Composite material plate foam cementing method

By processing steps on the honeycomb core and combining low-temperature ironing, sand blowing and water film verification technology, the problem of uncontrolled bonding quality in the composite honeycomb sandwich structure is solved, achieving higher nesting accuracy and glue The bonding quality reduces the debonding defect rate of the plate bubble.

CN119017716APending Publication Date: 2024-11-26CHENGDU AIRCRAFT INDUSTRY GROUP
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411148458.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing composite honeycomb sandwich structure of the foam adhesive bonding technology has problems such as uncontrolled bonding quality, hollowing or debonding caused by foaming foam, and inaccurate manual assembly, which affects product quality.

Method used

By processing steps on the honeycomb core, cleaning, low-temperature ironing of foam glue, sand blowing and water film failure verification, ensuring that the honeycomb core and composite rib parts are nested in place, and the assembly accuracy is judged by spacing, combined with vacuum bags Curing to improve bonding quality.

Benefits of technology

It effectively avoids the hollowing and debonding caused by foaming of foam, improves the bonding quality, reduces the debonding defect rate of the foam, and ensures accurate nesting and high-quality assembly of composite parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119017716A_ABST
    Figure CN119017716A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of cementing of composite material parts and honeycomb cores, in particular to a composite material plate bubble cementing method which comprises the following steps: processing a honeycomb core, so that a space is formed between the edge of a sleeved composite material rib part and a step surface of the honeycomb core; when the polystyrene foam is ironed, part of the polystyrene foam is pressed into the honeycomb core grids, and part of the polystyrene foam is left on the honeycomb core grids; and performing sand blasting treatment and water film non-breaking verification. Through cooperation of the technical scheme, the problem of foam glue joint of the composite nested structure plate can be effectively solved, and the glue joint quality is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of adhesive bonding technology for composite material parts and honeycomb cores, and in particular to an adhesive bonding method for composite material sheets and foams. Background Technology

[0002] Composite honeycomb sandwich structures are a commonly used composite adhesive bonding structure with wide applications in the aerospace field, such as in fuselage and aileron mechanisms. The composite honeycomb sandwich structure involves bonding composite parts to a honeycomb core, where the honeycomb core is nested within the cavity of a composite rib part, and J-118 expanding foam is used to bond the ribs to the honeycomb core at the bonding interface, as shown in the attached instruction manual. Figure 2 As shown, this is a typical board foam bonding structure.

[0003] Existing foam bonding involves machining the honeycomb core steps to match the depth of the composite material rib's inner cavity. To fit the foam-coated honeycomb core into the composite material rib, the foam is ironed at high temperature and forcefully pressed into the honeycomb core cells. Then, the inner cavity of the composite material rib is roughened by grinding to remove a layer of resin on the surface, increasing the adhesion of the inner cavity. Finally, the honeycomb core is assembled into the inner cavity of the composite material rib by tapping the composite material rib. If it cannot be tapped anymore, it means that the honeycomb core is in place.

[0004] Existing bonding methods have many problems: on the one hand, high-temperature ironing of the foam may cause localized gelation of the foam, and the force applied to the foam core will cause it to foam into the honeycomb core. On the other hand, this manual sanding and roughening method inevitably has areas that are not roughened. Furthermore, since the honeycomb core is nested inside the rib part, it is impossible to observe whether the honeycomb core and the rib part are properly assembled during assembly. The hammering assembly method is not accurate. These factors may lead to uncontrolled quality of the foam bonding area between the honeycomb core and the composite material rib part, resulting in foam debonding defects, i.e., the interface between the rib part cavity and the J-118 foam is not bonded, affecting product quality and delivery. Summary of the Invention

[0005] To address the aforementioned technical problems, this invention proposes a method for bonding composite material sheets and foams, which can effectively solve the problems encountered in the bonding of existing composite material nested structure sheets and foams, and improve the bonding quality.

