Molding composition comprising a sugar component
By using a molding composition with high content of sugar components as the disappearing mold material, the problems of toxicity, expensiveness and insufficient mechanical stability of the existing disappearing mold materials are solved, and efficient removal and good molding effects of complex shape workpieces are achieved.
Patent Information
- Application Number
- CN202410855764.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2018-12-20
- Filing Date
- 2019-12-20
- Publication Date
- 2024-11-26
AI Technical Summary
Existing disappearing mold materials, such as low melting point metal alloys and thermoplastics, have problems such as toxicity, expensiveness, insufficient mechanical stability and difficulty in removing, especially when manufacturing workpieces of complex shapes.
A molding composition containing at least 20% sugar component is used as the disappearance mold material, which has low porosity, high strength and good moldability, is easy to melt or burn out, and is suitable for forming complex internal structures.
Good mechanical stability and efficient removal of the vanishing mold materials used in various molding methods are achieved, reducing production costs and improving the surface strength and density distribution of the workpiece.
Smart Images

Figure SMS_2 
Figure SMS_3 
Figure SMS_5
Abstract
Description
[0001] This application is a divisional application of the patent application with application number 201980085278.4 filed on December 20, 2019 and invention name “Molding composition including sugar component”. Technical Field
[0002] The invention relates to a molding composition comprising at least one sugar component, a mold consisting of the molding composition for use in a molding method, and a method for molding a workpiece using the mold. Background Art
[0003] Molds, in particular lost foam molds, are used, for example, in the production of metallic, ceramic or polymer workpieces, by pressing, transfer molding, casting, injection molding, powder injection molding, or in the case of fiber composite workpieces by lamination processes, for molding workpieces using various molding methods. In this case, the mold is usually a negative mold of at least a part of the three-dimensional design of the workpiece.
[0004] As used herein, the term "mold" refers to a pattern, particularly a lost foam mold, lost foam core, or support structure.
[0005] Complex-shaped metal, ceramic or polymer workpieces - for example with cavities or so-called undercuts - cannot usually be produced using demoldable or removable tools by pressing or casting processes, since the internal or undercut molded parts cannot be removed at the end of the molding process for mechanical reasons. In order to be able to produce such workpieces, so-called lost foam or lost foam cores are used in the technology, which can be removed by dissolving in water or other liquids, by melting or by thermal decomposition or combustion, forming liquid, gaseous or loose powdery decomposition products. In other cases, removable tools are technically possible but are not economical compared to lost foam.
[0006] 1. Melting core-injection molding (lost core injection molding)
[0007] In the injection molding process, plastics (polymers) are primarily processed: mostly thermoplastic but also thermosetting or elastic plastic powders, granules or pastes are heated to plasticization in a heated cylinder with a plunger or rotating screw (extruder) to 150-300° C., compressed and then injected into a molded, water-cooled, mainly steel, two-component cavity at a pressure of 500-2000 bar. After cooling and hardening or vulcanization, the workpiece can be removed by opening the cavity. In order to be able to produce workpieces with cavities or undercuts, expendable molds or mold cores are also used here: these cores are firstly made of low-melting metal alloys (fused alloys), such as Wood's metal or Ross metal, by casting, which are removed from the injection molding by melting, or, for example, consist of water-soluble polyacrylate polymers, which are themselves produced by injection molding. Melt core injection molding can also be used to produce fiber-reinforced plastic workpieces, see, for example, EP 1 711 334 A2. When melting the molten alloy, it must be ensured that the metal mold core remains stable and plastic for a sufficiently long time at the selected injection molding temperature and that the plastic workpiece is not subsequently thermally affected at the necessary melting temperature (Michaeli, W.; Greif, H.; Kretzschmar, G.; Ehrig, F., Injection Molding Technology, 3rd edition; Hanser: Munich, 2009).
[0008] 2. Powder injection molding (powder injection molding)
[0009] A further development of the injection molding method for plastics described above is the so-called powder injection molding, which is also called metal injection molding when applied to sinterable powders such as metal powders (usually sintered ferrous and non-ferrous metals, hard metals, metal composites), also called ceramic injection molding when applied to ceramic powders (usually ceramics (cermets), oxide ceramics, nitride ceramics, carbide ceramics and functional ceramics), also called ceramic injection molding, and to special polymer powders such as Teflon. In this case, an injection molding mass consisting of metallic, ceramic or polymer particles (or a mixture of these particles), auxiliary materials such as lubricants and (organic) binders is used. After injection molding, the so-called green body is mostly removed by dissolving the binder in water or a suitable solvent or by heat treatment. The brown body thus obtained, which is almost free of binders, is then sintered in a material-specific thermal process to form the finished workpiece. In a variant of the method, special binders can also be left in the green body in a targeted manner in order to change the properties of the workpiece. Composite materials such as fiber composite materials can also be produced by powder injection molding. Analogous to basic normal injection molding—as described above, lost foam or lost foam cores can also be used in powder injection molding in order to be able to produce workpieces with cavities and undercuts (“Powder injection molding”; Volker Piotter et al., Wiley Encyclopedia of Composite Materials, 2nd edition (2012), 4, 2354-2367; “Recent Advances in CIM Technology”; BS Zlatkov et al., Sintering Science, 40, 2008, 185-195).
[0010] 3. Suppression
[0011] For example, the sinterable metal, ceramic or polymer powders described in 2. Powder injection molding can also be processed into workpieces by discontinuous pressing processes, wherein composite materials such as fiber composite materials can also be produced. For this purpose, a pressing mass composed of ceramic, metal or polymer particles, auxiliary materials such as lubricants and (organic) binders is produced, and these pressing masses are introduced into a pressing mold (pressing mold) made of wear-resistant steel or hard metal. The pressing mass can be processed dry (dry pressing) or wet (wet pressing), cold (cold pressing), warm (hot pressing) or hot (pressure sintering). By shaking (vibration compaction), uniform distribution of the pressing mass - especially important for complex shapes - and initial compaction can be achieved. By a pressing plunger (uniaxial pressing) or several pressing plungers (coaxial pressing), a green body is produced from the pressing mass at a pressure of from several hundred bar to 10,000 bar. In contrast to liquids, the pressure is not evenly distributed in all directions here, and the lateral material flow is small; here, due to internal friction and friction with the die, the resulting compression of the green body decreases with increasing distance from the pressing plunger or plungers.
[0012] In order to avoid this disadvantage, so-called isostatic pressing is increasingly used: Here, the molding compound to be pressed - mostly dry and powdered - is placed in a closable elastic mold (for example made of polyurethane, silicone or rubber) and is usually pre-compressed by shaking (vibration compression). The mold is now placed in a so-called receiver (pressure-resistant, closable container) which is filled with a liquid (usually water, oil or an oil-water mixture), rarely a gas, and is sealed. The pressure in the receiver is increased to several hundred to several thousand bar by a hydraulic system (gas compressor), and then, due to the uniform pressure distribution in the liquid or gas, the mold is isostatically pressed from all sides, so that compression does not occur axially, but from the outside to the inside. In addition, compared with the axial pressing method, the particles to be compressed in isostatic pressing travel a much shorter distance. This results in the green body produced having its highest degree of compression and therefore also the highest surface strength after sintering, which is also required in the finished workpiece, wherein the gradient of the density distribution and the resulting strength distribution is significantly lower than in the axial pressing process. Isostatic pressing is usually carried out cold (cold isostatic pressing), but can also be carried out hot (hot isostatic pressing) when a gas such as argon is used as the pressure medium and an elastic mold made of a metal container (so-called chamber) is used, wherein pressure sintering is also possible in the latter case. After the isostatic pressing process is completed, the excess pressure of the pressure medium is released and the green body is removed from the elastic mold. The further processing of the sintered end product is similar to 2. Powder injection molding, wherein the binder is also removed in this case by subsequent process steps or can be deliberately retained in the green body.
