Sodium-ion battery layered oxide positive electrode material precursor as well as preparation method and application of double complexing agents of sodium-ion battery layered oxide positive electrode material precursor
By using a dual complexing agent preparation method in sodium ion batteries, the physical and chemical parameters of sodium electrostatic precursors are coordinated by using ammonia water and oxalic acid solution to jointly optimize the physical and chemical parameters of the sodium electrostatic precursor, the precipitation and dissolution problems caused by a single complexing agent are solved, and better physical and chemical performance and application are achieved. Scope, suitable for industrial production.
Patent Information
- Application Number
- CN202411130938.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
During the liquid phase co-precipitation process, the existing sodium ion battery layered oxide positive electrode material precipitation has dissolution due to the defect of a single complexing agent, which affects the physical and chemical properties of the product and industrial production.
The preparation method of double complexing agent is adopted. By simultaneously using ammonia water and oxalic acid solution as complexing agent, and the relative concentration and pH value are adjusted, the physical and chemical parameters of the precursor are optimized and the reaction conditions are controlled to achieve better particle size and spherical degree. and tap density.
The physical and chemical properties of sodium-electric precursors are significantly optimized, the particle size, spherical shape and tap density are improved, and they are suitable for different series of sodium-electric layered oxide positive electrode materials, suitable for industrial production, and reduce production costs.
Smart Images

Figure CN119018937A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a sodium ion battery layered oxide positive electrode material precursor and a preparation method and application of a dual complexing agent thereof. Background Art
[0002] In recent years, sodium-ion batteries have attracted more and more attention due to their advantages of low cost and high safety. The key material of sodium-ion batteries is the cathode material, and its cost is one of the main factors determining the cost of sodium-ion batteries. The development of advanced cathode materials with large-scale production capacity is the key to realizing the commercial application of sodium-ion batteries.
[0003] Layered transition metal oxide cathode materials for sodium ion batteries (Na x TMO2 (TM = Fe, Mn, Ni, Cu, Zn, etc.) not only has low cost and a wide range of raw materials, but also has a simple synthesis process, which is convenient for large-scale industrial production. It also has the advantages of high energy density, high voltage platform, excellent comprehensive performance and flexible chemical composition design. It is currently the mainstream research direction of positive electrode materials for sodium ion batteries. Among them, Fe, Mn, Ni, Cu, Zn, etc. are the best elements for building low-cost commercial layered oxide positive electrode materials.
[0004] Since the cathode material plays a decisive role in the performance of the battery, and the precursor directly determines the core electrochemical properties of the cathode material, the precursor of the layered oxide cathode material (Fe x TM 1-x The research on (OH)2)(0<x<1, TM=Ni, Mn, Cu, Zn, etc.) is crucial to the development of sodium ion batteries. At present, the precursors of layered oxide cathode materials for sodium ion batteries are mainly produced in large quantities by liquid phase coprecipitation. The liquid phase coprecipitation method generally uses a mixed metal salt solution, a precipitant and a complexing agent, among which the complexing agent is crucial to the coprecipitation process. + ) cannot complex Fe 2+ Cu 2+ The hydroxide precipitate will dissolve under the condition of excess ammonia, which will eventually affect the growth of the product. If two complexing agents are used in the coprecipitation process, the defects of a single complexing agent can be effectively compensated, and the physicochemical parameters of the precursor can be synergistically optimized, so that the obtained sodium battery precursor has relatively better physicochemical properties. Therefore, the development of a dual complexing agent preparation method for sodium battery precursors is of great significance for the research of sodium ion batteries.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] One of the purposes of the present invention is to provide a method for preparing a double complexing agent precursor of a layered oxide positive electrode material for a sodium ion battery. During the coprecipitation process, by simultaneously using two complexing agents and regulating process parameters such as the relative concentration of the double complexing agents, the physicochemical parameters of the precursor can be synergistically optimized, and the obtained sodium battery precursor has relatively better physicochemical properties and a wide range of applications.
[0007] The second object of the present invention is to provide a sodium ion battery layered oxide positive electrode material precursor having relatively better physical and chemical properties, such as larger particle size, better sphericity and higher tap density.
[0008] The third object of the present invention is to provide a positive electrode material for a sodium ion battery, which is beneficial to improving the working performance of the battery.
[0009] A fourth object of the present invention is to provide a sodium ion battery with excellent electrochemical performance.