[0006] This invention is achieved by adopting the following technical solution: A method for bonding composite material foam boards includes the following steps: Step S1. A step for embedding composite rib parts is machined on the honeycomb core. After the honeycomb core and the composite rib parts are fitted together, there is a gap between the edge of the composite rib parts and the step surface of the honeycomb core. Step S2. Clean the honeycomb core to be bonded; Step S3. Iron the expanding foam, pressing part of the expanding foam into the honeycomb core and leaving part on top of the honeycomb core; Step S4. Perform sandblasting on the inner cavity surface of the composite material rib part involved in the board foam bonding, and clean the sandblasted surface; Step S5. Verify that the water film on the inner cavity surface of the composite material rib part after sandblasting and cleaning does not break; Step S6. Without breaking the water film, treat the inner cavity surface of the composite material rib part to keep the inner cavity surface of the composite material rib part dry. Step S7. Fit the honeycomb core with the expanded foam into the inner cavity of the composite material rib part. Determine whether the honeycomb core is properly nested in the inner cavity of the composite material rib part by observing the change in the distance between the edge of the composite material rib part and the stepped surface of the honeycomb core. Step S8. After the nesting is in place, assemble the upper skin and lower skin, seal in a vacuum bag and put into an autoclave for curing.

[0007] When ironing the expanding foam, the ironing temperature should be ≤60℃ and the ironing time should be within 5 minutes.

[0008] The spacing is 2mm.

[0009] The thickness of the foam is 1 mm.

[0010] The water film non-breakage verification specifically refers to: pouring water onto the inner cavity surface of the composite material rib part after sandblasting and cleaning, wetting the inner cavity surface, and observing the water's condition on the inner cavity surface. If a uniform water film is formed on the inner cavity surface and the water film is not broken, it proves that the sandblasting treatment in step S4 meets the requirements; if the water film is broken, mark the location, then perform sandblasting treatment on the marked location, and then perform the water film non-breakage verification again until the water film is not broken.

[0011] Assembling the upper and lower skins specifically refers to: assembling the lower skin onto the tooling, assembling the composite material ribs fitted with the honeycomb core onto the tooling, then placing the surrounding blocks and support blocks, and finally assembling the upper skin onto the tooling.

[0012] In step S6, the treatment of the inner cavity surface of the composite material rib part specifically refers to: wiping the water off the inner cavity surface of the composite material rib part and drying the inner cavity surface with a hair dryer.

[0013] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. In this invention, by widening the steps of the honeycomb core, a gap exists between the edge of the composite material rib and the stepped surface of the honeycomb core after the honeycomb core and the composite material rib are fitted together. Based on traditional sheet foam assembly, this widens the fitting area between the honeycomb core and the composite material rib, which facilitates the ventilation of the foam adhesive and prevents voids or detachment of the foam adhesive at the bonding surface when a large amount of gas generated during foaming cannot be expelled. Furthermore, this technical solution allows for observation of whether the honeycomb core is properly assembled during assembly, preventing excessive gaps between the honeycomb core and the inner cavity of the composite material rib, which could affect the bonding quality of the sheet foam.

[0014] This invention improves the stepped structure of the honeycomb core and controls the quality of the foam adhesive used for ironing the honeycomb core. This allows for the determination of whether the honeycomb core is properly nested within the composite material part by observing the change in the distance between the edge of the composite rib and the stepped surface of the honeycomb core. Compared to the existing method of tapping, this method more accurately determines whether the nesting is correct, thereby controlling the quality of the foam bonding area between the honeycomb core and the composite rib, and reducing the likelihood of foam debonding defects.