[0013] Analogously to the above-described methods, for uniaxial, coaxial or isostatic pressing, it is also possible to use lost foam or lost foam cores made of water-soluble, fusible or burnable substances in order to be able to produce workpieces with cavities and undercuts. Depending on the requirements of the pressing process (pressure, temperature), the sintering material used, the shape of the workpiece, etc., cores made of, for example, low-melting-point metals, salts, waxes, foamed or dense plastics or other decomposable materials can also be used here ("Introduction to Powder Metallurgy; Processes and Products"; 6th edition, 2010; European Powder Metallurgy Association (EPMA) Handbook, SY2 6LG Shrewsbury, UK; available from "Powder Metallurgy Association" eV, 58093 Hagen, Germany; www.pulvermetallurgie.com ).
[0014] 4. Investment Casting
[0015] In the investment casting process, a lost pattern of the workpiece is produced from a special fusible or water-soluble wax (for example based on polyethylene glycol or polyacrylate) or a burnable thermoplastic (for example made of foamed polyurethane or polystyrene), for example by injection molding technology, using aluminum or steel tools. In order to produce cavities or undercuts, this pattern can also be provided with a water-soluble, fusible or burnable lost core. The pattern is then immersed in a so-called slurry, a ceramic substance for producing a mold shell, which consists of refractory fine powder and a binder, such as ethyl silicate. The pattern moistened with the slurry is then sprinkled with sand and dried. The dipping and sprinkling with sand are repeated until the refractory mold shell has reached the desired stability. The water-soluble core is now dissolved and removed in a water bath, and the fusible core is removed by heat treatment, for example using steam. The mold shell is now fired at approximately 750-1200° C., wherein the burnable core or core residue is removed without residue. The actual metal casting (e.g. steel and alloys based on iron, aluminum, nickel, cobalt, titanium, copper, magnesium or zirconium) is then placed into the ceramic mold shell and the cooled workpiece is reworked. The castings obtained in this way are distinguished by their level of detail, dimensional accuracy and surface quality. Investment casting tends to serve shortfalls in the high-performance market segment in smaller quantities ("Investment Casting: Manufacturing, Performance, Applications"; Handbook of the German Foundry Industry Association, 2015, www.kug.bdguss.de; Gessereilexikon. 19th edition, Stephan Hasse, 2007; Schiele and Publishing House, ISBN 978-3794907533).
[0016] 5. Laminated fiber plastic composites
[0017] Modern fiber-plastic composite materials consist of a matrix (which consists, for example, of a thermosetting plastic such as a synthetic resin, etc., and rarely of a thermoplastic) and a plurality of layers stacked one above the other with different main fiber directions, which consist of fiber fabrics, nonwovens, knitted fabrics, mats, tiles, etc. In particular, tear-resistant fibers such as glass fibers, carbon fibers (carbon fibers), ceramic fibers, polyaramid fibers, steel fibers, polyamide fibers, polyester fibers, cellulose fibers, etc. are used here. In manual lamination technology, the fibers are placed on the molded body and impregnated with the matrix that has not yet hardened / cured. By pressing with a roller, the layer is compressed, degassed and the excess matrix is removed. This process is repeated layer by layer until the desired material thickness is reached. The workpiece is then thermally cured at normal pressure or in a vacuum until the matrix material is solidified. Other lamination processes that can be automated are resin transfer molding (RTM), high-pressure resin transfer molding (HD-RTM) and structural reaction injection molding (SRIM).
[0018] Here too, lost-waxing processes are used for complex workpiece geometries with cavities and undercuts. An example of this is a CFK mountain bike handlebar, which was manufactured using the process from the CAVUS project (see http: / / www.polyurethanes.basf.de / pu / solutions / de / content / group / innovation / concepts / Cavus and http: / / www.ktm-technologies.com / projekte / cavus ): Lost foam and lost foam cores made of a sand-binder mixture are used here to produce extremely light but strong, complex-shaped and hollow mountain bike handlebars. Here, the lost foam core is covered with a carbon fiber braided hose and processed into the finished workpiece in a few minutes at 200 bar in the HD-RTM process. The lost foam core is then removed in a water tank, where the water-soluble binder is dissolved.
[0019] According to the methods (1.-5.), the lost foam in the prior art is therefore formed by metals or alloys, thermoplastics or waxes with low melting temperatures. These materials themselves or during their processing have many disadvantages:
[0020] Low melting point alloys such as Wood's metal, Ross's metal, etc., although they can be reused to a limited extent, are toxic due to the heavy metals they contain, such as lead and cadmium. The relatively high density makes handling difficult, especially when the core volume is large due to the weight. Modern heavy metal-free melting alloys, such as those based on indium, bismuth and tin, are non-toxic, but their prices are several orders of magnitude higher.
[0021] Table 1: Properties of low melting point metals and molten alloys
[0022]
[0023] Source: http: / / www.matweb.com; Journal of Biomechanical Engineering, 2006, 128, 161;
[0024] https: / / www.azom.com / properties.aspx?ArticleID=590;
[0025] Characteristics of Lead-Free Solders, NIST Database Version 4.0, 2002:
[0026] https: / / www.msed.nist.gov / solder / NIST_LeadfireSolder_v4.pdf .
[0027] Table 1 shows the mechanical properties of such molten alloys and some of their alloy components. Pure metals lead, tin and indium are generally not suitable as core materials due to their softness, and pure indium is too expensive. Pure bismuth is significantly harder and therefore suitable for cores, but, as mentioned above, is also relatively expensive; it is also relatively brittle and breaks quite easily. The molten alloys listed already show relatively good hardness, but are either toxic (alloy components Pb, Cd) or very expensive (alloy component In). Bismuth-tin alloys appear to be relatively suitable (hardness, tensile strength, toxicity), but the price is also between 100 and 200 euros per liter. In addition to lead and cadmium, according to the GESTIS database of the German Institute for Labor Protection, statutory accident insurance, they are classified as "hazardous waste according to the waste catalogue ordinance (AVV)", (http: / / gestis.itrust.de), and thus incur disposal costs. As is known to the person skilled in the art, the melts of the mentioned metal alloys show a maximum viscosity of several mPa·s, which, when melted in the lost foam or lost foam core, together with the high density, makes it easy to discharge from cavities with narrow cross sections. However, it is foreseeable that metal residues are unavoidable and may lead to the generation of problematic metal and metal oxide vapors during processing at the more or less high temperatures required for the various forming processes (especially in the case of alloys containing heavy metals) and may also burden the final product.
[0028] Compared to the above metals, for example, lost foam and lost foam cores made of thermoplastics are several orders of magnitude cheaper and thus may be more economical for disposable use as opposed to metals. The density of suitable plastics is about 0.9 to 1.2 g / cm 3 The density of the alloy is within the range of 1.5 to 2.5 mm / s (see Table 2) and is therefore significantly lower than the density of metal alloys, which facilitates the processing of large mold cores.
[0029] Table 2: Properties of selected plastics (guide values)
[0030]
[0031] Source: https: / / www.kern.de / de / richtwerttabelle
[0032] Plastics often have higher tensile strength than metal alloys, have modulus values ten times smaller, and exhibit significantly better elasticity, which in the above-mentioned method leads to higher mechanical stability of the lost foam core (less prone to tearing of the structure due to shear forces) during the molding of the molded part under anisotropic pressure conditions, but also leads to greater deviations from the given geometry of the workpiece. In contrast to metal lost foam cores, it is not possible to remove them from the workpiece simply by melting and draining, because the naturally high viscosity of the plastic melt (high molecular weight) (approximately 100 to several 1000 Pa·s) is ten times higher than that of the above-mentioned metals (Plastics Paperback; Oberbach, Saechtling, 28th edition, Hanser Munich 2001, ISBN 978-3-446-21605-1). In order to be able to remove mold cores made of plastic without residue, they must therefore a.) either be soluble in a solvent or b.) decompose completely into gaseous components at high temperatures (protective gas, such as is required when sintering carbon-containing ceramics or carbides; this is usually unsuccessful because carbonization occurs) or burn (air).
