High-strength flame-retardant moisture-proof furniture board and preparation method thereof

Through the use of modified urea formaldehyde resin glue and flame retardant, combined with the directional paving and hot pressing process of bamboo shavings, high-strength flame-retardant and moisture-proof furniture boards were prepared, which solved the bearing capacity, stability and environmental protection of the particle boards, and realized the implementation of the load-bearing capacity, stability and environmental protection of the particle boards. Higher safety and environmental protection.

CN119017498AActive Publication Date: 2024-11-26WUXI YUSHEA FURNITURE CO LTD

Patent Information

Application Number
CN202411295747.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-26
Estimated Expiration
2044-09-18

AI Technical Summary

Technical Problem

Existing particle boards have disadvantages in load-bearing capacity, stability and environmental protection, and their flammability leads to frequent fire accidents. It is necessary to improve their raw material components to improve safety.

Method used

Bamboo shavings are steamed and dried, combined with modified urea-formaldehyde resin glue and flame retardant, and high-strength flame retardant and moisture-proof furniture boards are prepared through directional paving and hot pressing processes, and nanocellulose and waterproofing agent are added to improve mechanical properties and waterproofing properties. .

Benefits of technology

It improves the mechanical properties and flame retardant effect of the board, reduces the formaldehyde emission, enhances the toughness and thermal stability of the board, and improves the waterproof performance, solving the safety and environmental protection of particle boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a high-strength flame-retardant damp-proof furniture board and a preparation method thereof, and relates to the technical field of furniture boards. According to the prepared board, moso bamboo is adopted as a raw material for wood shaving processing, urea-formaldehyde resin glue, nano cellulose prepared from waste materials generated when the moso bamboo is used for processing wood shavings, a waterproof agent and a flame retardant are added, and the board is prepared through hot pressing and paving. Wherein hydroxymethylated sodium lignin sulfonate and melamine are added into the urea-formaldehyde resin, so that the performance of the resin adhesive is improved; the board is paved by transversely paving the core layer wood shavings and longitudinally paving the surface layer wood shavings, and then paving according to a surface layer-core layer-surface layer manner, so that the furniture board is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of furniture boards, in particular to a high-strength flame-retardant and moisture-proof furniture board and a preparation method thereof. Background Art

[0002] With the improvement of economic conditions, people's demand for living environment is no longer limited to basic living conditions, but is developing towards higher living quality and personalized living space; after buying a house, people often carry out renovations in the hope of achieving an ideal living environment, and the choice of furniture panels in the decoration is crucial. The mainstream panel products on the market include but are not limited to solid wood boards and artificial boards; solid wood boards are directly sawed and processed from intact wood, and have extremely high natural beauty, but the reduction of raw materials and high costs also make most people discouraged; the emergence of artificial boards provides more options for whole-house decoration. According to the 2024 China Particleboard Market Research Data, the demand for particleboard, one of the three major panels in artificial boards, continues to grow, showing a strong production growth trend.

[0003] Although particleboard has certain advantages in price and plasticity, it has great disadvantages in load-bearing capacity, stability and environmental protection. Particleboard was once "widely known" for exceeding the formaldehyde standard, and there are endless examples of fires causing serious casualties due to its flammability. Therefore, it is urgent to improve the raw material composition of particleboard for actual safe use. Summary of the invention

[0004] The object of the present invention is to provide a high-strength flame-retardant and moisture-proof furniture board and a preparation method thereof, so as to solve the problems raised in the prior art.