[0015] 2. In this invention, the ironing temperature is ≤60℃ and the ironing time is within 5 minutes. This allows the foam to be partially pressed into the honeycomb core while remaining partially on top of it. This prevents the foam from expanding into the honeycomb core instead of the mating composite material ribs, thus avoiding the phenomenon of detachment. It also solves the problem of localized gelation of the foam caused by high-temperature ironing in existing technologies. Once the foam gels, it will no longer expand, leading to detachment defects. Furthermore, by controlling the ironing temperature and time, the thickness of the foam after ironing can also be controlled, facilitating observation of the gap between the honeycomb core and the composite material ribs during subsequent assembly, thereby determining whether the nesting is in place.

[0016] 3. This invention uses sandblasting instead of traditional manual grinding. Sandblasting can make the surface treatment of the inner cavity of the composite material rib parts more uniform and avoid damage to the surface fibers of the composite material rib parts due to improper manual grinding. At the same time, the surface treatment effect is verified by using a water film without breaking, ensuring that all positions of the inner cavity are treated properly, and effectively guaranteeing the bonding quality.

[0017] 4. A defect of plate bubble detachment occurred in the ventral fin adhesive parts of a certain type of aircraft, with a failure rate of 20.3%. Through the synergy of the various technical solutions in this invention, the defect of plate bubble detachment was reduced to 1.9% (1 out of 52 products had plate bubble detachment, the reason for which was that the composite material rib parts of that product were not sandblasted), and the quality of plate bubble bonding was greatly improved. Attached Figure Description

[0018] The present invention will now be described in further detail with reference to the accompanying drawings and specific embodiments, wherein: Figure 1 This is a schematic diagram of the honeycomb core step processing in this invention; Figure 2 A schematic diagram of the existing honeycomb core step processing; Figure 3 This is a schematic diagram of the composite material nested structure plate foam bonding in this invention; Figure 4 A schematic diagram of the foam bonding of an existing composite material nested structure panel; Figure 5 This is a schematic diagram of the foam adhesive heat treatment effect of the present invention. Figure 1 ; Figure 6 This is a schematic diagram of the foam adhesive heat treatment effect of the present invention. Figure 2 ; Figure 7 This is a diagram illustrating the ironing effect of existing expanding foam. Figure 8 This is a time sequence diagram of the ventral fin adhesive plate debonding in this invention; Figure 9 This is a time series diagram of the debonding of the existing ventral fin adhesive plate. Marked in the image: 1. Upper skin, 2. Honeycomb core, 3. Composite material ribs, 4. Lower skin, 5. Foam. Detailed Implementation

[0019] Example 1 As a basic embodiment of the present invention, the present invention includes a method for bonding composite material boards with foam, comprising the following steps: Step S1. A step for embedding the composite material rib 3 is machined on the honeycomb core 2. After the honeycomb core 2 and the composite material rib 3 are fitted together, there is a gap between the edge of the composite material rib 3 and the step surface of the honeycomb core 2.

[0020] Step S2. Clean the honeycomb core 2 to be bonded.

[0021] Step S3. Iron the expanding foam 5, pressing part of the expanding foam 5 into the honeycomb core 2 cells, leaving part of it on top of the honeycomb core 2 cells.

[0022] Step S4. The inner cavity surface of the composite material rib part 3 involved in the board foam bonding is sandblasted and the sandblasted surface is cleaned.

[0023] Step S5. Verify that the water film does not break on the inner cavity surface of the composite material rib part 3 after sandblasting and cleaning.

[0024] Step S6. Without breaking the water film, treat the inner surface of the composite material rib part 3 to keep the inner surface of the composite material rib part 3 dry.

[0025] Step S7. Fit the honeycomb core 2, which has been ironed with foam 5, into the inner cavity of the composite material rib part 3. Determine whether the honeycomb core 2 is properly nested in the inner cavity of the composite material part by measuring the change in the distance between the edge of the composite material rib part 3 and the stepped surface of the honeycomb core 2.

[0026] Step S8. After the nesting is in place, assemble the upper skin 1 and the lower skin 4, seal them in a vacuum bag and put them into an autoclave for curing.

