Moisture-proof mildew-resistant medium-density light fiberboard

By adding modified chitosan solution and anti-mold powder to medium-density lightweight fiberboard, combined with nano-semiconductor active anti-mold agent, the problem of fiberboard being susceptible to moisture and anti-mold is solved, and better waterproof and anti-mold effect is achieved. Extends service life and improves antibacterial properties.

CN119017501AActive Publication Date: 2024-11-26NANJING HEADWAY FURNITURE CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411432862.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-15
Publication Date
2024-11-26
Estimated Expiration
2044-10-15

AI Technical Summary

Technical Problem

Medium-density lightweight fiberboard is prone to moisture and prevent mildew during use. The existing waterproofing agent is lost after a long period of use, resulting in the fiberboard being easily damp and moldy, making it difficult to effectively prevent mold growth.

Method used

By adding modified chitosan solution and anti-mold powder, including tetra-acid zinc oxide whiskers and thiodecafluorooctyl trimethoxysilane monomers, to the fiberboard, a nanosemiconductor active anti-mold agent is formed, combined with the modified shell. The glycan is cross-linked with ligno fibers to improve waterproof and mildew resistance.

Benefits of technology

It significantly improves the waterproof effect and mildew resistance level of medium-density lightweight fiberboard, extends its service life, and maintains high anti-mold performance after water immersion, and has high efficiency, broad spectrum and long-lasting antibacterial effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a moisture-proof mildew-resistant medium-density light fiberboard, and belongs to the technical field of medium-density fiberboards. Wood fibers are subjected to hot grinding and defibrating to prepare fiber slurry, a modified chitosan solution, melamine modified urea resin, an ammonium chloride curing agent and mildew preventive powder are added into the fiber slurry, stirring and mixing are performed, and the moisture-proof mildew-resistant medium-density light fiberboard is obtained. Drying until the water content of the fibers is 7-8%, paving the fibers in a mold, and performing hot pressing for 5-6 minutes under the conditions of 195-200 DEG C and 5-6 MPa to obtain the damp-proof mildew-resistant medium-density light fiberboard. Tetrapod-like zinc oxide whiskers serve as a base body of the mildew preventive powder, the tetrapod-like zinc oxide whiskers are coated after a tridecafluorooctyltrimethoxysilane monomer is subjected to self-polymerization, and a fluorine-containing side chain on the surface of the tetrapod-like zinc oxide whiskers is beneficial for improving the humidity resistance of the medium-density fiberboard; the modified chitosan solution contains disulfide bonds which can be cross-linked with hydroxyl groups on the surface of wood fibers, so that the strength and the antibacterial property of the wood fibers can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of medium density fiberboards, and in particular relates to a moisture-proof and mildew-resistant medium density lightweight fiberboard. Background Art

[0002] Medium-density fiberboard is a commonly used board material in many fields such as furniture manufacturing, building decoration, and interior decoration of vehicles and ships. Medium-density fiberboard is made of wood fiber or other plant fiber, mainly including pine, poplar, eucalyptus, bamboo, reed and other wood or plant fiber. These raw materials are mechanically separated and chemically treated to form sawdust or fiber, which is then mixed with auxiliary materials such as adhesives and waterproofing agents to form boards under heating and pressure conditions.

[0003] Medium-density lightweight fiberboard has strong water absorption and is easily affected by moisture and mildew. Even if auxiliary materials such as waterproofing agents are added during the preparation process, the surface waterproofing agents will be lost after long-term use, causing the fiberboard to still be susceptible to moisture and mildew. Summary of the invention

[0004] The purpose of the present invention is to provide a moisture-proof and mildew-resistant medium-density lightweight fiberboard, which improves its water-proof and mildew-proof effects by mildew-proof agent powder and modified chitosan solution, thereby extending its service life.

[0005] The purpose of the present invention can be achieved through the following technical solutions: A moisture-proof and mildew-resistant medium-density lightweight fiberboard is prepared by the following steps: The fiber slurry is prepared by heat grinding and defibration of wood fiber, and modified chitosan solution, melamine modified urea-formaldehyde resin, ammonium chloride curing agent and mildewproof agent powder are added to the fiber slurry, stirred and mixed at 20-25°C and 500-800r / min for 20-30min, dried to the fiber moisture content of 7-8%, spread into a mold, and hot pressed at 195-200°C and 5-6MPa for 5-6min to obtain a moisture-proof and mildew-resistant medium-density lightweight fiberboard.