[0005] To achieve the above object, the present invention provides the following technical solution: a method for preparing a high-strength flame-retardant and moisture-proof furniture board, comprising the following steps: Step 1, processing wood shavings: steam and soften the bamboo slices for 24 hours, control the moisture content to 65-70% and then shaving, then dry, control the moisture content to 2-5%, screen out core shavings with a length of 50-120mm, a width of 20-50mm, and a thickness of 0.3-0.8mm, surface shavings with a length of 20-50mm, a width of 20-50mm, and a thickness of 0.3-0.8mm, and excess waste for standby use; Step 2, prepare modified urea-formaldehyde resin glue: take formaldehyde solution and stir, add sodium hydroxide solution to adjust pH to 7.5-8.0, heat to 40℃ and add the first batch of urea, slowly heat to 90℃ within 30-40min, keep warm for 1h, add hydroxymethylated sodium lignin sulfonate, stir evenly, add formic acid solution dropwise to adjust pH to 4.8-5.1, keep warm for 1-2h, immediately add sodium hydroxide solution dropwise to adjust pH to 7.5-8.0, add the second batch of urea, heat at 80-85℃ ... heat at 80-85℃, stir evenly, add sodium hydroxide solution dropwise to adjust pH to 7.5-8.0, add the second batch of urea, heat at 80-85℃, stir evenly, stir evenly, add formic acid solution dropwise to adjust pH to 4.8-5.1, heat at 80-85℃, stir evenly, stir evenly, add formic acid solution dropwise to adjust pH to 4.8-5.1, heat at 80-85℃, stir evenly, stir evenly, add sodium hydroxide solution dropwise to adjust pH to 7.5-8.0, add the second batch of urea, heat at 80-85℃, stir evenly, stir After reacting at ℃ for 30 minutes, add the third batch of urea, melamine and glutaraldehyde, react at 70-80℃ for 30 minutes, adjust the pH to 7.5-8.0, cool to 40-50℃, and discharge; wherein the molar ratio of urea, formaldehyde, glutaraldehyde and melamine is 1: (1.00-1.05): (0.02-0.05): (0.03-0.05); the addition amount of hydroxymethylated sodium lignin sulfonate is 2-4wt% of the modified urea-formaldehyde resin glue; Step 3, making boards by mixing wood chips with glue: take the core layer wood chips and surface layer wood chips prepared in step 1, mix them with modified nanocellulose and flame retardant respectively, and stir them evenly, then add the modified urea-formaldehyde resin and waterproofing agent prepared in step 2, and continue stirring for 5-10 minutes to obtain the core layer and the surface layer in turn. The directional paving head of the core layer wood chips is responsible for the horizontal paving; the directional paving head of the surface layer wood chips is responsible for the longitudinal paving; the paving is carried out according to the "surface layer-core layer-surface layer", pre-pressed at 0.5-0.8MPa for 2-3min, and then hot pressed, the hot pressing pressure is set to 1.5-1.8MPa, the temperature is 190-200℃, hot pressed for 1-2min, and cooled to obtain the particleboard, that is, the high-strength flame-retardant and moisture-proof furniture board.

[0006] The preparation steps of hydroxymethylated sodium lignin sulfonate are as follows: dissolving sodium lignin sulfonate in water, adding sodium hydroxide to adjust the pH to 11, slowly dropping formaldehyde solution, reacting at 90°C for 2h, dropping formic acid to adjust the pH to 2, centrifuging and washing, and drying at 60°C for 12h to obtain hydroxymethylated sodium lignin sulfonate.

[0007] The preparation steps of the modified nanocellulose in step 3 are as follows: crush the excess waste in step 1, sieve 100 mesh bamboo powder, place it in deionized water, add 2,2,6,6-tetramethylpiperidinoxide and sodium bromide, add a sodium hypochlorite solution with a concentration of 3-5%, react for 3 hours under stirring, during which hydrochloric acid or alkali solution is added dropwise to control the pH to 10-10.5, add anhydrous ethanol after the reaction, filter and wash, disperse in deionized water, mix evenly with polyethyleneimine, heat to 100°C, stir and react for 10 hours, centrifuge after completion, pour off the supernatant, repeat 2-3 times, and freeze-dry to obtain modified nanocellulose.

[0008] The preparation steps of the flame retardant in step 3 are: placing polyethyleneimine in anhydrous ethanol and stirring to mix, adding ammonium polyphosphate and stirring for 2-3 hours, then heating to 60-70° C., filtering and washing, and drying at 60° C. to obtain the flame retardant.

[0009] The preparation steps of the waterproofing agent are as follows: paraffin wax, stearic acid and microcrystalline wax are weighed and mixed in a mass ratio of 1:1:1, and melted at 100°C.

[0010] The mass ratio of the wood chips in each layer of the particleboard (surface layer-core layer-surface layer) is 1:1:1; the amount of glue applied to the core layer is 2-5%, and the amount of glue applied to the surface layer is 5-10%; the amount of the flame retardant is 5-10wt% of the particleboard; the amount of the waterproofing agent is 1-3wt% of the particleboard; and the amount of the modified nanocellulose is 1-2wt%.

[0011] Compared with the prior art, the present invention has the following beneficial effects: 1. The board made by the present invention adopts directional paving of wood chips of different sizes to comprehensively improve the mechanical properties of the board. The wood chips are made of bamboo, and the raw material output is extremely large. The waste left over from the wood chip processing is crushed to prepare nanocellulose and added to the mixed glue to fill the gaps, thereby maximizing the utilization rate of the raw materials and effectively improving the toughness of the glue-cured board. The nanocellulose is modified and polyethyleneimine is introduced to improve the dispersion while improving the bonding performance of the resin glue. The flame retardant is self-assembled and polymerized by ammonium polyphosphate and polyethyleneimine and put into the particleboard. The polyethyleneimine is used to improve the interface bonding between the flame retardant and the wood chips, thereby bringing about an excellent flame retardant effect.

[0012] 2. A small amount of glutaraldehyde is added to the resin glue used in the board made by the present invention to replace part of the formaldehyde, thereby reducing the content of free formaldehyde in the resin glue. At the same time, hydroxymethylated lignin is added as a formaldehyde scavenger to react with free formaldehyde, effectively reducing the free formaldehyde content and improving the thermal stability of the resin.

[0013] 3. The waterproofing agent adopts a wax composite system to improve the waterproof performance of particleboard to a certain extent. DETAILED DESCRIPTION

[0014] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making any creative work shall fall within the scope of protection of the present invention.