[0027] Example 2 In a preferred embodiment of the present invention, the present invention includes a method for bonding composite material foam boards, comprising the following steps: Step S1. A step for embedding the composite material rib 3 is machined on the honeycomb core 2. After the honeycomb core 2 and the composite material rib 3 are fitted together, there is a gap between the edge of the composite material rib 3 and the step surface of the honeycomb core 2.

[0028] In the existing method of CNC machining of the honeycomb core 2, the steps of the honeycomb core 2 are machined to match the depth of the inner cavity of the composite material rib 3. However, a large amount of gas is generated when the foam 5 is foamed. If the gas cannot be expelled, voids or debonding of the foam 5 will occur at the bonding surface. In this invention, the width of the steps is increased by 2mm based on the depth of the composite material rib 3 during CNC machining of the honeycomb core 2. This ensures a 2mm gap between the edge of the assembled composite material rib 3 and the step surface of the honeycomb core 2, facilitating gas expulsion and preventing gas from being trapped inside the cavity of the composite material rib 3, thus preventing debonding. It also facilitates observation during subsequent assembly to ensure that the honeycomb core 2 is properly assembled within the composite material rib 3.

[0029] Step S2. Clean the honeycomb core 2 to be bonded.

[0030] Step S3. Iron the expanding foam 5. Visually inspect the expanding foam 5 to ensure there are no voids, meaning that the expanding foam 5 has not been completely ironed into the honeycomb core 2 cells. This confirms that part of the expanding foam 5 is pressed into the honeycomb core 2 cells, while part remains on top of the honeycomb core 2 cells. Control the thickness of the expanding foam 5 after ironing to approximately 1mm.

[0031] Step S4. The inner cavity surface of the composite material rib part 3 involved in the board foam bonding is sandblasted and the sandblasted surface is cleaned.

[0032] Step S5. Verify that the water film does not break on the inner cavity surface of the composite material rib part 3 after sandblasting and cleaning.

[0033] Step S6. If the water film is not broken, treat the inner cavity surface of the composite material rib part 3 to keep the inner cavity surface of the composite material rib part 3 dry.

[0034] Step S7. Fit the honeycomb core 2, which has been ironed with foam 5, into the inner cavity of the composite material rib part 3. Determine whether the honeycomb core 2 is properly nested in the inner cavity of the composite material part by measuring the change in the distance between the edge of the composite material rib part 3 and the stepped surface of the honeycomb core 2.

[0035] Step S8. After the nesting is in place, assemble the upper skin 1 and the lower skin 4, seal them in a vacuum bag and put them into an autoclave for curing.

[0036] Example 3 As a basic embodiment of the present invention, the present invention includes a method for bonding composite material boards with foam, comprising the following steps: Step S1. A step for embedding the composite material rib 3 is machined on the honeycomb core 2. After the honeycomb core 2 and the composite material rib 3 are fitted together, there is a gap a between the edge of the composite material rib 3 and the step surface of the honeycomb core 2.

[0037] Step S2. Clean the honeycomb core 2 to be bonded.

[0038] Step S3. Iron the expanding foam 5, pressing part of the expanding foam 5 into the honeycomb core 2 cells, leaving part of it above the honeycomb core 2 cells, and controlling the thickness of the expanding foam 5 after ironing to be approximately b, where a > b.

[0039] Step S4. The inner cavity surface of the composite material rib part 3 involved in the board foam bonding is sandblasted and the sandblasted surface is cleaned.

[0040] Step S5. Verify the water film integrity on the inner cavity surface of the composite material rib part 3 after sandblasting and cleaning. Pour water onto the inner cavity surface of the composite material rib part 3 after sandblasting and cleaning to wet the inner cavity surface. Observe the water's condition on the inner cavity surface. If a uniform water film forms on the inner cavity surface without breaking, it proves that the sandblasting treatment in step S4 meets the requirements. If the water film breaks, mark the location, then perform sandblasting treatment on the marked location, and then perform the water film integrity verification again until the water film does not break.