[0006] Furthermore, the usage ratio of wood fiber, modified chitosan solution, melamine modified urea-formaldehyde resin, ammonium chloride curing agent and mildewproofing agent powder is 100g: 50-60mL: 13-13.5g: 0.03325-0.03375g: 0.06-0.08g.

[0007] Furthermore, the mildewcide powder is prepared by the following steps: Deionized water, tetrahydrofuran, tetranepal zinc oxide whisker and tetramethylammonium hydroxide are added to a reactor at 20-25° C., and stirred at 2000-3000 r / min for 10-15 minutes. Then, under nitrogen protection, tridecafluorooctyltrimethoxysilane monomer is added to the reactor, and stirring is continued for 5-10 minutes. After that, the reaction is stirred at 35° C. for 24-26 hours to make the polymerized fluorinated polysilsesquioxane cover the tetranepal zinc oxide whisker. The solvent and unreacted monomer are removed by rotary evaporation. The reaction product is washed with anhydrous ethanol and deionized water for 2-3 times respectively, and vacuum dried to obtain a mildew inhibitor powder.

[0008] Furthermore, the mass ratio of deionized water, tetrahydrofuran, tetranepal-shaped zinc oxide whiskers, tetramethylammonium hydroxide and tridecafluorooctyltrimethoxysilane monomer is 5:15:5-6:0.05:15-16.

[0009] Further, the modified chitosan is prepared by the following steps: Chitosan and deionized water were added into a reactor, the pH value was adjusted to 3 with 1 mol / L acetic acid solution, and stirred at 300-500 r / min for 20-30 min. Then, the modifier solution and anhydrous ethanol as a water absorbent were added into the reactor, and the reaction was stirred at 20-25° C. for 16-18 h to obtain a modified chitosan solution.

[0010] Furthermore, the dosage ratio of chitosan, deionized water and modifier solution is 3.2 g: 160 mL: 40 mL: 15-20 mL.

[0011] Further, the modifier solution is prepared by the following steps: Add α-lipoic acid, sodium hydroxide and deionized water into a reactor, stir at 200-300 r / min for 30-40 min, then add EDC (1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride) and NHS (N-hydroxysuccinimide) into the reactor, continue stirring for 5-10 min to activate the carboxyl group in lipoic acid and obtain a modifier solution.

[0012] Furthermore, the usage ratio of α-lipoic acid, sodium hydroxide, deionized water, EDC and MHS is 0.2 g: 0.04 g: 40 mL: 0.096 g: 0.115 g.

[0013] Beneficial effects of the present invention: The moisture-proof and mildew-resistant medium-density lightweight fiberboard of the present invention has a good waterproof effect and can still maintain a high mildew-proof level after being immersed in water, which helps to improve the service life of the medium-density lightweight fiberboard.

[0014] The mildew-proof agent powder of the present invention uses four-needle zinc oxide whiskers as a matrix, and has the function of releasing active oxygen due to its nano-semiconductor activity, and exhibits a high-efficiency, broad-spectrum, and long-lasting antibacterial effect in a macroscopic sense. The tetra-needle zinc oxide whiskers are coated with tridecafluorooctyl trimethoxysilane monomers after self-polymerization, and the fluorine-containing side chains on the surface help to improve the moisture-proof performance of medium-density fiberboard. The preparation of the modified chitosan solution is to use the dehydration condensation of the carboxyl groups on the octyl sulfate in the modifier solution and the amino groups on the chitosan to prepare chitosan containing disulfide bonds, which can be cross-linked with the hydroxyl groups on the surface of wood fiber, which helps to improve the strength and antibacterial performance of the wood fiber, and further improve the mildew-proof effect of the medium-density light fiberboard. DETAILED DESCRIPTION

[0015] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0016] Embodiment 1: This embodiment provides a moisture-proof and mildew-resistant medium-density lightweight fiberboard, which is prepared by the following steps: Step 1: Add 50kg of deionized water, 150kg of tetrahydrofuran, 50kg of tetra-needle zinc oxide whisker and 0.5kg of tetramethylammonium hydroxide into a reactor at 20°C, stir at 2000r / min for 10min, then add 150kg of tridecafluorooctyltrimethoxysilane monomer into the reactor under nitrogen protection, continue stirring for 5min, and then stir and react at 35°C for 24h to make the polymerized fluorinated polysilsesquioxane coat the tetra-needle zinc oxide whisker, rotary evaporation to remove the solvent and unreacted monomer, wash the reaction product with anhydrous ethanol and deionized water twice respectively, and vacuum dry to obtain a mildew inhibitor powder.