[0015] In the experiment, the concentration of formaldehyde solution was 37%; the relative molecular weight of polyethyleneimine was 1800; and ammonium polyphosphate was purchased from Aladdin Biochemical Technology with the product number A669915.

[0016] The preparation steps of the flame retardant are as follows: 10 g of polyethyleneimine is placed in 300 ml of anhydrous ethanol and stirred, 100 g of ammonium polyphosphate is added and stirred for 2 hours, then heated to 60° C., filtered and washed, and dried at 60° C. to obtain the flame retardant.

[0017] The preparation steps of the waterproofing agent are as follows: paraffin wax, stearic acid and microcrystalline wax are weighed and mixed in a mass ratio of 1:1:1, and melted at 100°C.

[0018] The core layer shavings have a length of 60 mm, a width of 20 mm, and a thickness of 0.8 mm; The surface shavings have a length of 20 mm, a width of 20 mm, and a thickness of 0.4 mm.

[0019] Embodiment 1: This embodiment provides a high-strength flame-retardant and moisture-proof furniture board and a preparation method thereof. The specific preparation steps are as follows: Step 1, processing wood shavings: steam and soften the bamboo slices for 24 hours, control the moisture content to 65% before shaving, and then dry to control the moisture content to 3%, select the core shavings, surface shavings and excess waste for later use; Step 2, preparing modified urea-formaldehyde resin glue: take formaldehyde solution and stir, add 30% sodium hydroxide solution to adjust the pH to 8.0, heat to 40°C, add 35% urea, slowly heat to 90°C within 30°C, keep warm for 1h, add hydroxymethylated sodium lignin sulfonate, stir evenly, add 30% formic acid solution to adjust the pH to 5, keep warm for 90min, immediately add 30% sodium hydroxide solution to adjust the pH to 7.5, add 33% urea, react at 85°C for 30min, then add 32% urea and melamine and glutaraldehyde, react at 80°C for 30min, adjust the pH to 7.5, cool to 40°C, and discharge; wherein the molar ratio of urea, formaldehyde, glutaraldehyde and melamine is 1:1.03:0.02:0.03; the addition amount of hydroxymethylated sodium lignin sulfonate is 2wt% of the modified urea-formaldehyde resin glue; Step 3, making boards by mixing wood chips with glue: take the core layer wood chips and surface layer wood chips prepared in step 1, mix them with modified nanocellulose and flame retardant respectively, and stir evenly, then add the modified urea-formaldehyde resin and waterproofing agent prepared in step 2, and continue stirring for 10 minutes to obtain the core layer and the surface layer in turn. The directional paving head of the core layer wood chips is responsible for the horizontal paving; the directional paving head of the surface layer wood chips is responsible for the longitudinal paving; the paving is carried out according to the "surface layer-core layer-surface layer", pre-pressed at 0.8 MPa for 2 minutes, and then hot pressed, the hot pressing pressure is set to 1.5 MPa, the temperature is 200°C, and hot pressed for 2 minutes and cooled to obtain the particleboard, that is, the high-strength flame-retardant and moisture-proof furniture board.

[0020] Among them, the mass ratio of each layer of wood chips in the particleboard: surface layer-core layer-surface layer is 1:1:1; the amount of glue applied to the core layer is 4%, and the amount of glue applied to the surface layer is 10%; the amount of flame retardant is 6wt% of the particleboard; the amount of waterproofing agent is 1wt% of the particleboard; and the amount of modified nanocellulose is 1wt%.

[0021] The preparation steps of hydroxymethylated sodium lignin sulfonate are as follows: dissolving sodium lignin sulfonate in water, adding 30% sodium hydroxide to adjust the pH to 11, slowly dropping formaldehyde solution, reacting at 90°C for 2h, dropping 30% formic acid to adjust the pH to 2, centrifuging and washing, and drying at 60°C for 12h to obtain hydroxymethylated sodium lignin sulfonate. The material ratio of sodium lignin sulfonate to formaldehyde solution is 3:1.

[0022] The preparation steps of modified nanocellulose are as follows: crush the excess waste in step 1, sieve 100 mesh bamboo powder, take 1g of the sieved bamboo powder, put it in 100ml of deionized water, add 0.02g of 2,2,6,6-tetramethylpiperidinoxide and 0.1g of sodium bromide, add 60ml of 5% sodium hypochlorite solution, react for 3h under stirring, during which hydrochloric acid solution or alkali solution is added dropwise to control the pH to 10, and after the reaction, add 10ml of anhydrous ethanol in turn, filter and wash, disperse in deionized water to 1.5wt%, mix evenly with 100ml of polyethyleneimine, heat to 100°C, stir and react for 10h, centrifuge after completion, pour off the supernatant, repeat 3 times, and freeze-dry to obtain modified nanocellulose.