[0010] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0011] In a first aspect, a method for preparing a sodium ion battery layered oxide positive electrode material precursor using a dual complexing agent comprises the following steps:
[0012] The mixed metal salt solution, the precipitant and the double complexing agent are introduced into a reaction kettle in which the base liquid has been adjusted to carry out a co-precipitation reaction, the concentration of the mixed metal salt solution is controlled to be ≤2.0 mol / L, the concentration of the precipitant is ≤11.0 mol / L, the concentration of the complexing agent is ≤10.0 mol / L, and the process parameters such as the relative concentration of the double complexing agent are regulated, an inert gas is continuously introduced during the reaction, and the reaction is continued until the particle size of the product reaches the target particle size, thereby obtaining a sodium positive electrode material precursor;
[0013] In the granulation stage, the pH value in the reaction kettle is controlled to be a first pH value, and the values of the complexing agent A and the complexing agent B are a first complexing agent concentration value; in the growth stage, the pH in the reaction kettle is controlled to be a second pH value, and the values of the complexing agent A and the complexing agent B are a second complexing agent concentration value;
[0014] Among them, 12.50>first pH value>second pH value>9.50, 0.01mol / L≤first complexing agent concentration value<second complexing agent concentration value≤1.0mol / L, and the relative size of the concentration values of complexing agent A and complexing agent B is adjusted according to different systems;
[0015] Wherein, the dual complexing agents are ammonia water and oxalic acid solution respectively;
[0016] During the coprecipitation process, the ammonium concentration is 0.10 mol / L-0.50 mol / L, and the oxalate concentration is 0.01 mol / L-1.0 mol / L.
[0017] Furthermore, the chemical composition of the positive electrode material precursor is as follows:
[0018] Fe x TM 1-x (OH)2(0<x<1, TM is a metal ion); wherein TM is selected from one or more of Ni, Mn, Cu and Zn.
[0019] Furthermore, the preparation method comprises the following steps:
[0020] (a) mixing metal salts according to the chemical composition of the cathode material precursor to obtain a mixed metal salt solution;
[0021] (b) The mixed metal salt solution of step (a) is first subjected to a nucleation reaction in the presence of a dual complexing agent and a precipitant, and then subjected to a growth reaction until the product D50 particle size reaches a target particle size, and then subjected to aging, centrifugation, drying, screening, demagnetization and packaging operations in sequence to obtain a sodium positive electrode material precursor.
[0022] Furthermore, the D50 particle size of the precursor is 3.0 μm-15.0 μm.
[0023] Furthermore, the precipitant is sodium hydroxide or potassium hydroxide solution, and the inert gas is nitrogen or argon.
[0024] Furthermore, the precipitant is sodium hydroxide solution, and the inert gas is nitrogen.
[0025] Furthermore, the reaction temperature is 30°C-70°C.
[0026] In a second aspect, a sodium ion battery layered oxide positive electrode material precursor is prepared by any of the preparation methods described above.
[0027] In a third aspect, a sodium ion battery positive electrode material is prepared using the above-mentioned sodium ion battery layered oxide positive electrode material precursor, and the preparation method thereof comprises the following steps:
[0028] The sodium ion battery layered oxide positive electrode material precursor is uniformly mixed with a sodium source (NaOH, Na2CO3, etc.) and then calcined at a high temperature to obtain the sodium ion battery positive electrode material.
[0029] In a fourth aspect, a sodium ion battery is provided, wherein the positive electrode of the sodium ion battery comprises the positive electrode material described above.
[0030] Compared with the prior art, the present invention has at least the following beneficial effects:
[0031] The dual complexing agent preparation method of the sodium ion battery layered oxide positive electrode material precursor (sodium electric precursor) provided by the present invention uses two complexing agents simultaneously in the liquid phase coprecipitation process, which can effectively make up for the defects of a single complexing agent, such as ammonium (NH4 + ) cannot complex Fe 2+ Cu 2+ The hydroxide precipitate dissolves under excess ammonia water, and at a specific concentration, the dual complexing agent can cooperate more effectively, thereby significantly optimizing the physicochemical parameters of the precursor, so that the prepared sodium electric precursor has relatively better physicochemical properties, such as larger particle size, better sphericity and higher tap density, and is suitable for different series of sodium electric layered oxide positive electrode material precursors, such as iron manganese (FeMn), copper iron manganese (CuFeMn), nickel iron manganese (NiFeMn), nickel iron manganese copper (NiFeMnCu) and copper iron manganese zinc (CuFeMnZn) series. At the same time, the preparation method of the present invention is easy to operate and control, and is suitable for industrial production.
[0032] Fe 2+ Problems in ammonia: Fe 2+ Does not complex with ammonia (oxalate (C2O4 2- Yes, because Fe 2+ With OH - The bond is stronger with Ni 2+ and Co 2+ Different, Fe 2+ When reacted with excess ammonia water, a hydroxide precipitate will be directly generated and will not dissolve, rather than first generating an iron-ammine complex and then a precipitate.