[0017] Step 2: Add 20kg of α-lipoic acid, 4kg of sodium hydroxide and 4000L of deionized water into the reactor, stir at 200r / min for 30min, then add 9.6kg of EDC (1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride) and 11.5kg of NHS (N-hydroxysuccinimide) into the reactor, continue stirring for 5min to activate the carboxyl group in lipoic acid and obtain a modifier solution.

[0018] Step 3: Add 3.2 kg of chitosan and 160 L of deionized water into the reactor, adjust the pH value to 3 with 1 mol / L acetic acid solution, stir at 300 r / min for 20 min, then add 40 L of modifier solution and 15 L of anhydrous ethanol as a water absorbent into the reactor, stir and react at 20 ° C for 16 h to obtain a modified chitosan solution.

[0019] Step 4: 100kg of wood fiber is subjected to hot grinding and defibration to prepare fiber slurry, 50L of modified chitosan solution, 13kg of melamine-modified urea-formaldehyde resin, 33.25g of ammonium chloride curing agent and 0.06kg of mildewproof agent powder are added to the fiber slurry, stirred and mixed at 20℃ and 500r / min for 20min, dried to the fiber moisture content of 7%, spread into a mold, and hot pressed at 195℃ and 5MPa for 5min to obtain a moisture-proof and mildew-resistant medium-density lightweight fiberboard.

[0020] Embodiment 2: This embodiment provides a moisture-proof and mildew-resistant medium-density lightweight fiberboard, which is prepared by the following steps: Step 1: Add 50kg of deionized water, 150kg of tetrahydrofuran, 55kg of tetra-needle zinc oxide whisker and 0.5kg of tetramethylammonium hydroxide into a reactor at 22°C, stir at 2500r / min for 12min, then add 155kg of tridecafluorooctyltrimethoxysilane monomer into the reactor under nitrogen protection, continue stirring for 8min, and then stir and react at 35°C for 25h to make the polymerized fluorinated polysilsesquioxane coat the tetra-needle zinc oxide whisker, remove the solvent and unreacted monomer by rotary evaporation, wash the reaction product with anhydrous ethanol and deionized water twice respectively, and vacuum dry to obtain a mildew inhibitor powder.

[0021] Step 2: Add 20kg of α-lipoic acid, 4kg of sodium hydroxide and 4000L of deionized water into the reactor, stir at 250r / min for 30-40min, then add 9.6kg of EDC (1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride) and 11.5kg of NHS (N-hydroxysuccinimide) into the reactor, continue stirring for 8min to activate the carboxyl group in lipoic acid to obtain a modifier solution.

[0022] Step 3: Add 3.2 kg of chitosan and 160 L of deionized water into the reactor, adjust the pH value to 3 with 1 mol / L acetic acid solution, stir at 400 r / min for 25 min, then add 40 L of modifier solution and 18 L of anhydrous ethanol as a water absorbent into the reactor, stir and react at 22 ° C for 17 h to obtain a modified chitosan solution.

[0023] Step 4: 100kg of wood fiber is subjected to hot grinding and defibration to prepare fiber slurry, 55L of modified chitosan solution, 13.25kg of melamine-modified urea-formaldehyde resin, 33.5g of ammonium chloride curing agent and 0.07kg of mildewproof agent powder are added to the fiber slurry, stirred and mixed at 22°C and 600r / min for 25min, dried to a fiber moisture content of 7.5%, spread into a mold, and hot pressed at 198°C and 5.5MPa for 5.5min to obtain a moisture-proof and mildew-resistant medium-density lightweight fiberboard.