[0033] In order for the dissolution of water-soluble or other plastics in organic solvents to be economical, this must take place quickly enough and the disposal costs or re-preparation costs of the resulting solution must remain within acceptable limits. Since solutions of plastic polymers also have a high viscosity, the dissolution process is, as expected, relatively slow, especially when it can no longer be accelerated by mechanically generated turbulent flows or thermally generated turbulent convection. This also applies to situations where the material has to change direction several times while dissolving and emerging from the cavity. In the case of cavities or undercut structures of the tool to be produced, which are, for example, located deep inside, i.e. at a great distance from the surface or with a very small cross section, the dissolution process becomes increasingly diffusion-controlled and is therefore slower.
[0034] The thermal decomposition or combustion of the plastic core can only take place if the workpiece can withstand the temperature, duration and atmosphere (oxidizing, inert, reducing) required for this. During the decomposition process itself, large amounts of hot gases are naturally produced, which must be able to escape freely from the cavities or undercuts of the workpiece, because otherwise the pressure generated can lead to damage or destruction of the workpiece. Due to the high viscosity of the polymer melt produced before the thermal decomposition, problems arise in narrow and / or angular or complex, interconnected cavities or undercuts of the tool to be produced, when the escape of the gases is made more difficult or prevented by blocked still molten areas.
[0035] In principle, when thermally removing the lost plastic mold core, the decomposition gases generated need to be post-treated. Most of these decomposition gases contain toxic components (such as NOx, polycyclic aromatic hydrocarbons, monomers, etc. in polyurethane).
[0036] Cores made of water-soluble waxes (eg based on polyethylene glycol) or water-insoluble waxes (eg paraffin) can only be used to a very limited extent at relatively low pressures, such as in investment casting, due to their softness. Summary of the invention
[0037] The object is therefore to propose a composition which overcomes the aforementioned disadvantages and can be used as a lost foam in a variety of different processes. This means that a mold can be produced from the composition which has both good mechanical stability and, at the same time, the best removability.
[0038] Brief description of the invention
[0039] This object is achieved by a molding composition comprising:
[0040] at least one sugar component, whose weight fraction, relative to the weight of the molding composition, is at least 20%, preferably at least 50%, particularly preferably at least 80%; and
[0041] - At least one additive (aggregate).
[0042] This object is also achieved by a mold for a molding method, wherein the mold is a dense three-dimensional structure consisting of the molding composition according to the invention. This means that the molding composition according to the invention itself (without other fillers) can be used to produce the mold.
[0043] In another aspect, the present invention relates to a method for molding a workpiece, the method comprising the steps of:
[0044] - providing at least one mould;
[0045] - bringing the mold into contact with the material to be molded;
[0046] - Hardening the material to be moulded so as to obtain a workpiece;
[0047] - remove the mold from the tool;
[0048] It is characterized in that
[0049] At least one mold is a mold according to the invention, ie a compact three-dimensional structure consisting of the molding composition according to the invention.
[0050] The molding compositions according to the invention comprise the sugar component as a major constituent, preferably as a major constituent in terms of quantity.
[0051] Sugar components refer to monosaccharides, disaccharides or oligosaccharides (sugars / saccharides) or sugar alcohols derived from such sugars, hydrates of sugars or sugar alcohols or mixtures thereof. Sugars and sugar alcohols are long-known, extremely cheap, non-toxic and readily available substances, which are widely used in the field of food production as sweeteners, or in the production of pharmaceutical preparations, for example as tablet bases or as other auxiliary agents ("pharmaceutical auxiliary agents"; Schmidt, Lang, 2013, Govi-Verlag Pharmaceutical Publishing House GmbH, Eschborn, ISBN 978-3-7741-1298-8).
[0052] It has been found that the composition comprising the sugar component can be provided as a dense three-dimensional structure and is suitable, for example, as a mold for various molding methods in the method for molding workpieces according to the present invention. The mold made of the molding composition according to the present invention, due to the glassy surface, low porosity, high strength, low density and good formability, has been proven to be suitable for transmitting a three-dimensional profile when the mold contacts the material to be molded, for example in the production of ceramic workpieces. These molds can be particularly used to form areas located inside, such as undercuts and cavities, because they are easy to melt, burn out or can be dissolved in a hydrophilic solvent such as water due to the sugar component. Therefore, the mold is preferably used as a lost foam. In addition, the sugar component is very cheap, easily available, nontoxic and easy to handle (commercial waste, purification equipment).
[0053] The structure of the mold is achieved when the molding composition is provided as a (cooled) melt or compressed material. The molding composition can be formed by melting the sugar component, mixing with the additive (or vice versa) and pouring the molding composition, for example by pouring into a corresponding silicone mold, so that a mechanically stable mold is obtained after cooling. Other conceivable methods include injection molding, 3D printing or direct pressing without prior melting. These methods are known in food production (for example hard caramel) or the pharmaceutical industry.
[0054] The molding compositions according to the invention and the molds according to the invention further comprise at least one additive.
[0055] The additives have the surprising effect that molds made from the molding composition have a higher mechanical strength. In particular, the formation of cracks and sustained fractures in structures made from the sugar component can be reduced by adding relatively small amounts of additives, compared to molds made from only one sugar component, without impairing formability or other advantageous properties.
[0056] Detailed description of the invention
[0057] According to the present invention, the term sugar component means that it describes monosaccharides, disaccharides or oligosaccharides (synonymously also sugars or saccharides), sugar alcohols derived from such sugars, hydrates of such sugars or sugar alcohols or mixtures thereof. These compounds can be summarized as a subgroup of carbohydrates, whose general name includes both sugars and sugar alcohols obtained by carbonyl reduction (IUPAC. Compendium of Chemical Terminology (Compendium of Chemical Terminology) 2nd Edition ("Gold Book"), compiled by AD McNaught and A. Wilkinson, Blackwell Scientific Publications, Oxford (1997), XML online revised version: http: / / goldbook.iupac.org (2006-), created by M. Nie, J. Jirat, B. Kosata; updated by A. Jenkins, ISBN 0-9678550-9-8, "Carbohydrates"; doi: 10.1351 / goldbook.C00820).
[0058] The prefix "oligo" indicates a compound between a dimer and a higher polymer. Typically, oligomeric structures have 3 to 10 repeating units (IUPAC. Compendium of Chemical Terminology 2nd Edition ("Gold Book"), compiled by AD McNaught and A. Wilkinson, Blackwell Scientific Publications, Oxford (1997), XML online revision: http: / / goldbook.iupac.org (2006-), created by M. Nie, J. Jirat, B. Kosata; updated by A. Jenkins, ISBN 0-9678550-9-8, "oligo" doi: 10.1351 / goldbook.O04282), where the term oligosaccharide should also include carbohydrates composed of 3 to 10 sugar units. Thus, the sugar component may have 1-10 sugar units.
[0059] Sugars or sugar alcohols can be described as compounds of the general formula I:
[0060] C (n*a) H (n*a*2)+2b-2c O (n*a)-c (I)
[0061] in,
[0062] n is equal to 1 to 10, preferably 1 or 2,
[0063] a is equal to 4, 5 or 6,
[0064] b is equal to 0 or 1, and
[0065] c is equal to n-1 or n.
