Cerium-doped zinc oxide nano array carbon-based composite material as well as preparation method and application thereof
By using cerium-doped zinc oxide nanoarray carbon-based composite materials in lithium-ion batteries, the problems of small capacity and poor cycle stability of the negative electrode material of lithium-ion batteries are solved, and higher electrochemical performance and cycle life are achieved.
Patent Information
- Application Number
- CN202411114650.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-26
AI Technical Summary
The negative electrode material of existing lithium-ion batteries has small capacity, insufficient cycle stability and safety, and zinc oxide is easily damaged during the lithiation reaction, resulting in rapid attenuation of electrode performance.
Using cerium-doped zinc oxide nanoarray carbon-based composite material, the zinc oxide seed layer is grown on the carbon-based material and hydrothermal reaction is carried out to form elongated cerium-doped zinc oxide nanorods to improve the specific surface area and lithium ions of the material. Transmission performance.
It significantly improves the cycle life and rate performance of lithium-ion batteries, enhances the electrochemical performance of electrode materials, makes up for the disadvantage of poor conductivity of zinc oxide, and retains its high capacity advantages.
Smart Images

Figure CN119018930A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a cerium-doped zinc oxide nano-array carbon-based composite material and a preparation method and application thereof. Background Art
[0002] Lithium-ion batteries (LiBs) are secondary batteries that rely on the movement of lithium ions between the positive and negative electrodes. + Insertion and deinsertion back and forth between the two electrodes: During charging, Li + The negative electrode is in a lithium-rich state after being deintercalated from the positive electrode and embedded in the negative electrode through the electrolyte; the opposite is true during discharge. As an important component of LiBs, the negative electrode material has an important influence on its energy density, cycle stability, safety, and amplification performance. However, the theoretical specific capacity of the currently commercially available graphite negative electrode material is relatively small, and its lithium storage performance is difficult to meet the needs of high-performance lithium-ion batteries. Therefore, the development of high-performance negative electrode materials is imminent.
[0003] Nano transition metal oxides have good performance as negative electrode materials and have attracted widespread attention. Among them, zinc oxide has the characteristics of high theoretical capacity (987mAh / g), wide source, low cost, and good safety performance. For example, zinc oxide has strong lithium insertion activity, can undergo conversion and alloying reactions with lithium, and has a high specific capacity. However, although zinc oxide can have a high capacity, it often causes irreversible damage such as breakage and shedding of electrode materials due to stress and dendrite growth during the lithiation reaction, resulting in a decrease in the capacity of the electrode material and a greatly shortened cycle life. In addition, during repeated charging and discharging, the electrode material will agglomerate and collapse, which will reduce the specific surface area of the active material and cause rapid attenuation of electrode performance. Summary of the invention
[0004] In view of the above technical problems, the present invention provides a cerium-doped zinc oxide nano-array carbon-based composite material and a preparation method thereof and an application thereof in the preparation of lithium-ion batteries. The preparation method of the present invention is simple in process, and the synthesized composite material has a large specific surface area and good electrochemical performance. The present invention effectively reduces the band gap of zinc oxide through doping modification, improves the electronic conductivity of the material, and in addition, generates oxygen vacancies to expand the lithium ion transmission space, improve the lithium ion transmission performance of the material, and increase its discharge capacity.
[0005] To achieve the above object, the technical solution adopted by the present invention is:
[0006] In one aspect, the present invention provides a method for preparing a cerium-doped zinc oxide nanoarray carbon-based composite material, comprising the following steps:
[0007] Step (1): preparing a zinc oxide seed layer on a carbon-based material;
[0008] Step (2): subjecting the carbon-based material obtained in step (1) to a hydrothermal reaction in an epitaxial growth solution to grow cerium-doped zinc oxide nanorods on the carbon-based material;
[0009] Step (3): soaking the carbon-based substrate grown with cerium-doped zinc oxide nanorods obtained in step (2) in a zinc oxide seed layer precursor solution to obtain secondary seed crystals;
[0010] Step (4): subjecting the carbon-based substrate obtained in step (3) to a secondary hydrothermal reaction in an epitaxial growth solution;
[0011] In step (2) and step (4), the epitaxial growth solution contains a zinc source, a cerium source, hexamethylenetetramine and an epitaxial growth regulator; and the temperature of the hydrothermal reaction is 95-100°C.