[0033] Cu 2+ Problems in ammonia: Cu 2+ The hydroxide precipitate will dissolve in ammonia water because Cu 2+ Although hydroxide precipitates will form in the presence of a small amount of ammonia, excess ammonia will cause the precipitate to gradually dissolve and eventually form copper-ammonia complex ions (Cu(NH3)4 2+ ) is dispersed in water, so ammonia can only play an auxiliary role in trace amounts, and excessive amounts are not acceptable, so as not to affect product growth. Other complexing agents such as oxalic acid or carbonate solution can be used instead.
[0034] Comparison between oxalic acid solution and aqueous ammonia: Oxalic acid has a high unit price and is not easy to recycle. The solution is also prone to crystallization and requires high temperature insulation, which has a relatively higher cost. Ammonia solution has a low cost and is easy to recycle. It does not require insulation, has a relatively lower cost, and is more conducive to industrial production.
[0035] Therefore, the simultaneous use of two chelating agents, ammonia water and oxalic acid solution, can effectively make up for the defects of a single chelating agent, ammonia water or oxalic acid solution, and synergistically optimize the physicochemical parameters of the precursor, so that the obtained sodium battery precursor has relatively better physicochemical properties and is more conducive to industrial production.
[0036] The sodium ion battery layered oxide positive electrode material precursor provided by the present invention has relatively better physical and chemical properties, such as larger particle size, better sphericity and higher tap density.
[0037] The sodium ion battery positive electrode material provided by the present invention is beneficial to improving the working performance of the battery.
[0038] The sodium ion battery provided by the present invention has excellent electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0040] Figure 1 A flow chart for preparing a sodium electrode precursor provided in one embodiment of the present invention;
[0041] Figure 2 This is a SEM image of the sodium electrode precursor provided in Example 1 of the present invention;
[0042] Figure 3 This is a SEM image of the sodium electrode precursor provided in Example 2 of the present invention;
[0043] Figure 4 This is a SEM image of the sodium electrode precursor provided in Example 3 of the present invention;
[0044] Figure 5 This is a SEM image of the sodium electrode precursor provided in Example 4 of the present invention;
[0045] Figure 6 This is a SEM image of the sodium electrode precursor provided in Example 5 of the present invention;
[0046] Figure 7 This is a SEM image of the sodium electrode precursor provided in Comparative Example 1 of the present invention;
[0047] Figure 8 This is a SEM image of the sodium electrode precursor provided in Comparative Example 2 of the present invention;
[0048] Fig. 9 This is a SEM image of the sodium electrode precursor provided in Comparative Example 3 of the present invention. DETAILED DESCRIPTION
[0049] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0050] According to a first aspect of the present invention, there is provided a method for preparing a double complexing agent for a layered oxide positive electrode material precursor for a sodium ion battery, comprising the following steps:
[0051] The mixed metal salt solution, the precipitant and the double complexing agent are introduced into a reaction kettle in which the base liquid has been adjusted to carry out a co-precipitation reaction, the concentration of the mixed metal salt solution is controlled to be ≤2.0 mol / L, the concentration of the precipitant is ≤11.0 mol / L, the concentration of the complexing agent is ≤10.0 mol / L, and the process parameters such as the relative concentration of the double complexing agent are regulated, an inert gas is continuously introduced during the reaction, and the reaction is continued until the particle size of the product reaches the target particle size, thereby obtaining a sodium positive electrode material precursor;
[0052] In the granulation stage, the pH value in the reaction kettle is controlled to be a first pH value, and the values of the complexing agent A and the complexing agent B are a first complexing agent concentration value; in the growth stage, the pH in the reaction kettle is controlled to be a second pH value, and the values of the complexing agent A and the complexing agent B are a second complexing agent concentration value;
[0053] Among them, 12.50>first pH value>second pH value>9.50, 0.01mol / L≤first complexing agent concentration value<second complexing agent concentration value≤1.0mol / L, and the relative size of the concentration values of complexing agent A and complexing agent B is adjusted according to different systems;
[0054] The double complexing agents are ammonia water and oxalic acid solution;
[0055] During the coprecipitation process, the ammonium concentration is 0.10mol / L-0.50mol / L, and the oxalate concentration is 0.01mol / L-1.0mol / L.
[0056] The use of two complexing agents simultaneously in the liquid phase coprecipitation process can effectively make up for the defects of a single complexing agent, such as ammonium ion (NH4 + ) cannot complex Fe 2+ , while oxalate (C2O4 2- Yes, Cu 2+ The hydroxide precipitate will dissolve in excess ammonia water, while oxalic acid will not, thereby synergistically optimizing the physicochemical parameters of the precursor, making the resulting sodium electrode precursor have relatively better physicochemical properties and more conducive to industrial production.