[0066] In monosaccharides or sugar alcohols derived from monosaccharides, n is equal to 1, while in disaccharides or sugar alcohols derived from disaccharides, n is equal to 2. In oligosaccharides, n is equal to 3-10, depending on the number of repeating units.
[0067] For the corresponding repeating units, as variants, four carbon atoms (tetraoses), five carbon atoms (pentoses) and six carbon atoms (hexoses), a may therefore be equal to 4, 5 or 6, preferably 4 or 6, even more preferably 6. Although the term sugar component also includes mixed disaccharides and oligosaccharides with respect to the number of carbon atoms of the individual repeating units, formula I applies only to those sugar components in which the repeating units have the same number of carbon atoms.
[0068] In disaccharides and oligosaccharides, one or more water molecules are formally split by condensation. For each condensation, two H and one O are missing from the total formula, which is reflected in Formula I, because in disaccharides and oligosaccharides, n is greater than 1, and therefore the value of c is greater than or equal to 1 since c is equal to n-1. Then in Formula I, one H2O molecule is formally deducted for each condensation.
[0069] Cyclodextrins are a group of oligosaccharides with 6-8 glucose units connected by α-1,4-glycosidic bonds and forming a ring. By forming the ring, another water molecule is split. Therefore, in the case of cyclic oligosaccharides, c is equal to n. α-cyclodextrin with 6 glucose units has the overall formula C 36 H 60 O 30 , which corresponds to formula I, where n is equal to 6, a is equal to 6, b is equal to 0 and c is equal to n is equal to 6.
[0070] Sugar alcohols are obtained from the corresponding sugars by reduction, which is formally represented by two additional hydrogen atoms in the general formula. For sugar alcohols, b in formula I is therefore equal to 1, while for sugars, i.e. ketoses or aldoses, b is equal to 0.
[0071] In addition, the sugar component can be a hydrate of a sugar or sugar alcohol, or a compound of the general formula I. Sugars such as glucose exist in anhydrous form (anhydrate) or as hydrates. The term "hydrate" here can mean both a variant containing crystal water and an organic hydrate that combines water by addition reaction, which can occur, for example, in aldose. The anhydrous form of the sugar component or the compound of formula I is preferred.
[0072] The at least one sugar component may likewise be a mixture of at least two sugars or sugar alcohols or compounds of the general formula I or hydrates thereof.
[0073] Isomalt is a hydrogenated isomaltulose It consists of approximately equal parts of 6-O-α-D-glucopyranosyl-D-glucitol (GPS, isomalt) and 1-O-α-d-glucopyranosyl-D-mannitol (GPM). This is thus a preferred mixture of two sugar alcohols each derived from a disaccharide.
[0074] Mixtures are preferred in particular when they have a lower melting point than the individual sugar components, a so-called eutectic mixture.
[0075] Due to asymmetrically substituted carbon atoms, monosaccharides, disaccharides, oligosaccharides (saccharides) or sugar alcohols derived from such sugars or compounds of the general formula I can generally exist in different stereoisomers (enantiomers). The generic names or formulas include all conceivable enantiomers, but the naturally occurring enantiomers are always preferred.
[0076] In a preferred embodiment, the at least one sugar component is selected from the group consisting of sucrose, D-fructose, D-glucose, D-trehalose, cyclodextrin, erythritol, isomalt, lactitol, maltitol, mannitol, xylitol and mixtures thereof.
[0077] At least one sugar component usually has a decomposition temperature range and / or a melting point. The term "decomposition temperature range" describes the temperature range in which the sugar component softens under chemical decomposition, such as (strong) caramelization. During caramelization, various reactions occur between the individual molecules of the sugar component, such as condensation and polymerization and the splitting of smaller molecules, so that the original sugar component is decomposed. The final product of the thermal decomposition of the sugar component is CO2 and water under oxidizing conditions and carbon under reducing conditions. In practice, there is usually no difference between the decomposition temperature range and the melting point, and these two values are usually given in the form of mp in the literature, which is "melting point" in English. Here, the melting point is defined as the temperature range when the sugar component changes from a solid to a liquid or gel-like aggregate state without decomposition. As used herein, the melting point includes both the transition from a crystalline solid state to a liquid state and the transition from a glassy solid state to a liquid state (also known as the glass transition temperature). Therefore, the viscosity of the sugar component changes at the melting point. Generally, if the sugar component is heated from a temperature below the melting point to a temperature above the melting point, the viscosity decreases by at least one power of 10.
[0078] In a preferred embodiment, the at least one sugar component has a melting point and a decomposition temperature range, wherein the melting point is below the decomposition temperature range.
[0079] Many sugars decompose strongly even in their anhydrous form below their melting point and caramelize in the process. The actual melting point of sucrose is 185-186° C., wherein decomposition occurs from 160° C. D-fructose (mp 106° C.) or D-glucose (mp 146° C.) cannot be processed by melting either and are therefore not preferred as sugar components. By means of eutectic mixtures with one another, the melting point can be lowered to such an extent that this problem can be solved, for example sucrose (30% w)-glucose (mp 137° C.), sucrose (30% w)-fructose (mp 97° C.), glucose (27% w)-fructose (mp 93.2° C.) (see J. Appl. Chem., 1967, vol. 17, 125).
[0080] For example, D-trehalose (mp 214-216° C.) can be melted without caramelization and only decomposes at 284° C.; also most anhydrous sugar alcohols, such as erythritol (mp 122° C.), isomalt (mp 145-150° C.), lactitol (mp 144-146° C.), maltitol (mp 148-151° C.), mannitol (mp 165-168° C., Td 300° C.) or xylitol (mp 93-94.5° C.), do not show thermal decomposition far above their melting point and can therefore be processed according to the invention (“Pharmaceutical Auxiliary Agents”; Schmidt, Lang, 2013, Govi-Verlag Pharmaceutical Publishing GmbH, Eschborn, ISBN 978-3-7741-1298-8).
[0081] Therefore, particularly preferred sugar components include D-trehalose, isomalt, erythritol, lactitol, mannitol, and a eutectic mixture of sucrose and D-glucose.
[0082] In a preferred embodiment, the molding composition is not hygroscopic or is hygroscopic only above a relative humidity of the ambient air of 80%.
[0083] The hygroscopic properties of the moulding composition, i.e. its ability to absorb moisture from the environment, are mainly determined by the sugar component, but can also be influenced by additives. Some sugars or sugar alcohols are highly hygroscopic, i.e. they absorb even at low relative humidity (rF) of the ambient air. This property is mostly described in the literature or can be determined by the skilled person using conventional methods.
[0084] Hygroscopic sugar components are generally less suitable for the use according to the invention, since the glass transition temperature decreases with uncontrolled absorption of water (see https: / / de.wikipedia.org / wiki / Gordon-Taylor-Gleichung; "Critical water activity of disaccharide / maltodextrin blends"; Sillick, Gregson, Carbohydrate Polymers 79 (2010) 1028-1033), and at below room temperature the sugar or sugar alcohol changes from the glassy state into a plastically deformable rubbery state. As a result, the properties of the compact three-dimensional structure of molding compositions containing such sugar components are less suitable for certain applications. Molding compositions with hygroscopic properties may also be suitable if the mold has a relatively large surface area, is exposed to moist air for a relatively short time or not at all and / or the application allows tolerances.
[0085] As examples of highly hygroscopic sugars or sugar alcohols, D-fructose, D-sorbitol and D-lactose and, to a lesser extent, D-glucose may be mentioned. Slightly hygroscopic and therefore preferred are, for example, the sugars and sugar alcohols already mentioned: sucrose (from 85% rF), D-trehalose (from 92% rF), maltitol (from 80% rF) and xylitol (from 80% rF). The sugar alcohols erythritol, lactitol and mannitol are not hygroscopic. Mixtures of hygroscopic sugars and / or sugar alcohols with non-hygroscopic sugars and / or sugar alcohols (e.g. eutectic mixtures) are themselves not hygroscopic and may therefore be preferred.