[0012] As a preferred embodiment, in step (1), the carbon-based material is selected from at least one of carbon fiber cloth, carbon paper, carbon cloth, carbon felt and mesh glassy carbon;
[0013] In the technical solution of the present invention, in step (1), the preparation of the zinc oxide seed layer comprises the following steps: soaking the carbon-based material in a zinc oxide seed layer precursor solution, volatilizing the solvent and forming a zinc oxide seed layer on the carbon-based material by annealing;
[0014] The zinc oxide seed layer precursor solution is an ethanol solution of zinc acetate; the zinc acetate concentration in the ethanol solution of zinc acetate is 0.005-0.025 mol / L; the soaking time is ≥24h; the volatile solvent is dried at 60-80°C for 10-12h; the annealing temperature is 350-400°C; the annealing time is 20-30min; the heating rate in the annealing is 3-5°C / min;
[0015] In some specific embodiments, the preparation of the zinc oxide seed layer also includes pretreatment of the carbon-based material; the pretreatment includes washing and drying; wherein the washing solvents include acetone, water, and anhydrous ethanol in sequence; and the drying is drying at 60-80° C. for 10-12 hours.
[0016] As a preferred embodiment, in step (2), the epitaxial growth regulator is polyethyleneimine;
[0017] And / or, the zinc source is a soluble zinc salt and / or zinc chloride; the soluble zinc salt is, for example, zinc nitrate, zinc nitrate hexahydrate;
[0018] And / or, the cerium source is a soluble cerium salt and / or cerium chloride; the soluble cerium salt is, for example, cerium nitrate, cerium nitrate hexahydrate;
[0019] Preferably, the molar ratio of the zinc source to hexamethylenetetramine is 2:1 to 1.5;
[0020] Preferably, the molar ratio of zinc in the zinc source to cerium in the cerium source is 90 to 95:5;
[0021] Preferably, the mass ratio of the epitaxial growth regulator to hexamethylenetetramine is 1-1.5:0.14;
[0022] As a preferred embodiment, in step (2), the hydrothermal reaction time is 10 to 12 hours;
[0023] Preferably, the step (2) further comprises post-treatment of drying and annealing; the drying is preferably carried out at 60°C to 80°C for 10 to 12 hours; the annealing is preferably carried out at 350 to 400°C for 20 to 30 minutes; the heating rate of the annealing is preferably 3 to 5°C / min. In the technical solution of the present invention, the Zn(OH)2 generated in the hydrothermal reaction can be completely converted into ZnO by annealing;
[0024] Preferably, in step (2), the carbon-based material is vertically immersed in an epitaxial growth solution to perform a hydrothermal reaction; in the technical solution of the present invention, vertical immersion can make the seeds evenly planted on the carbon cloth.
[0025] As a preferred embodiment, in step (3), the zinc oxide seed layer precursor solution is an ethanol solution of zinc acetate; the zinc acetate concentration in the ethanol solution of zinc acetate is 0.005 to 0.025 mol / L; the immersion time is ≥ 24 h;
[0026] Preferably, in step (3), the immersion further includes volatilizing the solvent and annealing treatment;
[0027] Preferably, in step (3), the volatile solvent is dried at 60-80°C for 10-12h; the temperature of the annealing treatment is 350-400°C; the time of the annealing treatment is 20-30min; and the heating rate in the annealing treatment is 3-5°C / min.