[0057] During the liquid phase co-precipitation process, the ammonium concentration is 0.10 mol / L-0.50 mol / L, and the typical but non-limiting concentration of ammonium is 0.10, 0.15, 0.20, 0.25, 0.30, 0.35, 0.40 mol / L; the oxalate concentration is 0.01 mol / L-1.0 mol / L, and the typical but non-limiting concentration of oxalate is 0.05, 0.10, 0.20, 0.30, 0.40, 0.50, 0.60, 0.70 mol / L.
[0058] In the present invention, the dual complexing agents (ammonia water and oxalic acid) can be effectively combined at appropriate concentrations to synergistically optimize the physicochemical parameters of the precursor, so that the prepared sodium electric precursor has better physicochemical properties (larger particle size, better sphericity and higher tap density, etc.); for Cu-containing precursors, the complexing agent system is mainly oxalic acid and supplemented by ammonia water. If the ammonium concentration is too high, the generated hydroxide precipitation will dissolve, the particles will be pulverized, and the product will not be able to grow further. If the ammonium concentration is too low, it will lead to the inability to effectively synergistically optimize the physicochemical parameters of the precursor, such as further improving the tap density, etc.; and for Cu-free precursors, the complexing agent system is mainly ammonia water and supplemented by oxalic acid. If the oxalate concentration is too high, the primary particles of the product will be excessively coarsened, the particles will agglomerate, the sphericity will deteriorate, and the production cost will increase. If the oxalate concentration is too low, it will lead to the inability to effectively synergistically optimize the physicochemical parameters of the precursor, and small balls will easily appear in the production process, and the product will not be able to grow further.
[0059] In summary, the present invention simultaneously uses ammonia water and oxalic acid as complexing agents in the liquid phase co-precipitation process, which effectively makes up for the defects of a single complexing agent, and at a specific concentration, ammonia water and oxalic acid can cooperate more effectively, thereby significantly optimizing the physicochemical parameters of the precursor, so that the prepared sodium electric precursor has relatively better physicochemical properties, such as larger particle size, better sphericity and higher tap density, etc., and is suitable for different series of sodium electric layered oxide positive electrode material precursors, such as iron manganese (FeMn), copper iron manganese (CuFeMn), nickel iron manganese (NiFeMn), nickel iron manganese copper (NiFeMnCu) and copper iron manganese zinc (CuFeMnZn) series. At the same time, the preparation method of the present invention is easy to operate and control, and is suitable for industrial production.
[0060] In a preferred embodiment, the chemical composition of the cathode material precursor is as follows:
[0061] Fe x TM 1-x (OH)2; wherein TM is selected from one or more of Ni, Mn, Cu and Zn.
[0062] In a preferred embodiment, the preparation method of the present invention comprises the following steps:
[0063] (a) mixing metal salts according to the chemical composition of the cathode material precursor to obtain a mixed metal salt solution;
[0064] (b) The mixed metal salt solution of step (a) is first subjected to a nucleation reaction in the presence of a dual complexing agent and a precipitant, and then subjected to a growth reaction until the product D50 particle size reaches a target particle size, and then subjected to aging, centrifugation, drying, screening, demagnetization and packaging operations in sequence to obtain a sodium positive electrode material precursor.
[0065] In a preferred embodiment, the precipitant includes but is not limited to sodium hydroxide solution.
[0066] In the present invention, since oxalic acid has a certain reducing property, ammonia water and oxalic acid solution are used as complexing agents during liquid phase coprecipitation, and sodium hydroxide solution is used as precipitating agent, which is more conducive to realizing different series of sodium electrode precursors (Fe x TM 1-x (OH)2, TM=Ni, Mn, Cu, Zn, etc.) The smooth growth of secondary particles, especially the smooth growth of large particle precursors.
[0067] In a preferred embodiment, the pH condition of the liquid phase coprecipitation reaction can be 9.50-12.50, and typical but non-limiting pH values are, for example, 10.0, 10.30, 10.60, 10.80, 11.00, 11.30, 11.60, 11.80, 12.10, and 12.30.
[0068] In a preferred embodiment, the temperature of the liquid phase coprecipitation reaction can be 30°C-70°C, and typical but non-limiting temperatures are, for example, 35, 40, 45, 50, 55, 60, 65, 70°C.