[0086] Table 3: Properties of various sugar components
[0087]
[0088]
[0089] * Melting point or decomposition range.
[0090] 1 Molecules 2008, 13(8), 1773-1816.
[0091] 2G. Kumaresan, R. Velraj, and S. Iniyan. 2011. Thermal Analysis of D-mannitolfor Use as Phase Change Material for Latent Heat Storage. Journal of Applied Sciences, 11: 3044-3048.
[0092] 3 https: / / cameochemicals.noaa.gov / chemical / 20064 (retrieved in December 2018).
[0093] 4 Online 4.0, https: / / roempp.thieme.de (retrieved in December 2018).
[0094] 5 BJ Donnelly, JC Fruin and BL Scallet. 1973 Reactions of Oligosaccharides. III. Hygroscopic Properties. Cereal Chem 50: 512-519.
[0095] 6 Peter C. Schmidt, Siegfried Lang, Pharmazeutische Hilfsstoffe (Pharmaceutical Auxiliary Agents) 2013: mp 223° C. (pure anhydrous α-lactose), mp 252.2° C. (pure anhydrous β-lactose), mp 232.0° C. (typical commercial product).
[0096] In a further embodiment, it is preferred that the molding composition according to the invention also contains water, preferably in an amount by weight of up to 10%, relative to the weight of the molding composition.
[0097] In particular, when producing molds from cooled melts, the addition of small amounts of water to the molding composition has shown a clear improvement in the elastic properties, i.e., molds made from aqueous molding compositions exhibit better impact resistance or fracture resistance after scratching than molds made from corresponding anhydrous molding compositions (see Example 2).
[0098] Another component of the molding composition according to the invention is an additive. The additive is preferably present in a proportion by weight of not more than 20%, preferably not more than 10%, relative to the weight of the molding composition.
[0099] For the molding compositions according to the invention, the weight proportions of the three components described result in particular in the following compositions:
[0100] Sugar component: about 70% to about 99%, preferably about 85% to about 99%;
[0101] Additives: about 1% to about 20%, preferably about 1% to about 10%;
[0102] Water: 0% to about 10%, preferably about 0% to about 5%.
[0103] Weight proportions starting from a value of 0% include the meaning that the component is not included in the composition (0%) or is included (>0%). The weight proportions in % are respectively given as weight proportion (m / m) in the total mass of the molding composition.
[0104] The additives may be in the form of powders, fibers or other forms, wherein the additives are preferably solid and blocky at room temperature, that is, they can be provided, for example, as fibers or powders. Preference is given to using additives with a fiber length or particle size <5 mm, for example as fibers with a length of 0.2 mm to 3 mm. With such sizes, the additives can be distributed very well, i.e. evenly, in the molding composition. In a preferred embodiment, at least one additive is in the form of a powder or fiber.
[0105] Small amounts of additives already have a significant effect on the mechanical properties of molds made from the molding compositions according to the invention (see Examples 1C and 1D). The additives in particular suppress the usual tendency of glassy objects to crack or break under sudden pressure. The exact mechanism by which this effect is achieved is not yet clear. Since both crystalline and amorphous regions are to be expected in the structure due to the sugar components, the mechanical properties can be changed simply by influencing the distribution or boundaries of these regions.
[0106] The inventors examined a variety of different materials and forms for the additive and demonstrated numerous advantages for a wide selection of materials and forms (Examples 1C-D).
[0107] In general, the inventors expect that such materials, especially those present as solids, are well suited as additives, have good mechanical properties (high compressive and / or tensile strength), and interact with the sugar components, such as electrostatic interactions (e.g. ion-dipole interactions) and / or hydrogen bonds, but also weak interactions such as van der Waals interactions and hydrophobic interactions.
[0108] Preferably, the additive is insoluble in the sugar component or does not dissolve during the production of the mold. The molding composition is therefore preferably a heterogeneous mixture, wherein the additive is selected so that it can be distributed uniformly in the sugar component or in the melt of the sugar component.
[0109] Here, both oleophilic materials such as coal or polyethylene, and hydrophilic materials such as cellulose are suitable as additives. In contrast, materials that are both hydrophobic and oleophobic, such as perfluorinated polymers (such as polytetrafluoroethylene and polyvinylidene fluoride), have proven to be unsuitable. For such materials, it is expected that there will be no or almost no interaction with the sugar component. For example, the wetting angle between the material of the additive and the liquefied sugar component can be regarded as a relevant criterion, which is preferably less than 160°, more preferably less than 120°.
[0110] It is also preferred that the additive has good thermal stability. In one embodiment, the additive has a melting point or thermal decomposition point higher than the sugar component, which means that the additive is solid and does not thermally decompose even during the production of the mold by melting.
[0111] Suitable materials for the additives may be those known to the person skilled in the art, for example as fillers and / or reinforcing materials in connection with plastics (for example as described in DIN EN ISO 1043-2: 2012-03 Kunststoffe Teil (Plastics Part) 2: Füllstoffe und (fillers and reinforcements)) or as fiber materials in fiber composite materials (described, for example, in https: / / de.wikipedia.org / wiki / Faserverbundwerkstoff), such as fiber-plastic composites (described, for example, in https: / / de.wikipedia.org / wiki / Faser-Kunststoff-Verbund) are known.
[0112] Known fillers and reinforcing materials are, for example, selected from the group consisting of aromatic polyamides, boron, carbon (crystalline, partially crystalline or amorphous, for example carbon fibers, graphite, carbon black, activated carbon, graphene), aluminum hydroxide, aluminum oxide, clay, glass, calcium carbonate, cellulose, metals, minerals, organic natural substances such as cotton, sisal, flax, etc., mica, silicates, synthetic organic substances (such as polyethylene, polyimide), thermosetting plastics, talc, wood, chalk, sand, diatomaceous earth, zinc oxide, titanium dioxide, zirconium dioxide, quartz, starch.
[0113] Known fiber-shaped additives are, for example, selected from the group consisting of inorganic reinforcing fibers (e.g. basalt fibers, boron fibers, glass fibers, ceramic fibers, quartz fibers, silicate fibers), metal reinforcing fibers (e.g. steel fibers), organic reinforcing fibers (e.g. aramid fibers, carbon fibers, PBO fibers, polyester fibers, nylon fibers, polyethylene fibers, polymethyl methacrylate fibers) and natural fibers (e.g. flax fibers, wood fibers, sisal fibers, cotton fibers and products made from these fibers modified by chemical and / or physical treatments).
[0114] Preferably, only one additive is used in the molding composition according to the invention, ie a material in a certain form (eg powder or fibers). However, it is not excluded that the molding composition contains a plurality of additives, ie additives made of different materials and / or in different forms, for example.
[0115] In a preferred embodiment, at least one additive is selected from the group consisting of cellulose, carbon, glass, aramid, alumina, silica and polyethylene, preferably cellulose and carbon, more preferably glass fiber, cellulose fiber and carbon fiber.
[0116] A mold according to the invention suitable for use in a molding process is a dense three-dimensional structure made from a molding composition according to the invention. The term "dense three-dimensional structure" means that the mold forms a shape-stable body of a specific design / geometry. The body is preferably formed uniformly and integrally from the molding composition.
[0117] In the mold according to the invention, the heterogeneous characteristics of the mold composition can also be observed macroscopically or under an optical microscope. In one embodiment, it is a heterogeneous (two-phase) structure, in which the additive is distributed as a dispersed phase in the sugar component (as a continuous phase or matrix).