[0023] Embodiment 2: This embodiment provides a high-strength flame-retardant and moisture-proof furniture board and a preparation method thereof. The specific preparation steps are as follows: Step 1, processing wood shavings: steam and soften the bamboo slices for 24 hours, control the moisture content to 65% before shaving, and then dry to control the moisture content to 3%, select the core shavings, surface shavings and excess waste for later use; Step 2, preparing modified urea-formaldehyde resin glue: take formaldehyde solution and stir, add 30% sodium hydroxide solution to adjust the pH to 8.0, heat to 40°C, add 35% urea, slowly heat to 90°C within 30°C, keep warm for 1h, add hydroxymethylated sodium lignin sulfonate, stir evenly, add 30% formic acid solution to adjust the pH to 5, keep warm for 90min, immediately add 30% sodium hydroxide solution to adjust the pH to 7.5, add 33% urea, react at 85°C for 30min, then add 32% urea and melamine and glutaraldehyde, react at 80°C for 30min, adjust the pH to 7.5, cool to 40°C, and discharge; wherein the molar ratio of urea, formaldehyde, glutaraldehyde and melamine is 1:1.01:0.04:0.04; the addition amount of hydroxymethylated sodium lignin sulfonate is 3wt% of the modified urea-formaldehyde resin glue; Step 3, making boards by mixing wood chips with glue: take the core layer wood chips and surface layer wood chips prepared in step 1, mix them with modified nanocellulose and flame retardant respectively, and stir evenly, then add the modified urea-formaldehyde resin and waterproofing agent prepared in step 2, and continue stirring for 10 minutes to obtain the core layer and the surface layer in turn. The directional paving head of the core layer wood chips is responsible for the horizontal paving; the directional paving head of the surface layer wood chips is responsible for the longitudinal paving; the paving is carried out according to the "surface layer-core layer-surface layer", pre-pressed at 0.8 MPa for 2 minutes, and then hot pressed, the hot pressing pressure is set to 1.5 MPa, the temperature is 200°C, and hot pressed for 2 minutes and cooled to obtain the particleboard, that is, the high-strength flame-retardant and moisture-proof furniture board.

[0024] Among them, the mass ratio of each layer of wood chips in the particleboard: surface layer-core layer-surface layer is 1:1:1; the amount of glue applied to the core layer is 4%, and the amount of glue applied to the surface layer is 10%; the amount of flame retardant is 7wt% of the particleboard; the amount of waterproofing agent is 2wt% of the particleboard; and the amount of modified nanocellulose is 2wt%.

[0025] The preparation steps of hydroxymethylated sodium lignin sulfonate are as follows: dissolving sodium lignin sulfonate in water, adding 30% sodium hydroxide to adjust the pH to 11, slowly dropping formaldehyde solution, reacting at 90°C for 2h, dropping 30% formic acid to adjust the pH to 2, centrifuging and washing, and drying at 60°C for 12h to obtain hydroxymethylated sodium lignin sulfonate. The material ratio of sodium lignin sulfonate to formaldehyde solution is 3:1.

[0026] The preparation steps of modified nanocellulose are as follows: crush the excess waste in step 1, sieve 100 mesh bamboo powder, take 1g of the sieved bamboo powder, put it in 100ml of deionized water, add 0.02g of 2,2,6,6-tetramethylpiperidinoxide and 0.1g of sodium bromide, add 60ml of 5% sodium hypochlorite solution, react for 3h under stirring, during which hydrochloric acid solution or alkali solution is added dropwise to control the pH to 10, and after the reaction, add 10ml of anhydrous ethanol in turn, filter and wash, disperse in deionized water to 1.5wt%, mix evenly with 100ml of polyethyleneimine, heat to 100°C, stir and react for 10h, centrifuge after completion, pour off the supernatant, repeat 3 times, and freeze-dry to obtain modified nanocellulose.

[0027] Embodiment 3: This embodiment provides a high-strength flame-retardant and moisture-proof furniture board and a preparation method thereof. The specific preparation steps are as follows: Step 1, processing wood shavings: steam and soften the bamboo slices for 24 hours, control the moisture content to 65% before shaving, and then dry to control the moisture content to 3%, select the core shavings, surface shavings and excess waste for later use; Step 2, preparing modified urea-formaldehyde resin glue: take formaldehyde solution and stir, add 30% sodium hydroxide solution to adjust the pH to 8.0, heat to 40°C, add 35% urea, slowly heat to 90°C within 30°C, keep warm for 1h, add hydroxymethylated sodium lignin sulfonate, stir evenly, add 30% formic acid solution to adjust the pH to 5, keep warm for 90min, immediately add 30% sodium hydroxide solution to adjust the pH to 7.5, add 33% urea, react at 85°C for 30min, then add 32% urea and melamine and glutaraldehyde, react at 80°C for 30min, adjust the pH to 7.5, cool to 40°C, and discharge; wherein the molar ratio of urea, formaldehyde, glutaraldehyde and melamine is 1:1.00:0.05:0.05; the addition amount of hydroxymethylated sodium lignin sulfonate is 4wt% of the modified urea-formaldehyde resin glue; Step 3, making boards by mixing wood chips with glue: take the core layer wood chips and surface layer wood chips prepared in step 1, mix them with modified nanocellulose and flame retardant respectively, and stir evenly, then add the modified urea-formaldehyde resin and waterproofing agent prepared in step 2, and continue stirring for 10 minutes to obtain the core layer and the surface layer in turn. The directional paving head of the core layer wood chips is responsible for the horizontal paving; the directional paving head of the surface layer wood chips is responsible for the longitudinal paving; the paving is carried out according to the "surface layer-core layer-surface layer", pre-pressed at 0.8 MPa for 2 minutes, and then hot pressed, the hot pressing pressure is set to 1.5 MPa, the temperature is 200°C, and hot pressed for 2 minutes and cooled to obtain the particleboard, that is, the high-strength flame-retardant and moisture-proof furniture board.

