for at least 60 minutes, followed by furnace annealing.

[0017] Furthermore, in step S4, the solder is prepared by using A powder with components of Cr: 22.0, Ni: 8.0, W: 7.0, Ta: 3.5, Ti: 0.2, Zr: 0.5 and B powder with components of Cr: 22.5, Ni: 10.0, W: 7.0, Ta: 3.5, Ti: 0.2, Zr: 0.5, B: 4.0 and S glue in a weight ratio of 6:5:1.

[0018] Furthermore, in step S5, the sprayed nozzle is loaded into the brazing furnace and evacuated to ensure that the vacuum degree of the furnace is better than 5x10 -4 torr; heat up to 450℃ at a heating rate of 8~14℃ and keep at 450℃ for 40 minutes to allow the S glue to fully decompose. Before heating to the next temperature stage, ensure that the vacuum degree in the furnace returns to 5x10 -3 torr.

[0019] The beneficial effects of the present invention are:

[0020] (1) The present invention describes a process for active diffusion repair of cobalt-based high-temperature alloy nozzles. After repair, the strength of the component reaches more than 92% of the strength of the raw material. The raw material has a strength of 295 MPa at a high temperature of 870°C, and after repair, it reaches 275 MPa. After repair, a cycle can continue for 48,000 hours. This effectively extends the service life of the equipment and reduces maintenance costs.

[0021] (2) Compared with traditional welding, brazing in the present invention can be operated in batches, and the repair efficiency is increased by 50%. DETAILED DESCRIPTION

[0022] In order to make the purpose, technical scheme and advantages of the present invention more clear, the present invention is further described in detail by examples below. However, it should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the scope of the present invention.

[0023] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which the present invention belongs. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0024] In this embodiment, a cutting blade with a thickness of ≤1mm is used to cut off the connecting welds between the cooling cover plate, cooling core and other accessories and the outer edge plate of the nozzle, and all accessories are removed. The inner and outer edge plates are shaped by floating sealing grooves, and the inner and outer edge plates are installed in a specific posture to the shaping tooling, and the inner and outer edge plates are adjusted to R710mm and R844mm respectively. Use 220 mesh alumina with a purity greater than 98% to clean the entire nozzle at a pressure of 6Bar to remove surface oxides. Load the nozzle into the reactor of the FIC equipment, use the tooling to fix the front edge of the nozzle in the direction of gas purge, use hydrogen fluoride to continuously flush for at least 60 minutes at 1020°C, and then anneal in the furnace. Take out the nozzle from the furnace, use 80 mesh nickel sand to nickel blast the surface to be brazed, and the spray gun is at an angle of 60 degrees to the sandblasted surface to obtain a clean and rough surface.

[0025] After completing the above operation, within 4 hours, transfer the nozzle to the brazing room, use a 0.8mm needle to inject solder resist into all cooling holes of the nozzle, inject from the hole to the brazing surface, and stop at 0.3-0.5mm from the surface. The solder resist inside the hole edge is full and no gaps should be left.

[0026] Use A powder with components of Cr22.0Ni8.0W7.0Ta3.5Ti0.2Zr0.5 and B powder with components of Cr22.5Ni10.0W7.0Ta3.5Ti0.2Zr0.5B4.0 plus S glue in a weight ratio of 6:5:1 to prepare solder, and add appropriate amount of acetone to mix thoroughly.

[0027] Spray the prepared brazing solder evenly onto the surface to be brazed at a distance of 15 to 20 cm from the nozzle surface. For areas with many cracks, spray repeatedly after the surface is dry and solidified each time.

[0028] Load the sprayed nozzle into the brazing furnace and evacuate the furnace to ensure that the vacuum degree of the furnace is better than 5x10 -4 torr. Raise the temperature to 450°C at a heating rate of 8-14°C and keep it at 450°C for 40 minutes to allow the S glue to fully decompose. Before raising the temperature to the next temperature stage, ensure that the vacuum in the furnace returns to 5x10 -3 torr. Heating rate of 8-14℃ to 1100℃, and keep at 1100℃ for 40 minutes, the whole nozzle reaches uniform temperature at this temperature. Heating rate of 8-14℃ to 1180℃, keep at this temperature for 30 minutes. Cool to 1150℃ in the furnace, keep at this temperature for 4 hours. Heating rate of 8-14℃ to 1180℃ and keep at this temperature for 4 hours. Heating rate of 8-14℃ to 1200℃ and keep at this temperature for 4 hours. Cool to room temperature by argon.

[0029] Use 200-grit abrasive belt to polish from the leading edge to the trailing edge of the nozzle blade to remove excess brazing material and restore the original contour. EDM to open the cooling holes blocked by brazing, using 0.8mm, 1.2mm, and 1.5mm wire diameter electrodes. Fluorescent penetrant inspection and visual inspection to check the parts after diffusion brazing. If cracks or surface defects are found during visual inspection, repeat steps 5-17 to repair the defects.

[0030] The invention provides an advanced repair technology that can repair gas turbine hot channel components more efficiently and accurately, overcoming the shortcomings of existing technologies, such as expansion of heat-affected zones, damage to mechanical properties and corrosion resistance, residual stress and deformation problems, etc.