[0118] For the mold according to the invention, which is a structure consisting of the molding composition according to the invention, the expected weight proportion is equal to the weight proportion of the molding composition. Naturally, fluctuations between the composition and the mold can occur here. For example, the water proportion in the mold production can be reduced by evaporation of water compared to the mold composition and is therefore lower in the mold.
[0119] To obtain the structure, the components of the molding composition are provided, mixed and shaped into a three-dimensional body. This last step of the method for producing the mold can be achieved in at least two different ways.
[0120] The molding composition is preferably introduced as a melt into another three-dimensional casting mold, which forms a negative mold of a three-dimensional body and cools, and the mold according to the present invention is to receive the three-dimensional body. Melting is achieved in the following manner: the molding composition is heated to a temperature preferably higher than the melting point within the melting point range of the sugar component. The liquefied molding composition can then be molded by pouring. For melt molding, for example, silicone molds are suitable as casting molds, which, due to their elasticity, can also be removed from complex three-dimensional structures once the three-dimensional structure cools and is thus solid. In this case, the structure is a cooled melt. The cooled melt of the sugar component is also referred to as sugar glass. This method of producing a three-dimensional structure from a cooled melt is, for example, known from food production (for example, for hard caramel or sugar ornaments), and as shown here, can be used not only for sugar components, but also for molding compositions that also contain additives.
[0121] Those skilled in the art can envisage further variants in which the structure composed of the melt is produced from the molding composition by injection molding or 3D printing.
[0122] Alternatively, the molding composition can also be formed into a three-dimensional structure by pressing. For example, it is known from the pharmaceutical industry that sugar components can be formed into a dense three-dimensional structure by pressure. In this case, the structure is a compressed product. For the cohesion in the compressed product or pressed part, cohesion, adhesion, solid bridges or a combination of form fit are taken into account (Bauer KH, K.-H., Führer C., Pharmazeutische Technologie (Pharmaceutical Technology), 5th edition, 1997, Gustav Fischer Verlag, p. 332 "Bindung in Tabletten (Bind into Tablets)"). In particular for molds with relatively simple three-dimensional shapes, it would be preferable to produce the mold by pressing.
[0123] In a preferred embodiment, for the mold according to the invention and the method for molding a workpiece, the structure is a melt or a compact of the molding composition.
[0124] The method for molding a workpiece according to the invention comprises the following steps:
[0125] - providing at least one mould according to the invention;
[0126] - bringing the mold into contact with the material to be molded;
[0127] - Hardening the material to be moulded in order to obtain a workpiece;
[0128] -Remove the mold from the workpiece.
[0129] In one embodiment, the method for molding a workpiece may be used in the following process:
[0130] 1. Melt core-injection method;
[0131] 2. Powder injection molding method;
[0132] 3. Suppression method;
[0133] 4. Production of fiber-plastic composite materials by lamination; or
[0134] 5. For investment casting, manufacture ceramic mold shells.
[0135] The various molding methods (1. to 5.) described above are known in principle. The mold according to the invention is a dense three-dimensional structure made of the molding composition according to the invention, which can replace the known molds, in particular the known lost foam, in these methods. The embodiments with regard to the workpiece, the material to be molded, the hardness step or possible post-treatment are therefore partially derived from the prior art.
[0136] The material to be molded is preferably provided in a flowable, free-flowing or at least plastically deformable state for contacting a mold or, if necessary, multiple molds so as to achieve a shape fit between material and mold when contacting the mold and to transfer the three-dimensional design of the mold when the material hardens.
[0137] In the method according to the invention, the hardening step is regarded as the step in which the mold according to the invention permanently transfers its contour to the material to be molded. In a preferred embodiment, for example in pressing and powder injection molding, additional steps for further processing of the initially obtained workpiece (green body) can also be provided, which steps can also be referred to as hardening steps, but are to be distinguished from the hardening step according to the invention.
[0138] Depending on the type of molding process, the material can be hardened in different ways. Hardening is preferably performed mechanically or mechano-thermally.
[0139] In this embodiment, hardening is preferably carried out by applying pressure to the assembly of mold and material to be molded, which pressure is generated when the mold comes into contact with the material, such as in a pressing method, in particular an isostatic pressing method. When hardening by pressure, the favorable mechanical properties of the molding composition play a special role.
[0140] In molding methods such as molten core injection molding, powder injection molding or methods for producing fiber-plastic composite materials by lamination, the material to be molded (polymeric substance, raw material or layered matrix material) is usually provided at an elevated temperature so that the material contacts the mold in a plasticized state. Hardening is then also carried out by cooling (i.e. in a mechanical thermal manner). In the case of thermal hardening, the person skilled in the art will note that it is preferred to use such a mold according to the invention, wherein the sugar component has a decomposition temperature range and / or a melting point that is not significantly lower than the temperature adopted during contact with the material.
[0141] In a preferred embodiment of the method according to the invention, the structure of the mould is destroyed when the mould is removed.
[0142] In this embodiment, at least one mold according to the invention, which is a dense three-dimensional structure made of the molding composition according to the invention, is therefore a so-called lost foam. The lost foam loses at least its three-dimensional design, shape or geometry, i.e. structure, after transferring them to the material. Optionally, the components of the molding composition also decompose when damaged. At least one mold of the method can be removed by various process steps due to the sugar component, which is the basic component or main component of the molding composition.
[0143] The mold can preferably be removed by:
[0144] - dissolving the molding composition with a hydrophilic solvent, preferably water,
[0145] - melting the sugar component by heating and, if necessary, pouring the composition into a mold,
[0146] - decomposition of the sugar components by heating and, if necessary, shaking out the mold composition (gasification),
[0147] - or a combination of these measures.
[0148] In all cases, the structure of the mold is destroyed and the mold composition can be removed together with the additives. Dissolution and melting are preferred, in which the mold is removed in the liquid state. For heat-sensitive workpieces, dissolution is preferred because high temperatures do not have to be used here. On the other hand, if the further processing of the workpiece already provides for a heat treatment, it can be advantageous to remove the mold by melting. Thus, for ceramic and metal workpieces, after the initial hardening, i.e. the production of the green body, a further thermal hardening step (sintering) is usually provided, which in the method according to the invention can be accompanied by the removal of the mold from the workpiece. The decomposition of the sugar components generally requires higher temperatures than melting and is therefore less preferred, but can be used well to remove possible residues that have not yet been completely removed by melting.
[0149] During the decomposition process, the molding composition is removed at least partially in the gaseous state, ie, in this case it can also be removed from cavities which are particularly difficult to access.
[0150] In the method according to the invention, at least one mold according to the invention is preferably used as an internal mold. An internal mold is also called a mold core or a supporting structure and forms the internal product geometry of the workpiece to be molded.
[0151] In this embodiment, an external mold can be used in addition, which preferably consists of a different material than the mold according to the invention. The external mold can also be designed in multiple parts, such as a separate permanent mold. In the method design using another mold, when the mold is in contact with the material, an arrangement is formed in which a large part of the entire outer surface of the mold, preferably more than 80%, is in contact with the material to be molded. Therefore, the mold according to the invention is at least partially surrounded by the material when it is in contact with the material. The mold forms a cavity model in the workpiece to be molded, while the additional external mold forms an external negative model of the workpiece to be molded.