[0041] Step S6. If the water film is not broken, wipe the water off the inner surface of the composite material rib part 3 and use a hair dryer to dry the inner surface of the inner cavity, so that the inner surface of the composite material rib part 3 remains dry.

[0042] Step S7. Fit the honeycomb core 2, which has been ironed with expanding foam 5, into the inner cavity of the composite material rib part 3. Determine whether the honeycomb core 2 is properly nested in the inner cavity of the composite material part by observing the change in the distance between the edge of the composite material rib part 3 and the stepped surface of the honeycomb core 2. Specifically, when the distance between the edge of the composite material rib part 3 and the stepped surface of the honeycomb core 2 is ab, it is determined that the honeycomb core 2 is properly nested in the inner cavity of the composite material part.

[0043] Step S8. After the nesting is in place, assemble the upper skin 1 and the lower skin 4, seal them in a vacuum bag and put them into an autoclave for curing.

[0044] Example 4 As the preferred embodiment of the present invention, the present invention includes a method for bonding composite material boards with foam, comprising the following steps: Step S1. Machining a step on the honeycomb core 2 for embedding the composite material rib 3, ensuring that the composite material rib 3 is flush with the horizontal surface after fitting the honeycomb core 2. After fitting the honeycomb core 2 and the composite material rib 3, there is a gap between the edge of the composite material rib 3 and the step surface of the honeycomb core 2. Manual fitting at the fitting point of the honeycomb core 2 should be avoided as much as possible, ensuring the CNC-machined surface is as close as possible.

[0045] Specifically, the inner cavity depth of composite material rib part 3 is 18mm, as shown in the attached instruction manual. Figure 2 The existing method is to machine the step width of the honeycomb core 2 to 18mm during CNC machining. (Refer to the attached instruction manual.) Figure 1 In this embodiment, the spacing can be 2mm. In this invention, the step width of the honeycomb core 2 is increased by 2mm, that is, the step width of the honeycomb core 2 is processed to 20mm. When the honeycomb core 2 is CNC machined, the step width is processed to 20mm, so that there is a 2mm gap between the edge of the composite material rib part 3 and the step surface of the honeycomb core 2.

[0046] When the expanding foam 5 foams, it generates a large amount of gas. If the gas cannot be expelled, voids or detachment of the expanding foam 5 will occur at the adhesive surface. The widened 2mm spacing facilitates the expulsion of the gas generated during the foaming process, preventing the gas from being trapped inside the composite material rib part 3 and causing the foam to detach. It also facilitates subsequent assembly by allowing observation of whether the honeycomb core 2 is properly assembled inside the composite material rib part 3.

[0047] Step S2. Clean the honeycomb core 2 to be bonded.

[0048] Step S3. Iron the expanding foam 5 using a temperature-controlled iron at a temperature ≤60℃ for no more than 5 minutes. Press part of the expanding foam 5 into the honeycomb core 2 cells, leaving part above the cells. By controlling the ironing temperature and time, the thickness of the expanding foam 5 after ironing can be controlled to be approximately 1mm, making it easier to observe the gap between the honeycomb core 2 and the composite material rib part 3 during subsequent assembly. The gap is approximately 1mm (in this invention, the step is widened by 2mm, the expanding foam 5 is 1mm thick, and the gap after assembly is approximately 1mm).