[0069] The present invention adopts a method for preparing a sodium positive electrode material precursor using a double complexing agent, and the flow chart is shown in Figure 1 , and at the same time, a mixed metal salt solution, a complexing agent 1 (ammonia solution), a complexing agent 2 (oxalic acid solution) and a precipitant (sodium hydroxide solution) are pumped into a reactor to first perform a nucleation reaction, then a growth reaction, and finally a post-treatment. After the physical and chemical indicators are detected to be qualified, a sodium electric layered precursor is obtained; in the liquid phase co-precipitation process, the present invention can significantly synergistically optimize the physical and chemical parameters of the precursor by simultaneously using two complexing agents and synergistically regulating process parameters such as the relative concentration of the double complexing agents. The obtained sodium electric precursor has relatively better physical and chemical properties (larger particle size, better sphericity and higher tap density, etc.), and has a wide range of applications and is suitable for industrial production.
[0070] According to a second aspect of the present invention, there is provided a sodium ion battery layered oxide positive electrode material precursor, which is prepared by any of the preparation methods described above and has relatively better physical and chemical properties, such as larger particle size, better sphericity and higher tap density.
[0071] According to a third aspect of the present invention, there is provided a layered positive electrode material for a sodium ion battery, which is prepared using the positive electrode material precursor described above and is beneficial to improving the working performance of the battery.
[0072] According to a fourth aspect of the present invention, a sodium ion battery is provided, wherein the positive electrode of the sodium ion battery comprises the positive electrode material described above and has excellent electrochemical performance.
[0073] The present invention is further described below by way of examples. Unless otherwise specified, the materials in the examples are prepared according to existing methods or directly purchased from the market.
[0074] Example 1
[0075] A method for preparing a double complexing agent for a layered oxide positive electrode material precursor for a sodium ion battery comprises the following steps:
[0076] S1: Add pure water to the reactor and heat it to 45°C, and introduce nitrogen at a flow rate of 30L / h, then add ammonia solution to adjust the ammonium concentration of the bottom liquid to 0.20mol / L, add oxalic acid solution to adjust the oxalate concentration of the bottom liquid to 0.03mol / L, and then add sodium hydroxide solution to adjust the pH value of the bottom liquid to 12.30, and stir the bottom liquid at a speed of 500r / min inside the reactor to mix the bottom liquid evenly to obtain the bottom liquid for the coprecipitation reaction;
[0077] S2: 2.0 mol / L iron-manganese mixed salt solution, 11.0 mol / L sodium hydroxide solution, 7.5 mol / L ammonia solution and 1.5 mol / L oxalic acid solution are simultaneously pumped into the above reactor, and the molar ratio of iron to manganese is controlled to be 50:50. The reaction is carried out for 1 hour under the conditions that the pH value in the reactor is maintained at 12.30, the ammonium concentration is maintained at 0.20 mol / L and the oxalate concentration is maintained at 0.03 mol / L, to complete the nucleation task;
[0078] S3: After completing the nucleation task, the process is switched to a growth process, the pH value of the reactor is gradually reduced to 11.30, and the ammonium concentration is increased to 0.35 mol / L and the oxalate concentration is increased to 0.05 mol / L (ammonia water as the main component and oxalic acid as the auxiliary component), the reaction temperature is increased to 50°C, the speed is adjusted to 400 r / min, and the reaction is continued until the D50 particle size of the product reaches 4.0 μm;
[0079] S4: The slurry product is pumped into the aging tank through the discharge port, and then aged, centrifuged, dried, screened, demagnetized and packaged to obtain the sodium ferromanganese binary precursor (Fe 0.50 Mn 0.50 (OH)2), the scanning electron microscope image is as follows Figure 2 As shown, it can be seen that it has better sphericity and a tap density of 1.30g / cm 3 The growth process does not produce small balls and can grow smoothly to the target particle size of 4μm.