[0028] As a preferred embodiment, in step (4), the epitaxial growth regulator is polyethyleneimine;
[0029] And / or, the zinc source is a soluble zinc salt and / or zinc chloride; the soluble zinc salt is, for example, zinc nitrate, zinc nitrate hexahydrate;
[0030] And / or, the cerium source is preferably a soluble cerium salt and / or cerium chloride; the soluble cerium salt is, for example, cerium nitrate, cerium nitrate hexahydrate;
[0031] Preferably, the molar ratio of the zinc source to hexamethylenetetramine is preferably 2:1 to 1.5;
[0032] Preferably, the molar ratio of zinc in the zinc source to cerium in the cerium source is 90 to 95:5;
[0033] Preferably, the mass ratio of the epitaxial growth regulator to hexamethylenetetramine is 1-1.5:0.14.
[0034] As a preferred embodiment, in step (4), the hydrothermal reaction time is 10 to 12 hours;
[0035] Preferably, the step (4) further comprises post-treatments of drying and annealing; the drying is preferably carried out at 60°C to 80°C for 10 to 12 hours; the annealing is preferably carried out at 350 to 400°C for 20 to 30 minutes; and the heating rate of the annealing is preferably 3 to 5°C / min.
[0036] In the technical scheme of the present invention, the cerium-doped zinc oxide generated by the one-step hydrothermal reaction of step (1) and step (2) is a rod-shaped structure, which is relatively coarse and sparse, and the crystal form is incomplete; and in this process, the diameter of the cerium-doped rod-shaped zinc oxide is related to the time of the hydrothermal reaction and the amount of the epitaxial growth regulator, which is specifically manifested as follows: the diameter of the cerium-doped rod-shaped zinc oxide will increase with the increase of the hydrothermal reaction time, or the diameter of the cerium-doped rod-shaped zinc oxide will first decrease and then increase with the increase of the amount of polyethyleneimine. After the secondary hydrothermal treatment of step (3) and step (4), a thin and long cerium-doped zinc oxide nanoarray can be obtained.
[0037] In another aspect, the present invention provides a cerium-doped zinc oxide nanoarray carbon-based composite material obtained by the above preparation method.
[0038] In another aspect, the present invention provides a use of the cerium-doped zinc oxide nanoarray carbon-based composite material in preparing a lithium-ion battery;
[0039] Preferably, the invention is used in preparing a negative electrode of a lithium ion battery.
[0040] Compared with the prior art, the present invention has the following advantages:
[0041] The present invention grows a regularly arranged zinc oxide nanoarray on a carbon-based material by pre-seeding and hydrothermal method, improves the performance of the material by introducing Ce, and obtains a cerium-doped zinc oxide nanoarray carbon-based composite material by carbon coating reduction. The nanomaterial provided by the present invention can increase the active sites and cycle life of lithium, thereby having good rate performance and cycle life.
[0042] The present invention uses a carbon-based material as a substrate, which can provide support for the cerium-doped zinc oxide nanoarray. Since zinc oxide is often damaged or detached due to stress and dendrite growth in the lithiation reaction, the electrode material is irreversibly damaged, resulting in a decrease in the capacity of the electrode material. By rationally regulating the microscopic morphology and structure of zinc oxide, zinc oxide electrode materials in different dimensions such as nanoparticles, nanowires / nanorods, nanosheets, and nanospheres are prepared, which can effectively increase their specific surface area and alleviate problems such as volume expansion. On the other hand, by compounding with carbon materials, metal elements or metal oxide materials, combined with the catalytic synergistic effect of the composite elements, the cycle stability and rate performance of the electrode material can be significantly improved. The present invention prepares a carbon-based composite material with a regularly arranged zinc oxide nanoarray, and its unique structure has a high specific surface area, which provides more active sites for subsequent reactions to improve the electrochemical performance of the electrode material.