[0049] In this invention, by controlling the ironing temperature and time, the ironing effect of the foam adhesive 5 can be as shown in the instruction manual. Figure 5 Included with instruction manual Figure 6 As shown. In the prior art, the ironing method for the expanding foam 5 involves setting the temperature of the electric iron to a very high temperature and ironing the expanding foam 5 forcefully into the honeycomb core 2. The purpose of this is to minimize the volume occupied by the expanding foam 5 so that the honeycomb core 2 can be easily nested into the composite material rib part 3. However, the high-temperature ironing of the expanding foam 5 causes most of it to flow into the honeycomb core 2, creating many voids in the expanding foam 5. This results in the expanding foam 5 into the honeycomb core 2 instead of into the nested composite material rib part 3, leading to board bubble and delamination defects. At the same time, the high-temperature ironing of the expanding foam 5 causes localized gelation of the expanding foam 5, as shown in the attached instruction manual. Figure 7 Instruction manual attached Figure 7 The area circled in the middle shows that the expanding foam 5 has gelled. Once the expanding foam 5 has gelled, it will stop foaming, which will lead to the defect of the foam detaching from the board.

[0050] Step S4. The inner cavity surface of the composite material rib part 3 involved in the board foam bonding is sandblasted. After sandblasting is completed, the sandblasted surface is cleaned.

[0051] Step S5. Verify the water film integrity on the inner cavity surface of the composite material rib part 3 after sandblasting and cleaning. To verify the sandblasting effect, pour a small amount of tap water from top to bottom onto the inner cavity surface of the composite material rib part 3 after sandblasting and cleaning to wet the inner cavity surface. Observe the water's condition on the inner cavity surface. If a uniform water film forms on the inner cavity surface without breaking, it proves that the sandblasting treatment in step S4 meets the requirements. If the water film breaks, the broken area was not sandblasted. Mark this area, then sandblast the marked broken area, and then perform the water film integrity verification again until the water film remains intact. Step S6. If the water film remains intact, immediately treat the inner surface of the composite material rib part 3 to keep it dry. Specifically, wipe the water off the inner surface of the part and then dry it with a hair dryer.

[0052] Step S7. Fit the honeycomb core 2, which has been ironed with expanding foam 5, into the inner cavity of the composite material rib part 3. Determine whether the honeycomb core 2 is properly nested within the inner cavity of the composite material part by observing the change in the distance between the edge of the composite material rib part 3 and the stepped surface of the honeycomb core 2. Refer to the attached instruction manual. Figure 3 Specifically, an approximately 1mm allowance was observed in the fitting area, indicating that the honeycomb core 2 is properly nested within the cavity of the composite material rib part 3. Without widening the step of the honeycomb core 2 by 2mm, i.e., when the step width is 18mm, refer to the appendix of the instruction manual. Figure 4 A layer of expanding foam 5 is laid between the honeycomb core 2 and the composite material rib 3. Therefore, it is difficult to assemble the honeycomb core 2 into the theoretical position. So, the expanding foam 5 is ironed at high temperature to iron it into the honeycomb core 2. During assembly, the composite material rib 3 is usually tapped to make the honeycomb core 2 fit into the composite material rib 3 until the composite material rib 3 can no longer be tapped, which proves that the honeycomb core 2 is assembled in place. In reality, the honeycomb may not be in place (because the thickness of the expanding foam 5 varies depending on the degree of ironing on the honeycomb core 2). There may still be a gap between the composite material rib 3 and the honeycomb core 2. If the gap is too large, it may cause the foam to delaminate. In this invention, the step of the honeycomb core 2 is widened by 2mm, that is, the step of the honeycomb core 2 is 20mm. And by controlling the ironing temperature and ironing time of the expanding foam 5, the thickness of the expanding foam 5 is controlled to be about 1mm. During assembly, the gap between the composite material rib 3 and the honeycomb core 2 is observed. If there is still a gap of about 1mm, it proves that the honeycomb core 2 is assembled in place.

[0053] Step S8. After the nesting is in place, assemble the upper skin 1 and the lower skin 4, seal them in a vacuum bag and put them into an autoclave for curing. Specifically, assemble the lower skin 4 onto the fixture, then assemble the composite material rib part 3 with the honeycomb core 2 onto the fixture, then place the surrounding blocks and support blocks, and finally assemble the upper skin 1 onto the fixture, seal it in a vacuum bag and put it into an autoclave for curing.