[0024] Embodiment 3: This embodiment provides a moisture-proof and mildew-resistant medium-density lightweight fiberboard, which is prepared by the following steps: Step 1: Add 50kg of deionized water, 150kg of tetrahydrofuran, 60kg of tetra-needle zinc oxide whisker and 0.5kg of tetramethylammonium hydroxide into a reactor at 25°C, stir at 3000r / min for 15min, then add 160kg of tridecafluorooctyltrimethoxysilane monomer into the reactor under nitrogen protection, continue stirring for 10min, and then stir and react at 35°C for 26h to make the polymerized fluorinated polysilsesquioxane coat the tetra-needle zinc oxide whisker, remove the solvent and unreacted monomer by rotary evaporation, wash the reaction product with anhydrous ethanol and deionized water for 3 times respectively, and vacuum dry to obtain a mildew inhibitor powder.

[0025] Step 2: Add 20kg of α-lipoic acid, 4kg of sodium hydroxide and 4000L of deionized water into the reactor, stir at 300r / min for 30-40min, then add 9.6kg of EDC (1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride) and 11.5kg of NHS (N-hydroxysuccinimide) into the reactor, continue stirring for 10min to activate the carboxyl group in lipoic acid and obtain a modifier solution.

[0026] Step 3: Add 3.2 kg of chitosan and 160 L of deionized water into the reactor, adjust the pH value to 3 with 1 mol / L acetic acid solution, stir at 500 r / min for 30 min, then add 40 L of modifier solution and 20 L of anhydrous ethanol as a water absorbent into the reactor, stir and react at 25 ° C for 18 h to obtain a modified chitosan solution.

[0027] Step 4: 100kg of wood fiber is subjected to hot grinding and defibration to prepare fiber slurry, 60L of modified chitosan solution, 13.5kg of melamine-modified urea-formaldehyde resin, 33.75g of ammonium chloride curing agent and 0.08kg of mildewproof agent powder are added to the fiber slurry, stirred and mixed at 25°C and 800r / min for 30min, dried to the fiber moisture content of 8%, spread into a mold, and hot pressed at 200°C and 6MPa for 6min to obtain a moisture-proof and mildew-resistant medium-density lightweight fiberboard.

[0028] Comparative Example 1: Based on Example 3, the modified chitosan solution and the mildew inhibitor powder were not added in step 4, and the other steps remained unchanged to prepare a medium-density lightweight fiberboard.

[0029] Comparative Example 2: Based on Example 3, the modified chitosan solution was not added in step 4, and the other steps remained unchanged to prepare a medium-density lightweight fiberboard.

[0030] Comparative Example 3: Based on Example 3, no mildewcide powder is added in step 4, and the other steps remain unchanged to prepare a medium-density lightweight fiberboard.

[0031] Comparative Example 4: Based on Example 3, in step three, 3.2 kg of chitosan and 160 L of deionized water are added to the reactor, the pH value is adjusted to 3 with 1 mol / L acetic acid solution, and stirred at 500 r / min for 30 min. The obtained chitosan solution is used to replace the modified chitosan solution in step four, and the other steps remain unchanged to prepare a medium-density lightweight fiberboard.

[0032] Comparative Example 5: Based on Example 3, in step 4, the mildewcide powder is replaced with tetrapod-shaped zinc oxide whiskers of the same mass, and the other steps remain unchanged to prepare a medium-density lightweight fiberboard.

[0033] Performance tests were performed on Examples 1 to 3 and Comparative Examples 1 to 5. Different medium-density lightweight fiberboards were cut into samples of 5 cm × 5 cm × 2 cm. The mildew resistance levels of different samples were tested with reference to JIS Z 2801-2000 "Antibacterial processed products - Antibacterial test methods and antibacterial effects". The test bacteria used were Aspergillus niger (CFCC 82449) and Trichoderma viride (CFCC 85491). The mildew resistance levels after 14 days were observed and recorded (0-4 levels, no mycelium on the surface of the 0-level sample, 1-level sample surface infection area ≤10%, 2-level sample surface infection area ≤30%, 3-level sample surface infection area ≤70%, 4-level sample surface infection area >70%). After soaking different samples in clean water for 24 hours, the water absorption rate was calculated (water absorption rate = (mass after soaking - mass before soaking) / mass before soaking × 100%), and then the mildew resistance levels of the soaked and dried samples were tested using the same method. The results are shown in Table 1: Table 1

[0034] It can be seen from Table 1 that the medium density light fiberboard in Example 1 to Example 3 has a lower water absorption rate and a higher mildew resistance level, and still has a high mildew resistance level after soaking for 24 hours. The comparative example shows that the modified chitosan solution and the mildew resistance powder synergistically improve the mildew resistance level of the fiberboard. The coated modified mildew resistance powder and the disulfide bond modified chitosan solution can improve the waterproof effect of the fiberboard, among which the mildew resistance powder has a greater effect on improving the waterproof effect.