[0028] Among them, the mass ratio of each layer of wood chips in the particleboard: surface layer-core layer-surface layer is 1:1:1; the amount of glue applied to the core layer is 4%, and the amount of glue applied to the surface layer is 10%; the amount of flame retardant is 10wt% of the particleboard; the amount of waterproofing agent is 3wt% of the particleboard; and the amount of modified nanocellulose is 2wt%.

[0029] The preparation steps of hydroxymethylated sodium lignin sulfonate are as follows: dissolving sodium lignin sulfonate in water, adding 30% sodium hydroxide to adjust the pH to 11, slowly dropping formaldehyde solution, reacting at 90°C for 2h, dropping 30% formic acid to adjust the pH to 2, centrifuging and washing, and drying at 60°C for 12h to obtain hydroxymethylated sodium lignin sulfonate. The material ratio of sodium lignin sulfonate to formaldehyde solution is 3:1.

[0030] The preparation steps of modified nanocellulose are as follows: crush the excess waste in step 1, sieve 100 mesh bamboo powder, take 1g of the sieved bamboo powder, put it in 100ml of deionized water, add 0.02g of 2,2,6,6-tetramethylpiperidinoxide and 0.1g of sodium bromide, add 60ml of 5% sodium hypochlorite solution, react for 3h under stirring, during which hydrochloric acid solution or alkali solution is added dropwise to control the pH to 10, and after the reaction, add 10ml of anhydrous ethanol in turn, filter and wash, disperse in deionized water to 1.5wt%, mix evenly with 100ml of polyethyleneimine, heat to 100°C, stir and react for 10h, centrifuge after completion, pour off the supernatant, repeat 3 times, and freeze-dry to obtain modified nanocellulose.

[0031] Comparative Example 1: No sodium hydroxymethyl lignin sulfonate was added to Example 3, and the specific steps were as follows: Step 1, processing wood shavings: steam and soften the bamboo slices for 24 hours, control the moisture content to 65% before shaving, and then dry to control the moisture content to 3%, select the core shavings, surface shavings and excess waste for later use; Step 2, preparing modified urea-formaldehyde resin glue: take formaldehyde solution and stir, add 30% sodium hydroxide solution to adjust the pH to 8.0, heat to 40°C, add 35% urea, slowly heat to 90°C within 30°C, keep warm for 1h, add hydroxymethylated sodium lignin sulfonate, stir evenly, add 30% formic acid solution to adjust the pH to 5, keep warm for 90min, immediately add 30% sodium hydroxide solution to adjust the pH to 7.5, add 33% urea, react at 85°C for 30min, then add 32% urea and melamine and glutaraldehyde, react at 80°C for 30min, adjust the pH to 7.5, cool to 40°C, and discharge; wherein the molar ratio of urea, formaldehyde, glutaraldehyde and melamine is 1:1.00:0.05:0.05; the addition amount of hydroxymethylated sodium lignin sulfonate is 4wt% of the modified urea-formaldehyde resin glue; Step 3, making boards by mixing wood chips with glue: take the core layer wood chips and surface layer wood chips prepared in step 1, mix them with modified nanocellulose and flame retardant respectively, and stir evenly, then add the modified urea-formaldehyde resin and waterproofing agent prepared in step 2, and continue stirring for 10 minutes to obtain the core layer and the surface layer in turn. The directional paving head of the core layer wood chips is responsible for the horizontal paving; the directional paving head of the surface layer wood chips is responsible for the longitudinal paving; the paving is carried out according to the "surface layer-core layer-surface layer", pre-pressed at 0.8 MPa for 2 minutes, and then hot pressed, the hot pressing pressure is set to 1.5 MPa, the temperature is 200°C, and hot pressed for 2 minutes and cooled to obtain the particleboard, that is, the high-strength flame-retardant and moisture-proof furniture board.

[0032] Among them, the mass ratio of each layer of wood chips in the particleboard: surface layer-core layer-surface layer is 1:1:1; the amount of glue applied to the core layer is 4%, and the amount of glue applied to the surface layer is 10%; the amount of flame retardant is 10wt% of the particleboard; the amount of waterproofing agent is 3wt% of the particleboard; and the amount of modified nanocellulose is 2wt%.