[0080] Example 2
[0081] A method for preparing a double complexing agent for a layered oxide positive electrode material precursor for a sodium ion battery comprises the following steps:
[0082] S1: pure water was added to the reactor and heated to 45°C, and nitrogen was introduced at a flow rate of 30 L / h, and then an ammonia solution was added to adjust the ammonium concentration of the bottom liquid to 0.25 mol / L, and an oxalic acid solution was added to adjust the oxalate concentration of the bottom liquid to 0.03 mol / L, and then sodium hydroxide solution was added to adjust the pH value of the bottom liquid to 12.10, and the stirring blade inside the reactor was stirred at a speed of 500 r / min to mix the bottom liquid evenly to obtain the bottom liquid for the coprecipitation reaction;
[0083] S2: Pump 2.0 mol / L nickel-iron-manganese mixed salt solution, 11.0 mol / L sodium hydroxide solution, 7.5 mol / L ammonia solution and 1.5 mol / L oxalic acid solution into the reactor at the same time, control the molar ratio of nickel-iron-manganese to be 33.3:33.3:33.3, and react for 0.5 hour under the conditions of maintaining the pH value at 12.10, the ammonium concentration at 0.25 mol / L and the oxalate concentration at 0.03 mol / L in the reactor to complete the nucleation task;
[0084] S3: After completing the nucleation task, the process is switched to a growth process, the pH value of the reactor is gradually reduced to 10.80, and the ammonium concentration is increased to 0.30 mol / L and the oxalate concentration is increased to 0.05 mol / L (ammonia water as the main component and oxalic acid as the auxiliary component), the reaction temperature is increased to 50°C, the speed is adjusted to 400 r / min, and the reaction is continued until the D50 particle size of the product reaches 10.0 μm;
[0085] S4: The slurry product is pumped into an aging tank through a discharge port, and then aged, centrifuged, dried, screened, demagnetized and packaged to obtain a sodium-electro-nickel-iron-manganese ternary precursor (Ni 0.333 Fe 0.333 Mn 0.333 (OH)2), the scanning electron microscope image is as follows Figure 3 As shown, it can be seen that it has a larger particle size and better sphericity, and the tap density is 1.38g / cm3 The growth process does not produce small balls and can grow smoothly to the target particle size of 10μm.
[0086] Example 3
[0087] A method for preparing a double complexing agent for a layered oxide positive electrode material precursor for a sodium ion battery comprises the following steps:
[0088] S1: pure water is added to the reactor and heated to 40°C, and nitrogen is introduced at a flow rate of 30 L / h, and then oxalic acid solution is added to adjust the oxalate concentration of the bottom liquid to 0.10 mol / L, and ammonia solution is added to adjust the ammonium concentration of the bottom liquid to 0.10 mol / L, and then sodium hydroxide solution is added to adjust the pH value of the bottom liquid to 11.60, and the stirring blade inside the reactor mixes the bottom liquid uniformly at a speed of 500 r / min to obtain the bottom liquid for the coprecipitation reaction;
[0089] S2: 2.0 mol / L copper, iron and manganese mixed salt solution, 11.0 mol / L sodium hydroxide solution, 1.5 mol / L oxalic acid solution and 7.5 mol / L ammonia solution are pumped into the above reactor at the same time, and the molar ratio of copper, iron and manganese is controlled to be 17:33:50. The reaction is carried out for 1 hour under the conditions that the pH value in the reactor is maintained at 11.60, the oxalate concentration is maintained at 0.10 mol / L and the ammonium concentration is maintained at 0.10 mol / L, and the nucleation task is completed;
[0090] S3: After completing the nucleation task, the process is switched to a growth process, the pH value of the reactor is gradually reduced to 11.30, and the oxalate concentration is increased to 0.50 mol / L and the ammonium concentration is increased to 0.15 mol / L (oxalic acid is the main component, ammonia water is the auxiliary component), the reaction temperature is increased to 60°C, the speed is adjusted to 400 r / min, and the reaction is continued until the D50 particle size of the product reaches 4.0 μm;
[0091] S4: The slurry product is pumped into the aging tank through the discharge port, and the sodium electrolytic copper iron manganese ternary precursor (Cu 0.17 Fe 0.33 Mn 0.50 (OH)2), the scanning electron microscope image is as follows Figure 4 As shown in the figure, it can be seen that it has better sphericity and relatively coarsened primary particle morphology, which is more conducive to improving the tap density (1.26g / cm 3 ).
[0092] Example 4
[0093] A method for preparing a double complexing agent for a layered oxide positive electrode material precursor for a sodium ion battery comprises the following steps:
[0094] S1: pure water was added to the reactor and heated to 40°C, and nitrogen was introduced at a flow rate of 30 L / h, and then oxalic acid solution was added to adjust the oxalate concentration of the bottom liquid to 0.10 mol / L, and ammonia solution was added to adjust the ammonium concentration of the bottom liquid to 0.10 mol / L, and then sodium hydroxide solution was added to adjust the pH value of the bottom liquid to 11.80, and the stirring blade inside the reactor was stirred at a speed of 500 r / min to mix the bottom liquid evenly to obtain the bottom liquid for the coprecipitation reaction;
[0095] S2: 2.0 mol / L copper, iron, manganese and zinc mixed salt solution, 11.0 mol / L sodium hydroxide solution, 1.5 mol / L oxalic acid solution and 7.5 mol / L ammonia solution are pumped into the above reactor at the same time, and the molar ratio of copper, iron, manganese and zinc is controlled to be 12:33:50:5. The reaction is carried out for 0.5 hour under the conditions that the pH value in the reactor is maintained at 11.80, the oxalate concentration is maintained at 0.10 mol / L and the ammonium concentration is maintained at 0.10 mol / L, and the nucleation task is completed;
[0096] S3: After completing the nucleation task, the process is switched to a growth process, the pH value of the reactor is gradually reduced to 11.30, and the oxalate concentration is increased to 0.60 mol / L and the ammonium concentration is increased to 0.20 mol / L (oxalic acid is the main component, ammonia water is the auxiliary component), the reaction temperature is increased to 60°C, the speed is adjusted to 400 r / min, and the reaction is continued until the D50 particle size of the product reaches 10.0 μm;
[0097] S4: The slurry product is pumped into the aging tank through the discharge port, and the sodium electrolytic copper iron manganese zinc quaternary precursor (Cu 0.12 Fe 0.33 Mn 0.50 Zn 0.05 (OH)2), the scanning electron microscope image is as follows Figure 5 As shown in the figure, it can be seen that it has better sphericity and relatively coarsened primary particle morphology, which is more conducive to improving the tap density (1.56g / cm 3 ).
