Hollow silicon dioxide with adjustable structure and preparation method thereof

By gradually mixing polyacrylic acid with ammonia and tetraethyl orthosilicate under heating conditions, hollow silica nanoparticles with adjustable structures are solved, and the problem of difficulty in controlling hollow silica structures in the prior art is achieved. The precise regulation of particle size, shell thickness and pore size has expanded its application potential in many fields.

CN119018901APending Publication Date: 2024-11-26YUNNAN NORMAL UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411158316.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing hollow silica synthesis methods are difficult to achieve precise structure control, limiting their application potential in materials science and engineering.

Method used

By adding a polyacrylic acid gradient to ammonia water under vigorous stirring and gradually adding dropwise with ethanol and tetraethyl orthosilicate solutions under heating conditions, a regular positive-activity spherical particles are formed to form structurally adjustable hollow di-di Silicon oxide nanoparticles, adjust the ratio of polyacrylic acid, ammonia and tetraethyl orthosilicate to control particle size, shell thickness and pore size.

Benefits of technology

The precise regulation of hollow silica structural parameters has been achieved, the composite performance of the material has been enhanced, and the application possibility of it in the fields of drug delivery, catalysis, sensors and energy storage has been expanded.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119018901A_ABST
    Figure CN119018901A_ABST
Patent Text Reader

Abstract

The invention provides hollow silicon dioxide with an adjustable structure and a preparation method thereof, and relates to the technical field of nano materials, tetraethoxysilane is used as a reaction precursor, after ammonia water used as a catalyst is added, hydrolysis reaction is carried out, silicon dioxide with negative charges is generated, polyacrylic acid is gradually aminated along with addition of the ammonia water, and the hollow silicon dioxide with the adjustable structure is obtained. According to the invention, polyacrylic acid, ammonia water and tetraethyl orthosilicate are used as raw materials, regular spherical particles with positive electricity are formed in the reaction, the two particles attract each other to generate hollow silicon dioxide nanoparticles with regular structures and obvious core-shell structures, and electrostatic attraction of the spherical particles generated by silicon dioxide and PAA can be controlled by adjusting the ratio of polyacrylic acid, ammonia water and tetraethyl orthosilicate; therefore, the structure parameters including the particle size, the shell thickness and the pore diameter are regulated and controlled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nanomaterials, in particular to hollow silica with adjustable structure and a preparation method thereof. Background Art

[0002] With the rapid development of science and technology, the research and application of nanomaterials are becoming one of the important research directions in the field of materials science and engineering. In this context, hollow silica, as a nanomaterial with a special structure, has attracted widespread attention. The introduction of hollow silica not only expands the structural design of the material, but also gives it a series of properties such as low density, large surface area, and adjustable pore structure. This structurally adjustable hollow silica is not only widely used in the field of traditional materials, but also widely used in emerging fields such as drug delivery, catalysis, sensors, and energy storage. The introduction of the hollow structure gives silica new performance and application advantages, and has become a research hotspot, but there are still some challenges and limitations in existing technologies and materials. For example, traditional synthesis methods may not meet the demand for precise control of the hollow silica structure, and there may be performance bottlenecks in some applications. Therefore, it is particularly important to study a structurally adjustable hollow silica and its preparation method, which is expected to bring innovative solutions to the field of materials science and engineering. The present invention is intended to provide a wider range of possibilities for its application in various fields through the controllability of the structure. Summary of the invention

[0003] The purpose of the present invention is to provide a hollow silica with adjustable structure and a preparation method thereof, so as to solve the problems raised in the background technology.

[0004] To achieve the above object, the present invention provides the following technical solution: a hollow silica with adjustable structure and a preparation method thereof.

[0005] A method for preparing hollow silica with adjustable structure, characterized in that it comprises the following steps:

[0006] (1) adding a gradient of polyacrylic acid into ammonia water under vigorous stirring, heating to 30° C. and stirring for 5-10 minutes to obtain a mixed solution A;

[0007] (2) slowly adding the obtained mixed solution A into ethanol, heating to 30° C. and stirring for 15-20 min to obtain a mixed solution B;

[0008] (3) adding tetraethyl orthosilicate solution dropwise to the obtained mixed solution B, heating to 30° C. and stirring for 12-15 hours to obtain the product;

[0009] (4) The obtained product is aged at room temperature and then dried to obtain a hollow silica with adjustable structure.

[0010] Furthermore, the polyacrylic acid in step (1) is a polyacrylic acid aqueous solution with a mass fraction of 50%.