[0043] The present invention prepares a one-dimensional cerium-doped zinc oxide nanoarray with controllable morphology by regulating the reaction conditions in the preparation method, such as the temperature and time of the hydrothermal reaction, and the amount of the reaction raw materials. The present invention further finds that the morphology of the cerium-doped zinc oxide nanoarray affects the electrochemical properties of the electrode, such as cycle life and rate performance. The cerium-doped zinc oxide nanoarray carbon-based composite material prepared by the present invention not only makes up for the disadvantage of poor conductivity of zinc oxide itself, but also retains its own advantages such as high capacity.
[0044] The preparation method of the present invention has readily available raw materials, low cost, simple preparation technology, easy-to-control process, and high feasibility and commercial transformation potential. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 This is a SEM image of the cerium-doped zinc oxide nanoarray carbon-based composite material prepared in Example 1 of the present invention.
[0046] Figure 2 This is a cyclic stability curve of the cerium-doped zinc oxide nanoarray carbon-based composite material prepared in Example 1 of the present invention.
[0047] Figure 3 This is a rate performance diagram of the cerium-doped zinc oxide nanoarray carbon-based composite material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0048] The following embodiments are only some embodiments of the present invention, rather than all embodiments. Therefore, the detailed description in the embodiments of the present invention provided below is not intended to limit the scope of the present invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making creative work belong to the protection scope of the present invention.
[0049] In the present invention, unless otherwise specified, all equipment and raw materials can be purchased from the market or are commonly used in the industry. The methods in the following embodiments are all conventional methods in the art unless otherwise specified.
[0050] In the following examples, the M of polyethyleneimine is W is 10000.
[0051] Example 1
[0052] This embodiment provides a cerium-doped zinc oxide nanoarray carbon-based composite material, and the preparation process is as follows:
[0053] (1) Carbon cloth cleaning
[0054] The carbon cloth was cut into a size of 2 cm × 4 cm, and washed in acetone, water, and anhydrous ethanol for 15 min in sequence. After washing, it was dried in a forced air drying oven at 60 °C for 12 h.
[0055] (2) Carbon cloth seed crystal
[0056] The carbon cloth was soaked in 0.005 mol / L zinc acetate ethanol solution for 24 hours; then placed in a vacuum drying oven and dried at 60°C for 12 hours; the carbon cloth was spread on a clean porcelain boat, placed in a tube furnace, and heated to 350°C at 5°C / min for annealing for 30 minutes;
[0057] (3) Preparation of cerium-doped zinc oxide nanorods
[0058] In a 50mL beaker, 0.565g zinc nitrate hexahydrate and 0.14g hexamethylenetetramine were mixed, and then 0.0434g cerium nitrate hexahydrate and 0.1g polyethyleneimine were added. Then 40mL deionized water was added, and ultrasonic dissolution and stirring were performed for 30min. The dissolved solution was placed in a reactor, and the carbon cloth was placed vertically in the reactor for hydrothermal reaction at a temperature of 95°C. The reaction was kept warm for 10h and then cooled naturally.
[0059] The cooled carbon cloth was washed with water and anhydrous ethanol for 3-4 times respectively, and then placed in a vacuum drying oven and dried at 60°C for 12 hours; the carbon cloth was spread on a clean porcelain boat, placed in a tube furnace, and heated to 350°C at 5°C / min and annealed for 30 minutes to obtain a carbon cloth with Ce-doped zinc oxide nanorods grown thereon;
[0060] (4) Preparation of cerium-doped zinc oxide nanoarray composites
[0061] The carbon cloth obtained in step (3) is subjected to the operation in step (2) to obtain a secondary seeded carbon cloth; and the operation in step (3) is then repeated to obtain a cerium-doped zinc oxide nanoarray carbon-based composite material after secondary hydrothermal treatment and annealing.
[0062] This embodiment also prepares a zinc oxide (ZnO) material without cerium doping. The preparation process is the same as that of the cerium-doped zinc oxide nanoarray composite material, except that the cerium nitrate hexahydrate in step (3) and step (4) is omitted.