[0031] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A repair process for active diffusion brazing of a cobalt-based high-temperature alloy nozzle, characterized in that: The steps include: Step S1: Use a cutting blade with a thickness of ≤1 mm to cut off the connecting welds between the cooling cover plate, cooling core and other accessories and the outer edge plate of the nozzle, and remove all accessories; Correct the shape of the floating sealing groove of the inner and outer edge plates. Install the inner and outer edge plates to the correction tooling in a specific posture and adjust the inner and outer edge plates respectively; Clean the entire nozzle with aluminum oxide to remove surface oxides; Step S2: Load the nozzle into the reactor of the FIC equipment, fix the front edge of the nozzle toward the gas purge direction using a tool, continuously flush with hydrogen fluoride, and then anneal in the furnace; then take out the nozzle from the furnace, use 80 mesh nickel sand to nickel blast the surface to be brazed, and the spray gun is at an angle of 60 degrees to the sandblasted surface to obtain a clean and rough surface; Step S3: After completing the previous operation, within 4 hours, transfer the nozzle to the brazing room, use a 0.8mm needle to inject solder resist into all cooling holes of the nozzle, inject from the inside of the hole to the brazing surface, and stop at 0.3-0.5mm away from the surface; the solder resist at the edge of the hole is full, and no gaps should be left; Step S4: prepare the solder, add an appropriate amount of acetone and mix thoroughly; Step S5: Spray the prepared brazing solder uniformly onto the surface of the nozzle to be brazed at a distance of 15 to 20 cm from the nozzle surface. For areas with more cracks, spray repeatedly after the surface is dried and solidified each time. Load the sprayed nozzle into the brazing furnace, evacuate it, and then heat it to a certain temperature to react and fully decompose the S glue. Step S6: then heating to 1100°C at a heating rate of 8-14°C and maintaining at 1100°C for 40 minutes, the overall temperature of the nozzle is uniform at this temperature, then heating to 1180°C at a heating rate of 8-14°C and maintaining at this temperature for 30 minutes; then cooling to 1150°C in the furnace and maintaining at this temperature for 4 hours; then heating to 1180°C at a heating rate of 8-14°C and maintaining for 4 hours, then heating to 1200°C at a heating rate of 8-14°C and maintaining for 4 hours; Step S7: After the temperature adjustment reaction, argon gas is introduced to cool to room temperature, and a 200-mesh sand belt is used to polish from the leading edge to the trailing edge of the nozzle blade to remove excess brazing material and restore the original profile; Step S8: EDM to open the cooling holes blocked by brazing, using 0.8 mm, 1.2 mm, and 1.5 mm wire diameter electrodes; Step S9: Perform fluorescent penetrant inspection and visual inspection on the parts after diffusion brazing. If cracks or surface defects are found during the visual inspection, repeat steps S2-S7 to repair the defects.

2. The repair process of a cobalt-based high-temperature alloy nozzle by active diffusion brazing according to claim 1, characterized in that: In the step S1, the surface oxide is removed, and the entire nozzle is cleaned using 220 mesh alumina with a purity greater than 98% at a pressure of 6 Bar.

3. The repair process of active diffusion brazing of a cobalt-based high-temperature alloy nozzle according to claim 1 is characterized in that: In the step S2, hydrogen fluoride is used for continuous flushing at 1020° C. for at least 60 minutes, followed by furnace annealing.

4. The repair process of activated diffusion brazing of a cobalt-based high-temperature alloy nozzle according to claim 1, characterized in that: In step S4, the solder is prepared by using A powder with components of Cr: 22.0, Ni: 8.0, W: 7.0, Ta: 3.5, Ti: 0.2, Zr: 0.5 and B powder with components of Cr: 22.5, Ni: 10.0, W: 7.0, Ta: 3.5, Ti: 0.2, Zr: 0.5, B: 4.0 and S glue in a weight ratio of 6:5:

1.

5. The repair process of activated diffusion brazing of a cobalt-based high-temperature alloy nozzle according to claim 1, characterized in that: In step S5, the sprayed nozzle is loaded into the brazing furnace and evacuated to ensure that the vacuum degree of the furnace is better than 5x10 -4 torr; heat up to 450℃ at a heating rate of 8~14℃ and keep at 450℃ for 40 minutes to allow the S glue to fully decompose. Before heating to the next temperature stage, ensure that the vacuum degree in the furnace returns to 5x10 -3 torr.

Citation Information

Patent Citations

  • Brazing process of turbine stator blade of gas turbine

    CN110919289A

  • DZ40M alloy part large-gap brazing repair method

    CN111218584A

  • Brazing process for blade of turbine moving blade of gas turbine

    CN114682868A

  • Process of masking colling holes of a gas turbine component

    EP1365039A1

  • Closure of Cooling Holes with a Filling Agent

    US20140174092A1

Cited By

  • Cobalt-based brazing filler metal for brazing of service damage area of high-temperature alloy hot end component with oxidation film on surface and preparation method of cobalt-based brazing filler metal

    CN119566617A