[0152] Some experiments are disclosed below which illustrate the composition according to the invention and / or contribute to the understanding of the invention. It goes without saying that the design variants are exemplary. BRIEF DESCRIPTION OF THE DRAWINGS
[0153] The accompanying drawings show the various stages of a method for molding a workpiece, in particular:
[0154] Figure 1 Two molds, an inner mold and an outer mold, are shown in side view;
[0155] Figure 2 shows in cross-section the contact of the mold with the material to be molded before hardening (A), after hardening and removal of the outer mold (B), and after rehardening (C) and after complete removal of the mold from the workpiece (D); and
[0156] Figure 3 The molded workpiece is shown in side view. DETAILED DESCRIPTION
[0157] Example 1 - Fabrication and characterization of molds
[0158] A. Mold manufacturing (test strips)
[0159] Two different types of sugar were used for the test measurements. On the one hand, commercially available isomalt ("Isomalt ST-M", Beneo GmbH) and on the other hand, a mixture of sucrose ("Wiener Feinkristallzucker", Agrana Zucker GmbH) and glucose ("Dextropur", Dextro Energie GmbH & Co. KG) was used.
[0160] Isomalt ST-M contains about 2.5% by weight of water and is melted overnight at 155° C. in a closed aluminum container in order to keep the water content constant during the melting process. The sucrose / glucose mixture is mixed with water in a ratio of 62% by weight of sucrose, 14% by weight of glucose and 24% by weight of water (known as "sugar boil"). The sugar mixture is heated to a temperature of 150° C. in a beaker (1000 ml, low type) on a heatable laboratory magnetic stirrer with vigorous stirring (wherein a large amount of water evaporates), and the resulting melt is then immediately processed further. The melt thus obtained generally contains 2-3% by weight of water.
[0161] On the basis of the two sugar melts ("isomaltol ST-M" and sucrose / glucose), the results now produce test bars with dimensions of 4.7 cm x 2.5 cm x 1.0 cm (tactile test) and 7.0 cm x 3.8 cm x 3.5 cm (measurement of strength and V modulus), using commercially available silicone molds as negative molds.
[0162] B. Characterization of molds without additives
[0163] It has been found that in particular Isomalt ST-M is very brittle after pouring and cooling, so that although the test bodies are obviously very strong (it is impossible to break them by hand), they break very easily after scratching or puncturing the surface with a sharp object; in addition, after a short and rapid blow with a hard object (for example with a screwdriver), the test bodies, such as glass, break into many fragments. Here, it was also observed that the test bodies made of Isomalt ST-M have a very strong dispersion in the described properties, which may indicate thermal stress.
[0164] Therefore, attempts have now been made to remove these stresses by annealing. For this purpose, the produced test bodies were cooled once under ambient conditions (room temperature), once at 40° C. (24 hours) and once cured in a freezer (4° C., 24 hours) in order to clarify the differences. The hardness of the test bodies produced differently was assessed by touch (breaking by hand, scratching the surface and breaking by hand, rapid tapping). However, annealing of the test bodies clearly had no positive effect on the hardness and brittleness and the dispersion of these properties of the test bodies studied.
[0165] In another series of experiments, isomalt ST-M was melted in a closed container and mixed with water to obtain a water content of 5% by weight or 10% by weight. In addition, isomalt ST-M was melted in an open container to obtain a water content of 0% by weight. Test bodies were produced using different isomalt ST-M types (0, 2.5, 5, 10% by weight of water), and their hardness was then again assessed tactilely. The test bodies with a higher water content (5% by weight or 10% by weight) were clearly softer than standard isomalt ST-M, clearly no longer brittle, but unfortunately no longer strong enough, because they could be deformed or broken relatively easily by hand. The test bodies without water are extremely susceptible to impacts or mechanical stress, which can be inferred from increased brittleness.
[0166] In another similar test series using a sucrose / glucose mixture, the same effect or trend was observed with Isomalt ST-M.
[0167] Furthermore, during the handling and storage of test bodies made of isomalt ST-M, a clear difference was observed in terms of hygroscopicity compared to sucrose / glucose mixtures: while the former showed a negligible tendency to absorb water in practice, the sucrose / glucose test bodies had a viscous consistency observed after a short time after contact with the open atmosphere, which led to a gradual plasticization of the test body surface within a few hours, making these test bodies unusable. In practice, molds made of sucrose / glucose must therefore be processed immediately or tightly packed for storage, especially in the case of increased humidity.
[0168] C. Tactile Description of Molds Made from Molding Compositions with Additives
[0169] Various additions with isomalt ST-M and sucrose-glucose (as described above) as matrix (sugar component) were investigated in a series of tests (Table 4).
[0170] Table 4: Investigated additives
[0171]
[0172] 1 Order from Sigma-Aldrich
[0173] To produce the molding composition, the corresponding amount of isomalt ST-M is melted as described above, the appropriate amount of additives is provided and carefully distributed evenly in a beaker with a glass rod. The amount of additives is limited to a maximum of 10% by weight, but some additives can only be evenly distributed in the sugar matrix in smaller amounts.
[0174] In order to prevent premature hardening of the material, the resulting mixture was smoothly poured into the corresponding silicone mold and small test bars (4.7 cm x 2.5 cm x 1 cm) were made. Similar to the above method, the mechanical properties of the test bars were tactilely evaluated (breaking by hand, scratching the surface and breaking by hand, rapid tapping) and compared with the properties of the corresponding mold consisting of only the sugar component (Table 5).
[0175] Table 5: Results of tactile-mechanical tests on candy bars containing various additives.
[0176] Composition Comparison with sugar matrix without additives Isomalt ST-M + 10% by weight activated carbon Significantly improved properties Isomalt ST-M + 0.5% by weight aromatic polyamide Improved features Isomalt ST-M + 10% by weight calcium carbonate Improved features Isomalt ST-M + 2% by weight carbon-filler SFR Significantly improved properties Isomalt ST-M + 2% by weight carbon-chopped Significantly improved properties Isomalt ST-M + 10% by weight cellulose fiber Significantly improved properties Isomalt ST-M + 10% by weight of glass fiber (0.2 mm) Improved features Isomalt ST-M + 10% by weight glass fiber (3mm) Improved features Isomalt ST-M + 10% by weight carbon fiber (0.2 mm) Significantly improved properties Isomalt ST-M + 2% by weight carbon fiber (3mm) Significantly improved properties Isomalt ST-M + 10% by weight polyethylene Significantly improved properties Isomalt ST-M + 10% by weight polytetrafluoroethylene Significantly inferior properties Isomalt ST-M + 10% by weight polyvinylidene fluoride Significantly inferior properties Isomalt ST-M + 10% by weight titanium (IV) oxide Improved features Isomalt ST-M + 10% by weight silica gel 60 powder Significantly improved properties Isomalt ST-M + Alumina Powder Significantly improved properties Sucrose-glucose + 10% by weight cellulose Significantly improved properties
[0177] D. Mechanical Description of the Mold Made of the Molding Composition with Additives
[0178] From some of the candidates that performed better than the sugar matrix without additives in the tactile test, larger test bars (7.0 cm x 3.8 cm x 3.5 cm) were produced. The compressive strength, bending strength and V modulus were measured for each of the described. To determine the compressive strength, a test system from Form&Test Testing Systems (www.formtest.de) was used. Model: DigiMaxx C-20, according to DIN EN 993-5 (1998), maximum piston stroke of 15 mm, maximum force of 600 kN, maximum feed pressure of 1 MPa / s. For the measurements, test bars with the following dimensions were cast: 7 cm x 3.8 cm x 3.5 cm.
[0179] To determine the flexural strength or V modulus, a flexural strength machine from Messphysik (www.messphysik.com, Model Midi 5) with a measuring unit up to 500 kN was used. A feed pressure of 0.15 MPa / s (according to DIN EN 993-6, 1995) was used for processing. The V modulus (also called deformation modulus) is related to the E modulus and, like the E modulus, is the first derivative of stress on elongation or deformation. The V modulus is calculated by dividing the curve in the region of ε Br / 2 is determined by creating a regression line, where ε Br is the degree of deformation that occurs at fracture.