[0063] The SEM images of the cerium-doped zinc oxide nanoarray carbon-based composite material and the zinc oxide (ZnO) material prepared in this embodiment are shown in FIG. Figure 1 ,in, Figure 1 a is the ZnO material at low rate; Figure 1 b is the ZnO material at high rate; Figure 1 c is a cerium-doped zinc oxide nanoarray carbon-based composite material at low magnification; Figure 1 d is a cerium-doped zinc oxide nanoarray carbon-based composite material at a high magnification. It can be seen from the figure that after doping with Ce, the nanorods change from a hexagonal shape to a needle-like tip, and the diameter of the nanorods becomes smaller.
[0064] Electrochemical performance test
[0065] The composite material is cut into a circular electrode sheet using a sheet cutting machine, placed in a vacuum drying oven at 80° C. for 10 h, and then used as a positive electrode of the battery. The electrode sheet is weighed and set aside;
[0066] Assemble the button CR2032 type button battery in the following order: negative electrode shell, lithium sheet, diaphragm, electrolyte, electrode sheet, gasket and shrapnel. A single-layer microporous polyethylene membrane was selected as the diaphragm, the metal lithium sheet was used as the counter electrode, the electrolyte was a 1 mol / L LiPF6 solution, and the solvent was a mixed solvent of ethylene carbonate (EC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) in a volume ratio of 1:1:1. The assembly process was carried out in a glove box filled with high-purity argon (99.999%) (water value and oxygen value were both less than 0.1×10 -6 ) is carried out in
[0067] This experiment uses the Land-2001B model of the blue electric tester to test the rate performance and cycle stability of the above-mentioned battery. The current density set for the rate performance test is 0.1A / g, 0.2A / g, 0.5A / g, 1A / g, 2A / g, 4A / g, and 5A / g, and runs 5 cycles at these current densities respectively; the current density set for the long cycle performance test is 1A / g, and the test voltage range is 0.01~3V. The test results are shown in Figure 2 , 3 :from Figure 2It can be seen that the coulombic efficiency of the first cycle is 83.23%; the discharge capacity at a current density of 0.1A / g is 1919.2mAh / g, and after 100 cycles at a current density of 1A / g, the discharge capacity remains at 1648.7mAh / g, and the cycle retention rate is stable at 92%. Figure 3 In the experiment, the current density was 0.1A / g, 0.2A / g, 0.5A / g, 1A / g, 2A / g, 4A / g and 5A / g respectively. When it returned to 0.1A / g, the specific capacity of the nanoarray was basically restored to 1919.2mAh / g, reflecting its good reversibility.
[0068] Example 2
[0069] This embodiment provides a cerium-doped zinc oxide nanoarray carbon-based composite material, and the preparation process is as follows:
[0070] (1) Carbon cloth cleaning
[0071] The carbon cloth was cut into a size of 2 cm × 4 cm, and washed in acetone, water, and anhydrous ethanol for 15 min in sequence. After washing, it was dried in a forced air drying oven at 60 °C for 12 h.
[0072] (2) Carbon cloth seed crystal
[0073] The carbon cloth was soaked in 0.005 mol / L zinc acetate ethanol solution for 24 hours; then placed in a vacuum drying oven and dried at 70°C for 12 hours; the carbon cloth was spread on a clean porcelain boat, placed in a tube furnace, and heated to 400°C at 5°C / min for annealing for 30 minutes;
[0074] (3) Preparation of cerium-doped zinc oxide nanorods
[0075] In a 50mL beaker, 0.565g zinc nitrate hexahydrate and 0.14g hexamethylenetetramine were mixed, and then 0.0434g cerium nitrate hexahydrate and 0.1g polyethyleneimine were added, and 40mL deionized water was added, and ultrasonic dissolution and stirring were performed for 30min; the dissolved solution was placed in a reactor, and the carbon cloth was placed vertically in the reactor for hydrothermal reaction at a temperature of 100°C; the reaction was kept warm for 10h and then cooled naturally;
[0076] The cooled carbon cloth was washed with water and anhydrous ethanol for 3-4 times respectively, and then placed in a vacuum drying oven and dried at 70°C for 12 hours; the carbon cloth was spread on a clean porcelain boat, placed in a tube furnace, and heated to 400°C at 5°C / min and annealed for 30 minutes to obtain a carbon cloth with Ce-doped zinc oxide nanorods grown thereon;
[0077] (4) Preparation of cerium-doped zinc oxide nanoarray composites
[0078] The carbon cloth obtained in step (3) is subjected to the operation in step (2) to obtain a secondary seeded carbon cloth; and the operation in step (3) is then repeated to obtain a cerium-doped zinc oxide nanoarray carbon-based composite material after secondary hydrothermal treatment and annealing.