[0098] Example 5
[0099] A method for preparing a double complexing agent for a layered oxide positive electrode material precursor for a sodium ion battery comprises the following steps:
[0100] S1: pure water is added to the reactor and heated to 40°C, and nitrogen is introduced at a flow rate of 30 L / h, and then oxalic acid solution is added to adjust the oxalate concentration of the bottom liquid to 0.10 mol / L, and ammonia solution is added to adjust the ammonium concentration of the bottom liquid to 0.10 mol / L, and then sodium hydroxide solution is added to adjust the pH value of the bottom liquid to 11.60, and the stirring blade inside the reactor mixes the bottom liquid uniformly at a speed of 500 r / min to obtain the bottom liquid for the coprecipitation reaction;
[0101] S2: 2.0 mol / L nickel-iron-manganese-copper mixed salt solution, 11.0 mol / L sodium hydroxide solution, 1.5 mol / L oxalic acid solution and 7.5 mol / L ammonia solution are simultaneously pumped into the above reactor, and the molar ratio of nickel-iron-manganese-copper is controlled to be 22:22:44:12. The reaction is carried out for 1 hour under the conditions that the pH value in the reactor is maintained at 11.60, the oxalate concentration is maintained at 0.10 mol / L, and the ammonium concentration is maintained at 0.10 mol / L, to complete the nucleation task;
[0102] S3: After completing the nucleation task, the process was switched to a growth process, the pH value of the reactor was gradually reduced to 11.30, and the oxalate concentration was increased to 0.40 mol / L and the ammonium concentration was maintained at 0.10 mol / L (oxalic acid was the main component, and ammonia water was the auxiliary component). The reaction temperature was increased to 60°C, the speed was adjusted to 400 r / min, and the reaction was continued until the D50 particle size of the product reached 4.0 μm;
[0103] S4: The slurry product is pumped into an aging tank through a discharge port, and then aged, centrifuged, dried, screened, iron removed and packaged to obtain a sodium-electro-nickel-iron-manganese-copper quaternary precursor (Ni 0.22 Fe 0.22 Mn 0.44 Cu 0.12 (OH)2), the scanning electron microscope image is as follows Figure 6 As shown in the figure, it can be seen that it has better sphericity and relatively coarsened primary particle morphology, which is more conducive to improving the tap density (1.11g / cm 3 ).
[0104] Comparative Example 1
[0105] The difference between this comparative example and Example 1 is that only oxalic acid solution is used as the complexing agent instead of ammonia water, and the oxalate concentrations in the granulation and growth stages are 0.05 and 0.10 mol / L respectively. The remaining steps and process parameters are the same as those in Example 1 to obtain a sodium electric iron manganese binary precursor (Fe 0.50 Mn 0.50 (OH)2), the scanning electron microscope image is as follows Figure 7 shown.
[0106] Compared with the sodium battery precursor obtained in Example 1, the defects of the sodium battery precursor obtained in this comparative example are that the primary particles of the product are excessively coarsened, the particles are agglomerated, the sphericity is deteriorated, and the tap density is low (1.15 g / cm 3 ), and oxalic acid is not easy to recover, which increases production costs.
[0107] Comparative Example 2
[0108] The difference between this comparative example and Example 3 is that only ammonia water is used as the complexing agent instead of oxalic acid solution, and the ammonium concentrations in the granulation and growth stages are 0.15 and 0.30 mol / L respectively. The remaining steps and process parameters are the same as those in Example 3 to obtain a sodium electrolytic copper iron manganese ternary precursor (Cu 0.17 Fe 0.33 Mn 0.50 (OH)2), the scanning electron microscope image is as follows Figure 8 shown.