[0033] The preparation steps of modified nanocellulose are as follows: crush the excess waste in step 1, sieve 100 mesh bamboo powder, take 1g of the sieved bamboo powder, put it in 100ml of deionized water, add 0.02g of 2,2,6,6-tetramethylpiperidinoxide and 0.1g of sodium bromide, add 60ml of 5% sodium hypochlorite solution, react for 3h under stirring, during which hydrochloric acid solution or alkali solution is added dropwise to control the pH to 10, and after the reaction, add 10ml of anhydrous ethanol in turn, filter and wash, disperse in deionized water to 1.5wt%, mix evenly with 100ml of polyethyleneimine, heat to 100°C, stir and react for 10h, centrifuge after completion, pour off the supernatant, repeat 3 times, and freeze-dry to obtain modified nanocellulose.

[0034] Comparative Example 2: The nanocellulose of Example 3 is not modified, and specifically comprises the following steps: Step 1, processing wood shavings: steam and soften the bamboo slices for 24 hours, control the moisture content to 65% before shaving, and then dry to control the moisture content to 3%, select the core shavings, surface shavings and excess waste for later use; Step 2, preparing modified urea-formaldehyde resin glue: take formaldehyde solution and stir, add 30% sodium hydroxide solution to adjust the pH to 8.0, heat to 40°C, add 35% urea, slowly heat to 90°C within 30°C, keep warm for 1h, add hydroxymethylated sodium lignin sulfonate, stir evenly, add 30% formic acid solution to adjust the pH to 5, keep warm for 90min, immediately add 30% sodium hydroxide solution to adjust the pH to 7.5, add 33% urea, react at 85°C for 30min, then add 32% urea and melamine and glutaraldehyde, react at 80°C for 30min, adjust the pH to 7.5, cool to 40°C, and discharge; wherein the molar ratio of urea, formaldehyde, glutaraldehyde and melamine is 1:1.00:0.05:0.05; the addition amount of hydroxymethylated sodium lignin sulfonate is 4wt% of the modified urea-formaldehyde resin glue; Step 3, making boards by mixing wood chips with glue: take the core layer wood chips and surface layer wood chips prepared in step 1, mix them with modified nanocellulose and flame retardant respectively, and stir evenly, then add the modified urea-formaldehyde resin and waterproofing agent prepared in step 2, and continue stirring for 10 minutes to obtain the core layer and the surface layer in turn. The directional paving head of the core layer wood chips is responsible for the horizontal paving; the directional paving head of the surface layer wood chips is responsible for the longitudinal paving; the paving is carried out according to the "surface layer-core layer-surface layer", pre-pressed at 0.8 MPa for 2 minutes, and then hot pressed, the hot pressing pressure is set to 1.5 MPa, the temperature is 200°C, and hot pressed for 2 minutes and cooled to obtain the particleboard, that is, the high-strength flame-retardant and moisture-proof furniture board.

[0035] Among them, the mass ratio of each layer of wood chips in the particleboard: surface layer-core layer-surface layer is 1:1:1; the amount of glue applied to the core layer is 4%, and the amount of glue applied to the surface layer is 10%; the amount of flame retardant is 10wt% of the particleboard; the amount of waterproofing agent is 3wt% of the particleboard; and the amount of nanocellulose is 2wt%.

[0036] The preparation steps of hydroxymethylated sodium lignin sulfonate are as follows: dissolving sodium lignin sulfonate in water, adding 30% sodium hydroxide to adjust the pH to 11, slowly dropping formaldehyde solution, reacting at 90°C for 2h, dropping 30% formic acid to adjust the pH to 2, centrifuging and washing, and drying at 60°C for 12h to obtain hydroxymethylated sodium lignin sulfonate. The material ratio of sodium lignin sulfonate to formaldehyde solution is 3:1.

[0037] The preparation steps of nanocellulose are as follows: crush the excess waste in step 1, sieve 100 mesh bamboo powder, take 1g of the sieved bamboo powder, put it in 100ml of deionized water, add 0.02g of 2,2,6,6-tetramethylpiperidinoxide and 0.1g of sodium bromide, add 60ml of 5% sodium hypochlorite solution, react for 3h under stirring, during which hydrochloric acid solution or alkali solution is added dropwise to control the pH to 10, and after the reaction is completed, add 10ml of anhydrous ethanol in sequence, filter, wash, and dry to obtain the nanocellulose.