[0079] Example 3
[0080] (1) Carbon cloth cleaning
[0081] The carbon cloth was cut into a size of 2 cm × 4 cm, and washed in acetone, water, and anhydrous ethanol for 15 min in sequence. After washing, it was dried in a forced air drying oven at 60 °C for 12 h.
[0082] (2) Carbon cloth seed crystal
[0083] The carbon cloth was soaked in 0.005 mol / L zinc acetate ethanol solution for 24 hours; then placed in a vacuum drying oven and dried at 80°C for 12 hours; the carbon cloth was spread on a clean porcelain boat, placed in a tube furnace, and heated to 350°C at 5°C / min for annealing for 30 minutes;
[0084] (3) Preparation of cerium-doped zinc oxide nanorods
[0085] In a 50mL beaker, 0.565g zinc nitrate hexahydrate and 0.14g hexamethylenetetramine were mixed, 0.0434g cerium nitrate hexahydrate and 0.1g polyethyleneimine were added, and 40mL deionized water was added. The mixture was ultrasonically dissolved and stirred for 30min. The dissolved solution was placed in a reactor, and the carbon cloth was placed vertically in the reactor for hydrothermal reaction at a temperature of 95°C. The reaction was kept warm for 12h and then cooled naturally.
[0086] The cooled carbon cloth was washed with water and anhydrous ethanol for 3-4 times respectively, and then placed in a vacuum drying oven and dried at 80°C for 12 hours; the carbon cloth was spread on a clean porcelain boat, placed in a tube furnace, and heated to 400°C at 5°C / min and annealed for 30 minutes to obtain a carbon cloth with Ce-doped zinc oxide nanorods grown thereon;
[0087] (4) Preparation of cerium-doped zinc oxide nanoarray composites
[0088] The carbon cloth obtained in step (3) is subjected to the operation in step (2) to obtain a secondary seeded carbon cloth; and the operation in step (3) is then repeated to obtain a cerium-doped zinc oxide nanoarray carbon-based composite material after secondary hydrothermal treatment and annealing.
[0089] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a cerium-doped zinc oxide nanoarray carbon-based composite material, characterized in that: The following steps are involved: Step (1): preparing a zinc oxide seed layer on a carbon-based material; Step (2): subjecting the carbon-based material obtained in step (1) to a hydrothermal reaction in an epitaxial growth solution to grow cerium-doped zinc oxide nanorods on the carbon-based material; Step (3): soaking the carbon-based substrate grown with cerium-doped zinc oxide nanorods obtained in step (2) in a zinc oxide seed layer precursor solution to obtain secondary seed crystals; Step (4): subjecting the carbon-based substrate obtained in step (3) to a secondary hydrothermal reaction in an epitaxial growth solution; In step (2) and step (4), the epitaxial growth solution contains a zinc source, a cerium source, hexamethylenetetramine and an epitaxial growth regulator; and the temperature of the hydrothermal reaction is 95-100°C.
2. The preparation method according to claim 1, characterized in that: In step (1), the carbon-based material is selected from at least one of carbon fiber cloth, carbon paper, carbon cloth, carbon felt and mesh glassy carbon.