[0109] Compared with the sodium electrolyte precursor obtained in Example 3, the defect of the sodium electrolyte precursor obtained in this comparative example is that the hydroxide precipitate generated in the coprecipitation process is dissolved, and the particles of the product are pulverized and cannot continue to grow.
[0110] Comparative Example 3
[0111] The difference between this comparative example and Example 2 is that only ammonia water is used as the complexing agent, and no oxalic acid solution is used. The remaining steps and process parameters are the same as those in Example 2 to obtain a sodium-electro-nickel-iron-manganese ternary precursor (Ni 0.333 Fe 0.333 Mn 0.333 (OH)2), the scanning electron microscope image is as follows Fig. 9 shown.
[0112] Compared with the dual complexing agent preparation method of Example 2, the preparation method of this comparative example produces a large number of small balls in the later stage of the growth process due to the lack of the reducing effect of oxalic acid, and the final D50 particle size is only 7.823 μm, which is less than 10 μm.
[0113] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a double complexing agent for a sodium ion battery layered oxide positive electrode material precursor, characterized in that: The steps include: The mixed metal salt solution, the precipitant and the double complexing agent are introduced into a reaction kettle in which the base liquid has been adjusted to carry out a co-precipitation reaction, the concentration of the mixed metal salt solution is controlled to be ≤2.0 mol / L, the concentration of the precipitant is ≤11.0 mol / L, the concentration of the complexing agent is ≤10.0 mol / L, and the process parameters such as the relative concentration of the double complexing agent are regulated, an inert gas is continuously introduced during the reaction, and the reaction is continued until the product particle size reaches the target particle size, thereby obtaining a sodium positive electrode material precursor; In the granulation stage, the pH value in the reaction kettle is controlled to be a first pH value, and the values of the complexing agent A and the complexing agent B are a first complexing agent concentration value; in the growth stage, the pH in the reaction kettle is controlled to be a second pH value, and the values of the complexing agent A and the complexing agent B are a second complexing agent concentration value; Among them, 12.50>first pH value>second pH value>9.50, 0.01mol / L≤first complexing agent concentration value<second complexing agent concentration value≤1.0mol / L, and the relative size of the concentration values of complexing agent A and complexing agent B is adjusted according to different systems; The dual complexing agents are ammonia water and oxalic acid solution respectively; During the coprecipitation process, the ammonium concentration is 0.10 mol / L-0.50 mol / L, and the oxalate concentration is 0.01 mol / L-1.0 mol / L.
2. The preparation method according to claim 1, characterized in that: The chemical composition of the sodium cathode material precursor is as follows: Fe x TM 1-x (OH)2(0<x<1, TM is a metal ion); wherein TM is selected from one or more of Ni, Mn, Cu and Zn.
3. The preparation method according to claim 2, characterized in that: The preparation method comprises the following steps: (a) mixing metal salts according to the chemical composition of the cathode material precursor to obtain a mixed metal salt solution; (b) The mixed metal salt solution of step (a) is first subjected to a nucleation reaction in the presence of a dual complexing agent and a precipitant, and then subjected to a growth reaction until the product D50 particle size reaches a target particle size, and then subjected to aging, centrifugation, drying, screening, demagnetization and packaging operations in sequence to obtain a sodium positive electrode material precursor.
4. The preparation method according to claim 3, characterized in that: The D50 particle size of the precursor is 3.0 μm-15.0 μm.
5. The preparation method according to claim 3, characterized in that: The precipitant is sodium hydroxide or potassium hydroxide solution, and the inert gas is nitrogen or argon.
6. The preparation method according to claim 5, characterized in that: The precipitant is sodium hydroxide solution, and the inert gas is nitrogen.
7. The preparation method according to claim 3, characterized in that: The reaction temperature is 30°C-70°C.
8. A sodium ion battery layered oxide positive electrode material precursor, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 7.
9. A sodium ion battery positive electrode material, characterized in that: The sodium ion battery layered oxide positive electrode material precursor is prepared by using the sodium ion battery layered oxide positive electrode material precursor according to claim 8, and the preparation method thereof comprises the following steps: The sodium ion battery layered oxide positive electrode material precursor is uniformly mixed with a sodium source, and then calcined at a high temperature to obtain the sodium ion battery positive electrode material.
10. A sodium ion battery, characterized in that: The positive electrode of the sodium ion battery comprises the positive electrode material according to claim 9.
Citation Information
Patent Citations
Nickel-iron-manganese ternary precursor, preparation method and sodium ion battery positive electrode material
CN116239161A
Preparation method of double-complexing-agent NCM622 type precursor multi-kettle series concentration process
CN118255399A
Sodium-ion battery precursor, sodium-ion battery positive electrode material and preparation method of sodium-ion battery positive electrode material
CN118289836A