[0011] Furthermore, the concentration of the ammonia water in step (1) is 25%-28%.

[0012] Furthermore, the frequency of the gradient addition in step (1) is 0.03 g as a gradient, added once every 10 seconds.

[0013] Furthermore, in the step (1), the ratio of polyacrylic acid to aqueous ammonia is 0.1-0.3 g: 5-15 mL.

[0014] Furthermore, in the step (3), the frequency of adding tetraethyl orthosilicate is 0.2 mL as a gradient, once every 1 hour.

[0015] Furthermore, the aging time in step (4) is 7-10 days.

[0016] Furthermore, the drying method in step (4) is to dry the mixture in a fume hood at a temperature of 30° C. for 5 days.

[0017] Compared with the prior art, the present invention has the following beneficial effects: tetraethyl orthosilicate (TEOS) is used as a precursor of the reaction, and after adding ammonia water as a catalyst, a hydrolysis reaction occurs and negatively charged silica is generated. With the addition of ammonia water, polyacrylic acid (PAA) is gradually aminated, and regular spherical particles with positive charge are formed in the reaction. The two attract each other to generate hollow silica nanoparticles with regular structure and obvious core-shell structure. By adjusting the ratio of polyacrylic acid, ammonia water and tetraethyl orthosilicate, the electrostatic attraction of the spherical particles generated by silica and PAA can be controlled, thereby achieving the regulation of structural parameters including particle size, shell thickness and / or pore size; by adjusting the amount of ammonia water added, the pH value of the solution can be directly adjusted, thereby affecting the charge state and charge density of PAA; ethanol as a solvent affects the dielectric constant of the solution and indirectly affects the intensity of the electrostatic effect; and the addition of TEOS and the formation of the hydrolysis product SiO2 interact with PAA through electrostatic action, affecting the microstructure and performance of the system. This adjustment is very important for controlling the structure of the composite material. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 The electron microscope images of the hollow silica products in each example are shown in Figure a for Example 1, Figure b for Example 2, Figure c for Example 3, and Figure d for Example 4.

[0019] Figure 2Graphs showing particle size distribution of hollow silica products in various examples, wherein Graph a is for Example 1, Graph b is for Example 2, Graph c is for Example 3, and Graph d is for Example 4. DETAILED DESCRIPTION

[0020] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Referring to the accompanying drawings, the present invention provides a technical solution: a hollow silica with adjustable structure and a preparation method thereof.

[0022] Embodiment 1:

[0023] (1) 0.15 g of polyacrylic acid was added in a gradient of 0.03 g at intervals of 10 s into 10 mL of ammonia water under vigorous stirring, heated to 30° C. and stirred for 5-10 minutes to obtain a mixed solution A;

[0024] (2) Slowly introduce the mixed solution A into 250 mL of ethanol, heat to 30° C. and stir for 15-20 minutes to obtain a mixed solution B;

[0025] (3) A total of 1.0 mL of tetraethyl orthosilicate solution was added dropwise to the mixed solution B at a frequency of 0.2 mL per drop at one hour intervals, and the mixture was heated to 30° C. and stirred for 12-15 hours.

[0026] (4) The obtained product is aged at room temperature for 7-10 days to allow the product reaction to be more complete, and then dried in a fume hood at 30° C. for 5 days to obtain a hollow silica with adjustable structure.

[0027] Embodiment 2:

[0028] (1) 0.15 g of polyacrylic acid was added in a gradient of 0.03 g at intervals of 10 s into 10 mL of ammonia water under vigorous stirring, heated to 30° C. and stirred for 5-10 minutes to obtain a mixed solution A;

[0029] (2) Slowly introduce the mixed solution A into 250 mL of ethanol, heat to 30° C. and stir for 15-20 minutes to obtain a mixed solution B;

[0030] (3) A total of 1.2 mL of tetraethyl orthosilicate solution was added dropwise to the mixed solution B at a frequency of 0.2 mL per drop at intervals of one hour, and the mixture was heated to 30° C. and stirred for 12-15 hours.

[0031] (4) The obtained product is aged at room temperature for 7-10 days to allow the product reaction to be more complete, and then dried in a fume hood at 30° C. for 5 days to obtain a hollow silica with adjustable structure.