[0038] Comparative Example 3: The waterproofing agent in Example 3 is replaced with paraffin wax and melted at 100° C. The specific steps are as follows: Step 1, processing wood shavings: steam and soften the bamboo slices for 24 hours, control the moisture content to 65% before shaving, and then dry to control the moisture content to 3%, select the core shavings, surface shavings and excess waste for later use; Step 2, preparing modified urea-formaldehyde resin glue: take formaldehyde solution and stir, add 30% sodium hydroxide solution to adjust the pH to 8.0, heat to 40°C, add 35% urea, slowly heat to 90°C within 30°C, keep warm for 1h, add hydroxymethylated sodium lignin sulfonate, stir evenly, add 30% formic acid solution to adjust the pH to 5, keep warm for 90min, immediately add 30% sodium hydroxide solution to adjust the pH to 7.5, add 33% urea, react at 85°C for 30min, then add 32% urea and melamine and glutaraldehyde, react at 80°C for 30min, adjust the pH to 7.5, cool to 40°C, and discharge; wherein the molar ratio of urea, formaldehyde, glutaraldehyde and melamine is 1:1.00:0.05:0.05; the addition amount of hydroxymethylated sodium lignin sulfonate is 4wt% of the modified urea-formaldehyde resin glue; Step 3, making boards by mixing wood chips with glue: take the core layer wood chips and surface layer wood chips prepared in step 1, mix them with modified nanocellulose and flame retardant respectively, and stir evenly, then add the modified urea-formaldehyde resin and waterproofing agent prepared in step 2, and continue stirring for 10 minutes to obtain the core layer and the surface layer in turn. The directional paving head of the core layer wood chips is responsible for the horizontal paving; the directional paving head of the surface layer wood chips is responsible for the longitudinal paving; the paving is carried out according to the "surface layer-core layer-surface layer", and hot pressing is carried out after pre-pressing at 0.8 MPa for 2, and the hot pressing pressure is set to 1.5 MPa and the temperature is 200°C. Hot pressing is carried out for 2 minutes and then cooled to obtain the particleboard, that is, the high-strength flame-retardant and moisture-proof furniture board.

[0039] Among them, the mass ratio of each layer of wood chips in the particleboard: surface layer-core layer-surface layer is 1:1:1; the amount of glue applied to the core layer is 4%, and the amount of glue applied to the surface layer is 10%; the amount of flame retardant is 10wt% of the particleboard; the amount of waterproofing agent is 3wt% of the particleboard; and the amount of modified nanocellulose is 2wt% of the particleboard.

[0040] The preparation steps of hydroxymethylated sodium lignin sulfonate are as follows: dissolving sodium lignin sulfonate in water, adding 30% sodium hydroxide to adjust the pH to 11, slowly dropping formaldehyde solution, reacting at 90°C for 2h, dropping 30% formic acid to adjust the pH to 2, centrifuging and washing, and drying at 60°C for 12h to obtain hydroxymethylated sodium lignin sulfonate. The material ratio of sodium lignin sulfonate to formaldehyde solution is 3:1.

[0041] The preparation steps of modified nanocellulose are as follows: crush the excess waste in step 1, sieve 100 mesh bamboo powder, take 1g of the sieved bamboo powder, put it in 100ml of deionized water, add 0.02g of 2,2,6,6-tetramethylpiperidinoxide and 0.1g of sodium bromide, add 60ml of 5% sodium hypochlorite solution, react for 3h under stirring, during which hydrochloric acid solution or alkali solution is added dropwise to control the pH to 10, and after the reaction, add 10ml of anhydrous ethanol in turn, filter and wash, disperse in deionized water to 1.5wt%, mix evenly with 100ml of polyethyleneimine, heat to 100°C, stir and react for 10h, centrifuge after completion, pour off the supernatant, repeat 3 times, and freeze-dry to obtain modified nanocellulose.

[0042] Detection test The physical and mechanical properties of the plates prepared in Examples 1-3 and Comparative Examples 1-3 were tested according to GB / T 41715.

[0043] Flame retardant performance: Use an oxygen index meter to carry out the limiting oxygen index LOI test.

[0044]

[0045] Through the above experimental data, the board prepared in Example 3 has good physical and mechanical properties and flame retardant properties; the fact that no sodium hydroxymethyl lignin sulfonate is added in Comparative Example 1 and no modification of nanocellulose in Comparative Example 2 both affect the gluing properties and mechanical properties of the board, and the formaldehyde emission increases; the waterproofing agent in Comparative Example 3 is replaced with a single molten paraffin, which reduces the moisture-proof performance of the board.

[0046] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a high-strength flame-retardant and moisture-proof furniture board, characterized in that: The following steps are involved: Step 1, processing wood shavings: steam and soften the bamboo slices for 24 hours, control the moisture content to 65-70% and then shaving, then dry, control the moisture content to 2-5%, screen out core shavings with a length of 50-120mm, a width of 20-50mm, and a thickness of 0.3-0.8mm, surface shavings with a length of 20-50mm, a width of 20-50mm, and a thickness of 0.3-0.8mm, and excess waste for standby use; Step 2, preparing modified urea-formaldehyde resin glue: take formaldehyde solution and stir, add sodium hydroxide solution to adjust pH to 7.5-8.0, heat to 40°C and add the first batch of urea, slowly heat to 90°C within 30-40min, keep warm for 1h, add hydroxymethylated sodium lignin sulfonate, stir evenly, add formic acid solution dropwise to adjust pH to 4.8-5.1, keep warm for 1-2h, immediately add sodium hydroxide solution dropwise to adjust pH to 7.5-8.0, add the second batch of urea, react at 80-85°C for 30min, then add the third batch of urea and melamine, glutaraldehyde, react at 70-80°C for 30min, adjust pH to 7.5-8.0, cool to 40-50°C, and discharge; Step 3, wood chips and glue-mixed board making: take the core layer wood chips and surface layer wood chips prepared in step 1, mix them with modified nanocellulose and flame retardant respectively, and stir them evenly, then add the modified urea-formaldehyde resin and waterproofing agent prepared in step 2, and continue stirring for 5-10 minutes to obtain the core layer and the surface layer in turn. The directional paving head of the core layer wood chips is responsible for the horizontal paving; the directional paving head of the surface layer wood chips is responsible for the longitudinal paving; the paving is carried out according to "surface layer-core layer-surface layer", and hot pressing is carried out after the pre-pressing is completed to obtain the particleboard, that is, the high-strength flame-retardant and moisture-proof furniture board.