[0054] Refer to the instruction manual appendix Figure 8 Included with instruction manual Figure 9 A certain type of aircraft ventral fin adhesive bonding component had a defect of plate bubble detachment, with a failure rate of 20.3%. After adopting the method of the present invention, the defect of plate bubble detachment was reduced to 1.9% (1 out of 52 products had plate bubble detachment, the reason for which was that the composite material rib part 3 of the product was not subjected to sandblasting treatment), and the quality of plate bubble bonding was greatly improved.

[0055] In summary, any other corresponding modifications made by those skilled in the art after reading this invention document, without requiring creative mental effort, based on the technical solutions and concepts of this invention, are all within the scope of protection of this invention.

Claims

1. A composite material board foam bonding method, characterized in that: The following steps are involved: Step S1. machining a step on the honeycomb core (2) for embedding the composite material rib part (3); after the honeycomb core (2) and the composite material rib part (3) are fitted together, a gap exists between the edge of the composite material rib part (3) and the step surface of the honeycomb core (2); Step S2. Cleaning the honeycomb core to be bonded (2); Step S3. Ironing the foam glue (5), pressing part of the foam glue (5) into the cells of the honeycomb core (2) and leaving part of the foam glue (5) on the cells of the honeycomb core (2); Step S4. sandblasting the inner surface of the composite material rib part (3) involved in the board-foam bonding, and cleaning the sandblasted surface; Step S5. Verifying that the water film on the inner surface of the composite material rib part (3) after sandblasting cleaning is not broken; Step S6. The water film is not broken, and the inner surface of the composite material rib part (3) is treated to keep the inner surface of the composite material rib part (3) dry; Step S7. inserting the honeycomb core (2) with the ironed foam glue (5) into the inner cavity of the composite material rib part (3), and judging whether the honeycomb core (2) is properly nested in the inner cavity of the composite material rib part (3) by the change in the distance between the edge of the composite material rib part (3) and the step surface of the honeycomb core (2); Step S8. After being nested in place, assemble the upper skin (1) and the lower skin (4), seal them in a vacuum bag and put them into an autoclave for curing.

2. A composite material board foam bonding method according to claim 1, characterized in that: When ironing the foaming glue (5), the ironing temperature is ≤ 60°C and the ironing time is within 5 minutes.

3. A composite material board foam bonding method according to claim 2, characterized in that: The spacing is 2 mm.

4. A composite material board foam bonding method according to claim 3, characterized in that: The thickness of the foam glue (5) is 1 mm.

5. A composite material board foam bonding method according to any one of claims 1 to 4, characterized in that: The water film unbroken verification specifically refers to: pouring water on the inner cavity surface of the composite material rib part (3) after the sandblasting cleaning is completed, wetting the inner cavity surface, and observing the situation of the water on the inner cavity surface. If a uniform water film is formed on the inner cavity surface and the water film is not broken, it is proved that the sandblasting treatment in step S4 meets the requirements; if the water film is broken, the place is marked, and the marked position is sandblasted again, and then the water film unbroken verification is performed again until the water film is not broken.

6. A composite material board foam bonding method according to claim 5, characterized in that: Assembling the upper skin (1) and the lower skin (4) specifically includes: assembling the lower skin (4) onto the tooling, assembling the composite material rib part (3) fitted with the honeycomb core (2) onto the tooling, placing surrounding stoppers and support blocks, and finally assembling the upper skin (1) onto the tooling.

7. A composite material board foam bonding method according to claim 5, characterized in that: In step S6, treating the inner surface of the composite material rib part (3) specifically refers to: wiping off the water on the inner surface of the composite material rib part (3), and blowing the inner surface dry with a hair dryer.

Citation Information

Cited By

  • Method for cementing front edge structure of complex honeycomb sandwich

    CN119734450A

  • A method of bonding a complex honeycomb sandwich leading edge structure