[0032] Embodiment 3:

[0033] (1) 0.18 g of polyacrylic acid was added in a gradient of 0.03 g at intervals of 10 s into 10 mL of ammonia water under vigorous stirring, heated to 30° C. and stirred for 5-10 minutes to obtain a mixed solution A;

[0034] (2) Slowly introduce the mixed solution A into 250 mL of ethanol, heat to 30° C. and stir for 15-20 minutes to obtain a mixed solution B;

[0035] (3) A total of 1.4 mL of tetraethyl orthosilicate solution was added dropwise to the mixed solution B at a frequency of 0.2 mL per drop at intervals of one hour, and the mixture was heated to 30° C. and stirred for 12-15 hours.

[0036] (4) The obtained product is aged at room temperature for 7-10 days to allow the product reaction to be more complete, and then dried in a fume hood at 30° C. for 5 days to obtain a hollow silica with adjustable structure.

[0037] Embodiment 4:

[0038] (1) 0.18 g of polyacrylic acid was added in a gradient of 0.03 g at intervals of 10 s into 10 mL of ammonia water under vigorous stirring, heated to 30° C. and stirred for 5-10 minutes to obtain a mixed solution A;

[0039] (2) Slowly introduce the mixed solution A into 250 mL of ethanol, heat to 30° C. and stir for 15-20 minutes to obtain a mixed solution B;

[0040] (3) A total of 1.6 mL of tetraethyl orthosilicate solution was added dropwise to the mixed solution B at a frequency of 0.2 mL per drop at intervals of one hour, and the mixture was heated to 30° C. and stirred for 12-15 hours.

[0041] (4) The obtained product is aged at room temperature for 7-10 days to allow the product reaction to be more complete, and then dried in a fume hood at 30° C. for 5 days to obtain a hollow silica with adjustable structure.

[0042] The products obtained in the examples were tested and the electron microscope photos of the examples were taken to obtain Figure 1 It can be seen that the particle size, pore size and shell thickness of the products of each embodiment are different; the particle size distribution diagram of the products of each embodiment measured by the zeta potential instrument is obtained. Figure 2; Among them, Example 1: particle size 42.86nm, pore size 28.70nm, shell thickness 7.08nm; Example 2: particle size 39.95nm, pore size 21.71nm, shell thickness 9.12nm; Example 3: particle size 59.56nm, pore size 28.84nm, shell thickness 15.36nm; Example 4: particle size 31.96nm, pore size 13.72nm, shell thickness 9.12nm; In summary, by adjusting the ratio of polyacrylic acid, ammonia water and tetraethyl orthosilicate, the electrostatic attraction of the spherical particles generated by silica and PAA can be controlled, thereby achieving the regulation of structural parameters including particle size, shell thickness and / or pore size.

[0043] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing hollow silica with adjustable structure, characterized in that: The following steps are involved: (1) adding a gradient of polyacrylic acid into ammonia water under vigorous stirring, heating to 30° C. and stirring for 5-10 minutes to obtain a mixed solution A; (2) slowly adding the obtained mixed solution A into ethanol, heating to 30° C. and stirring for 15-20 min to obtain a mixed solution B; (3) adding tetraethyl orthosilicate solution dropwise to the obtained mixed solution B, heating to 30° C. and stirring for 12-15 hours to obtain the product; (4) The obtained product is aged at room temperature and then dried to obtain a hollow silica with adjustable structure.

2. The method for preparing a hollow silica with adjustable structure according to claim 1, characterized in that: The polyacrylic acid in step (1) is a polyacrylic acid aqueous solution with a mass fraction of 50%.

3. The method for preparing a hollow silica with adjustable structure according to claim 1, characterized in that: The concentration of the ammonia water in step (1) is 25%-28%.

4. The method for preparing a hollow silica with adjustable structure according to claim 1, characterized in that: The frequency of the gradient addition in step (1) is 0.03 g as a gradient, added once every 10 seconds.

5. The method for preparing a hollow silica with adjustable structure according to claim 1, characterized in that: In the step (1), the ratio of polyacrylic acid to ammonia water is 0.1-0.3 g: 5-15 mL.

6. The method for preparing a hollow silica with adjustable structure according to claim 1, characterized in that: The frequency of adding tetraethyl orthosilicate in the step (3) is once every 1 hour in a gradient of 0.2 mL.

7. The method for preparing a hollow silica with adjustable structure according to claim 1, characterized in that: The aging time in step (4) is 7-10 days.

8. The method for preparing a hollow silica with adjustable structure according to claim 1, characterized in that: The drying method in the step (4) is to dry in a fume hood at a temperature of 30° C. for 5 days.

9. A hollow silica with adjustable structure prepared by the preparation method according to any one of claims 1 to 8.

Citation Information

Cited By

  • High-temperature-resistant UV acrylic pressure-sensitive adhesive

    CN120737766A