3. The preparation method according to claim 1, characterized in that: In step (1), the preparation of the zinc oxide seed layer comprises the following steps: soaking the carbon-based material in a zinc oxide seed layer precursor solution, volatilizing the solvent and forming a zinc oxide seed layer on the carbon-based material through annealing; Among them, the zinc oxide seed layer precursor solution is an ethanol solution of zinc acetate; in the ethanol solution of zinc acetate, the concentration of zinc acetate is 0.005-0.025 mol / L; the immersion time is ≥24h; the volatile solvent is dried at 60-80°C for 10-12h; the annealing temperature is 350-400°C; the annealing time is 20-30min; the heating rate in the annealing is 3-5°C / min.
4. The preparation method according to claim 1, characterized in that: In step (2), the epitaxial growth regulator is polyethyleneimine; Preferably, the zinc source is a soluble zinc salt and / or zinc chloride; Preferably, the cerium source is a soluble cerium salt and / or cerium chloride; Preferably, the molar ratio of the zinc source to hexamethylenetetramine is 2:1 to 1.5; Preferably, the molar ratio of zinc in the zinc source to cerium in the cerium source is 90 to 95:5; Preferably, the mass ratio of the epitaxial growth regulator to hexamethylenetetramine is 1-1.5:0.
14.
5. The preparation method according to claim 1, characterized in that: In step (2), the hydrothermal reaction time is 10 to 12 hours; Preferably, the step (2) further comprises post-treatment of drying and annealing; the drying is preferably carried out at 60°C to 80°C for 10 to 12 hours; the annealing is preferably carried out at 350 to 400°C for 20 to 30 minutes; the heating rate of the annealing is preferably 3 to 5°C / min; Preferably, in step (2), the carbon-based material is vertically immersed in an epitaxial growth solution to perform a hydrothermal reaction.
6. The preparation method according to claim 1, characterized in that: In step (3), the zinc oxide seed layer precursor solution is an ethanol solution of zinc acetate; the zinc acetate concentration in the ethanol solution of zinc acetate is 0.005-0.025 mol / L; the immersion time is ≥24h; Preferably, in step (3), the immersion further includes volatilizing the solvent and annealing treatment; Preferably, in step (3), the volatile solvent is dried at 60-80°C for 10-12h; the temperature of the annealing treatment is 350-400°C; the time of the annealing treatment is 20-30min; and the heating rate in the annealing treatment is 3-5°C / min.
7. The preparation method according to claim 1, characterized in that: In step (4), the epitaxial growth regulator is polyethyleneimine; Preferably, the zinc source is a soluble zinc salt and / or zinc chloride; Preferably, the cerium source is preferably a soluble cerium salt and / or cerium chloride; Preferably, the molar ratio of the zinc source to hexamethylenetetramine is preferably 2:1 to 1.5; Preferably, the molar ratio of zinc in the zinc source to cerium in the cerium source is 90 to 95:5; Preferably, the mass ratio of the epitaxial growth regulator to hexamethylenetetramine is 1-1.5:0.
14.
8. The preparation method according to claim 1, characterized in that: In step (4), the hydrothermal reaction time is 10 to 12 hours; Preferably, the step (4) further comprises post-treatment of drying and annealing; the drying is preferably carried out at 60°C to 80°C for 10 to 12 hours; the annealing is preferably carried out at 350 to 400°C for 20 to 30 minutes; the heating rate of the annealing is preferably 3 to 5°C / min; Preferably, in step (4), the carbon-based material is vertically immersed in an epitaxial growth solution to perform a secondary hydrothermal reaction.
9. The cerium-doped zinc oxide nanoarray carbon-based composite material obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the cerium-doped zinc oxide nanoarray carbon-based composite material according to claim 9 in the preparation of lithium-ion batteries; Preferably, the invention is used in preparing a negative electrode of a lithium ion battery.
Citation Information
Cited By
Method for growing zinc oxide on surface of conductive carbon cloth and photocatalytic application thereof
CN120592032A