2. The method for preparing a high-strength flame-retardant and moisture-proof furniture board according to claim 1, characterized in that: The molar ratio of urea, formaldehyde, glutaraldehyde and melamine in the modified urea-formaldehyde resin glue prepared in step 2 is 1: (1.00-1.05): (0.02-0.05): (0.03-0.05).

3. The method for preparing a high-strength flame-retardant and moisture-proof furniture board according to claim 1, characterized in that: The preparation steps of hydroxymethylated sodium lignin sulfonate are as follows: dissolving sodium lignin sulfonate in water, adding sodium hydroxide to adjust the pH to 11, slowly dropping formaldehyde solution, reacting at 90°C for 2h, dropping formic acid to adjust the pH to 2, centrifuging and washing, and drying at 60°C for 12h to obtain hydroxymethylated sodium lignin sulfonate; the addition amount of hydroxymethylated sodium lignin sulfonate is 2-4wt% of the modified urea-formaldehyde resin glue.

4. The method for preparing a high-strength flame-retardant and moisture-proof furniture board according to claim 1, characterized in that: The preparation steps of the modified nanocellulose in step 3 are as follows: crush the excess waste in step 1, sieve 100 mesh bamboo powder, place it in deionized water, add 2,2,6,6-tetramethylpiperidinoxide and sodium bromide, add a sodium hypochlorite solution with a concentration of 3-5%, react for 3 hours under stirring, during which hydrochloric acid solution or alkali solution is added dropwise to control the pH to 10-10.5, add anhydrous ethanol after the reaction, filter and wash, disperse in deionized water, mix evenly with polyethyleneimine, heat to 100°C, stir and react for 10 hours, centrifuge after completion, pour off the supernatant, repeat 2-3 times, and freeze-dry to obtain modified nanocellulose.

5. The method for preparing a high-strength flame-retardant and moisture-proof furniture board according to claim 1, characterized in that: The preparation steps of the flame retardant in step 3 are: placing polyethyleneimine in anhydrous ethanol and stirring to mix, adding ammonium polyphosphate and stirring for 2-3 hours, then heating to 60-70° C., filtering and washing, and drying at 60° C. to obtain the flame retardant.

6. The method for preparing a high-strength flame-retardant and moisture-proof furniture board according to claim 1, characterized in that: The preparation steps of the waterproofing agent are as follows: paraffin wax, stearic acid and microcrystalline wax are weighed and mixed in a mass ratio of 1:1:1, and melted at 100°C.

7. The method for preparing a high-strength flame-retardant and moisture-proof furniture board according to claim 1, characterized in that: The mass ratio of the shavings in each layer of the surface layer-core layer-surface layer is 1:1:1; the glue application amount of the core layer is 2-5%, and the glue application amount of the surface layer is 5-10%.

8. The method for preparing a high-strength flame-retardant and moisture-proof furniture board according to claim 1, characterized in that: The amount of the flame retardant is 5-10wt% of the particle board; the amount of the waterproofing agent is 1-3wt% of the particle board; and the amount of the modified nanocellulose is 1-2wt%.

9. The method for preparing a high-strength flame-retardant and moisture-proof furniture board according to claim 1, characterized in that: In step 3, the pre-pressing pressure is 0.5-0.8 MPa, and the pre-pressing is 2-3 min; after the pre-pressing, the hot pressing pressure is 1.5-1.8 MPa, the hot pressing temperature is 190-200° C., and the hot pressing is 1-2 min.

Citation Information

Patent Citations

  • Modified lignin and urea-formaldehyde resin synthesized from same and preparation methods of modified lignin and urea-formaldehyde resin

    CN102241826A

  • Method for improving product surface properties by pennisetum man-made board processing residues

    CN103112072A

  • Oxidation nanocellulose adsorbing material and preparation method thereof

    CN105498733A

  • Production process of moisture-proof super-E0 bamboo shaving board

    CN111571758A

  • Production process of colored solid wood particle board

    CN115972342A

Cited By

  • Manufacturing method of large thin OSB (oriented strand board) composite floor with stable size

    CN120155982A

  • A method for manufacturing a dimensionally stable large-piece thin OSB composite floor

    CN120155982B