[0035] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0036] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A moisture-proof and mildew-resistant medium-density lightweight fiberboard, characterized in that: Prepared by the following steps: The fiber slurry is prepared by heat grinding and defibration of wood fiber, and modified chitosan solution, melamine modified urea-formaldehyde resin, ammonium chloride curing agent and mildewproof agent powder are added to the fiber slurry, stirred and mixed at 20-25°C and 500-800r / min for 20-30min, dried to the fiber moisture content of 7-8%, spread into a mold, and hot pressed at 195-200°C and 5-6MPa for 5-6min to obtain a moisture-proof and mildew-resistant medium-density lightweight fiberboard.

2. The moisture-proof and mildew-resistant medium-density lightweight fiberboard according to claim 1, characterized in that: The dosage ratio of wood fiber, modified chitosan solution, melamine modified urea-formaldehyde resin, ammonium chloride curing agent and mildewproofing agent powder is 100g: 50-60mL: 13-13.5g: 0.03325-0.03375g: 0.06-0.08g.

3. The moisture-proof and mildew-resistant medium-density lightweight fiberboard according to claim 1, characterized in that: The antifungal powder is prepared by the following steps: Deionized water, tetrahydrofuran, tetranepal zinc oxide whisker and tetramethylammonium hydroxide are added to a reactor at 20-25° C., and stirred at 2000-3000 r / min for 10-15 minutes. Then, under nitrogen protection, tridecafluorooctyltrimethoxysilane monomer is added to the reactor, and stirring is continued for 5-10 minutes. After that, the reaction is stirred at 35° C. for 24-26 hours to make the polymerized fluorinated polysilsesquioxane cover the tetranepal zinc oxide whisker. The solvent and unreacted monomer are removed by rotary evaporation. The reaction product is washed with anhydrous ethanol and deionized water for 2-3 times respectively, and vacuum dried to obtain a mildew inhibitor powder.

4. The moisture-proof and mildew-resistant medium-density lightweight fiberboard according to claim 3, characterized in that: The mass ratio of deionized water, tetrahydrofuran, tetranepal-shaped zinc oxide whisker, tetramethylammonium hydroxide and tridecafluorooctyltrimethoxysilane monomer is 5:15:5-6:0.05:15-16.

5. The moisture-proof and mildew-resistant medium-density lightweight fiberboard according to claim 1, characterized in that: Modified chitosan is prepared by the following steps: Chitosan and deionized water were added into a reactor, the pH value was adjusted to 3 with 1 mol / L acetic acid solution, and stirred at 300-500 r / min for 20-30 min. Then, the modifier solution and anhydrous ethanol as a water absorbent were added into the reactor, and the reaction was stirred at 20-25° C. for 16-18 h to obtain a modified chitosan solution.

6. The moisture-proof and mildew-resistant medium-density lightweight fiberboard according to claim 5, characterized in that: The dosage ratio of chitosan, deionized water and modifier solution is 3.2 g: 160 mL: 40 mL: 15-20 mL.

7. The moisture-proof and mildew-resistant medium-density lightweight fiberboard according to claim 5, characterized in that: The modifier solution was prepared by the following steps: Add α-lipoic acid, sodium hydroxide and deionized water into a reactor, stir at 200-300 r / min for 30-40 min, then add EDC (1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride) and NHS (N-hydroxysuccinimide) into the reactor, continue stirring for 5-10 min to activate the carboxyl group in lipoic acid and obtain a modifier solution.

8. The moisture-proof and mildew-resistant medium-density lightweight fiberboard according to claim 7, characterized in that: The usage ratio of α-lipoic acid, sodium hydroxide, deionized water, EDC and MHS is 0.2g:0.04g:40mL:0.096g:0.115g.

Citation Information

Patent Citations

  • Dye wastewater absorbent prepared by compounding lignocellulose and calcium-based montmorillonite

    CN102416312A

  • Antibacterial biological activity stent and preparation method thereof

    CN103007345A

  • Composite multifunctional polyethylene flame retardation chitin wooden fiber plastic floor sheet material

    CN103205043A

  • Digestive tract multi-region liquid biopsy sampling device

    US20200237350A1