[0180] The corresponding measurement results are shown in Table 6 below:
[0181] Table 6: Results for the compressive strength or flexural strength and V modulus (± standard deviation, absolute and relative) for various molding compositions (measured as bars)
[0182]
[0183] 4 times determination, Isomalt ST-M 10 times determination
[0184] It was observed that the compressive strength of all investigated additives or sugar components increased compared to the pure sugar component - but also compared to the molding composition consisting of sugar component and water. Therefore, the molding composition according to the invention is more suitable for processes requiring high compressive strength.
[0185] For the moulds made with isomalt, the flexural strength showed a very high scatter, indicating the presence of mechanical stresses inside the mould. Although no quantitative effect was achieved on the flexural strength of all materials by the additive, a reduced scatter between the different measurements was found. The improved reproducibility of the flexural strength indicates that the mechanical properties of the moulds have been optimised compared to those without the additive. For some mould compositions (containing cellulose and powdered carbon fibres), flexural strengths comparable in magnitude to the tensile strength of metal fusion alloys were achieved (see Table 1).
[0186] Depending on the sugar component, the addition of additives showed different effects on the V modulus. For isomalt, the V modulus tended to decrease, i.e. the elasticity increased, but here in particular a reduction in the dispersion was also achieved. For sucrose / glucose, the additive (10% by weight of cellulose) had the opposite effect. However, in both cases, the V modulus achieved with the additives was in the order of magnitude of the E modulus specified for the plastic used as lost foam (see Table 2).
[0187] Example 2 - Method for molding a ceramic workpiece
[0188] Technical ceramics are usually produced by isostatic pressing (see also point 3 above).
[0189] The mold according to the present invention is used as an internal mold inside a ceramic blank in such a method, which will be described in detail herein with reference to the accompanying drawings.
[0190] first( Figure 1 ), as described in Example 1, the mold 1 according to the present invention is made of a mold composition having isomalt STM as a sugar component and carbon fibers (ground carbon fibers) as an additive by melting and pouring into a silicone mold. The mold composition is heated to 160° C. in a controlled manner (5 hours), stirred with a simple laboratory mixer, and poured into a new silicone mold (20×15×120 mm). After the melt cools, a high-strength and hard casting, i.e., a rod-shaped mold 1, is produced. In addition, an external rubber mold 2 is provided, in which the mold according to the present invention is centrally arranged.
[0191] In the second step ( Figure 2A), the ceramic particles 3 are poured into the external mold as the material to be formed, thereby producing Figure 2 Assembly of B. The outer mould is filled to the edge. Ceramic granules based on alumina graphite and resin binder.
[0192] The rubber mould is closed with a complementary rubber mould and wrapped with a waterproof membrane. The assembly is then pressed using 360 bar of water pressure.
[0193] The rubber mold 2 can be easily removed due to its flexibility. After the pressing process, the ceramic mass 3 surrounds the mold 1 without visible deformation of the mold ( Figure 2 B).
[0194] To remove the mold 2, the assembly is heated to 240°C in a hardening furnace, whereupon the molding composition 4 incompletely flows out of the workpiece 3 to be molded and disappears in the mold 2. The residue can be dissolved in water or only after subsequent burning.
[0195] After hardening, the product is fired by heating to 1000°C under reducing conditions. Here, most of the residues used evaporate, and only a small amount of ash remains in the product 5 ( Figure 2 D). These ashes can be easily removed by water jets.
[0196] By this technique, the final product 5 (see also Figure 3 ) can have internal geometries of varying complexity. The slight shrinkage of the resulting cavity is caused by the shrinkage of the ceramic substance used and not by deformation of the fusible tool. The shrinkage can therefore be taken into account when planning the final geometry in order to achieve an exact geometry.
Claims
1. A molding composition comprising: at least one sugar component, whose weight fraction, relative to the weight of the molding composition, is at least 20%, preferably at least 50%, particularly preferably at least 80%; and - At least one additive.
2. The molding composition according to claim 1, wherein The at least one sugar component is selected from the group consisting of monosaccharides, disaccharides, oligosaccharides, sugar alcohols derived from monosaccharides, disaccharides or oligosaccharides, hydrates thereof, and mixtures thereof.
3. The molding composition according to claim 1, wherein The at least one sugar component is a compound of general formula I: C (n*a) H (n*a*2)+2b-2c O (n*a)-c (I), in, n is equal to 1 to 10, preferably 1 or 2, a is equal to 4, 5 or 6, b is equal to 0 or 1, and c is equal to n-1 or n, It is a hydrate of the compound of the general formula I, or a mixture of at least two compounds of the general formula I and / or their hydrates.
4. The molding composition according to any one of claims 1 to 3, wherein The at least one sugar component is selected from the group consisting of sucrose, D-fructose, D-glucose, D-trehalose, cyclodextrin, erythritol, isomalt, lactitol, maltitol, mannitol, xylitol and mixtures thereof, with D-trehalose, isomalt, erythritol, lactitol, mannitol and a eutectic mixture of sucrose and D-glucose being particularly preferred.
5. The molding composition according to any one of claims 1 to 4, wherein The at least one sugar component has a melting point and a decomposition temperature range, wherein the melting point is below the decomposition temperature range.
6. The molding composition according to any one of claims 1 to 5, wherein The molding composition further comprises water, preferably in an amount of up to 10% by weight, relative to the weight of the molding composition.
7. The molding composition according to any one of claims 1 to 6, wherein The at least one sugar component is not hygroscopic or is hygroscopic only from a relative humidity of 80%.
8. The molding composition according to any one of claims 1 to 7, wherein The at least one additive is contained in a proportion by weight of at most 20%, preferably at most 10%, relative to the weight of the molding composition.
9. The molding composition according to any one of claims 1 to 8, wherein The at least one additive is in powder form or fiber form.
10. The molding composition according to any one of claims 1 to 9, wherein The at least one additive is selected from the group consisting of cellulose, carbon, glass fiber, aramid, alumina, silica and polyethylene, preferably cellulose and carbon.
11. A mold for a molding method, wherein: The mold is a dense three-dimensional structure made of the molding composition according to any one of claims 1 to 10.
12. The mold according to claim 11, wherein The structure is a melt or a compression of the molding composition.
13. The mold according to claim 11 or 12, wherein: The mold is a heterogeneous structure in which the additives are distributed as a dispersed phase in the sugar component.
14. A method for molding a workpiece, comprising the steps of: - providing at least one mold according to any one of claims 11 to 13; - bringing the mold into contact with the material to be molded; - causing the material to be moulded to harden in order to obtain the workpiece; - Removing the mould from the workpiece.
15. The method of claim 14, wherein: The structure of the mold is damaged during removal.
16. The method of claim 15, wherein: The damage to the structure of the mold is carried out in the following ways: - melting the sugar component by heating and removing the mould composition, in particular pouring it out; - dissolving the molding composition with a hydrophilic solvent, preferably water; - decomposing the sugar component by heating and optionally removing the residues of the molding composition; - or a combination of these measures.
17. The method according to any one of claims 14 to 16, wherein: At least one of the moulds is located inside the material to be moulded when in contact, and optionally another mould is brought into contact with the material to be moulded from the outside.
18. The method according to any one of claims 14 to 17, wherein: The method for molding a workpiece is used in the following process: -Manufacture of ceramic mold shells for investment casting; - molten core-injection method; - Powder injection molding method; - a method of suppression; or, - Production of fiber-plastic composite materials by lamination.
19. The method according to any one of claims 14 to 17, wherein: The hardening to obtain the workpiece is carried out mechanically, preferably by applying a pressure to the assembly of the mold and the material to be molded, which pressure is generated when the mold comes into contact with the material.