Method for degrading micro-plastics by using surface hydroxyl modified defective bismuth oxyhalide photocatalytic material
By modifying the defective bismuth oxychloride BiOCl photocatalytic material on the surface hydroxyl group, the problem of low efficiency of existing photocatalytic materials in catalyzing the degradation of microplastics was solved, and G/BOC-15 photocatalyst was prepared to achieve the polystyrene micropolytics micropolytics The efficient degradation of plastics provides an environmentally friendly water treatment method.
Patent Information
- Application Number
- CN202411217879.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-09-02
AI Technical Summary
When existing photocatalytic materials such as bismuth oxychloride (BiOCl) catalyze the degradation of microplastics, there is a problem that photogenerated electron-hole pairs are easily recombined, have low specific surface area and narrow photoresponse range, making it difficult to efficiently degrade microplastics in water.
By modifying the defective bismuth oxychloride BiOCl photocatalytic material on the surface hydroxyl group, G/BOC-15 photocatalyst is prepared by simple hydrothermal synthesis method to regulate the mass ratio of glucose to BiOCl to improve the content of surface hydroxyl functional groups and enhance its catalytic performance. to accelerate the photodegradation of microplastics.
The degradation weight loss rate of polystyrene microplastics reached 38% within 12 hours, significantly improving the degradation performance of the catalyst, providing an efficient and low-cost method to remove microplastics from water and protect the environment.
Smart Images

Figure CN119018975A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of photocatalysis, and particularly relates to a preparation method of a defective bismuth oxyhalide photocatalytic material modified with surface hydroxyl groups and application research on accelerating the photodegradation of microplastics. Background Art
[0002] Microplastics are plastic particles with a particle size of less than 5 mm. Due to their difficult decomposition and easy adsorption of pollutants, they have received widespread attention in recent years. Microplastics mainly come from the production, use and disposal of plastic products. They are widely present in water, soil, air and organisms, causing serious harm to the ecological environment and human health. The hazards of microplastics are mainly reflected in the following aspects:
[0003] 1. Ecological environmental damage: Microplastics are difficult to decompose in nature and accumulate in the ecosystem for a long time, leading to ecological imbalance. 2. Human health threats: Microplastics enter the food chain and endanger human health. Many foods, such as seafood, bottled water, milk, coffee, etc., contain microplastic particles. After these microplastics enter the human body, they may cause diseases in the digestive tract, cardiovascular system, and nervous system. 3. Water resource pollution: Microplastic particles float, deposit, or are ingested by organisms in water bodies, leading to aquatic ecological pollution. This further threatens terrestrial ecology, destroys soil, air, and even affects the earth's life system. 4. Reduction of biodiversity: The accumulation of microplastics in organisms will affect the growth, reproduction, and survival rate of organisms, thereby reducing biodiversity. 5. Environmental risks: Microplastic particles are blown away by the wind, enter the atmosphere, become air dust, and affect air quality. In addition, the use of personal protective equipment such as masks and gloves has exacerbated microplastic pollution. In order to deal with microplastic pollution, the Chinese government and all sectors of society should increase environmental protection publicity, raise public awareness of environmental protection, promote the use of degradable plastics, strengthen the recycling and treatment of waste plastics, reduce the production and use of plastic products, and thus reduce the risk of microplastic pollution. How to degrade microplastics in water efficiently and environmentally friendly remains an urgent problem to be solved. Because microplastics are very stable, traditional water treatment processes cannot effectively remove them. Therefore, there is an urgent need to find efficient and low-cost technologies to eliminate microplastics in aquatic environments.
[0004] In recent years, many studies have shown that photocatalysis is a promising treatment technology that can convert organic pollutants into harmless substances under mild conditions. Many researchers have also tried to develop a variety of efficient photocatalysts to decompose microplastics in water.
[0005] Among the numerous reported photocatalytic materials, bismuth oxychloride (BiOCl) has attracted much attention due to its suitable band gap structure, simple synthesis method, good chemical stability and unique layered structure. However, the catalytic ability of BiOCl is limited by its shortcomings such as easy recombination of photogenerated electron-hole pairs, low specific surface area and narrow photoresponse range. Summary of the invention
[0006] The technical problem solved by the present invention is to provide a method for degrading microplastics using a surface hydroxyl-modified defective bismuth oxychloride BiOCl photocatalytic material, and the application of the BiOCl photocatalyst for degrading microplastics, which is simple to operate and environmentally friendly, to accelerate the photodegradation of microplastics. The present invention is a surface-modified hydroxyl-defective BiOCl photocatalytic material, which focuses on studying the differences in the surface hydroxyl photoenergy group modification amount and catalytic performance of BiOCl photocatalysts prepared by different synthesis processes (the content of reducing α-D-glucose), and proposes a simple and effective method for synthesizing G / BOC-15 photocatalyst, which can effectively degrade typical microplastics polystyrene microplastics (PS-MPs), providing a new method for treating wastewater and protecting the environment. The presence of G / BOC-15 makes the weight loss rate of PS-MPs the highest, and can achieve a degradation weight loss rate of 38% for PS-MPs in 12 hours, and has very good catalytic degradation performance for PS-MPs.
[0007] In order to solve the technical problem of the present invention, the proposed technical solution is: a method for using a surface hydroxyl-modified defective bismuth oxyhalide photocatalytic material to degrade microplastics, the specific steps are:
[0008] (1) Bi(NO3)3·5H2O and potassium chloride in a mass ratio of 1:1 were added to a mixture of ethanol and water;
[0009] (2) dissolving a certain amount of α-D-glucose in a mixture of water and ethanol, wherein the volume ratio of water to ethanol is 1:1;
[0010] (3) then dripping the glucose solution prepared in step (2) into the mixed solution in step (1), and continuing stirring for 60 minutes;
[0011] (4) The final solution was transferred to a polytetrafluoroethylene autoclave, and then heated to 100-150° C. for hydrothermal reaction for 10 h;
[0012] (5) collecting the product obtained in step (4), washing it alternately with deionized water and ethanol, and then drying it in a drying oven at 60° C. overnight, wherein the mass ratio of α-D-glucose to BiOCl is 15%, and the obtained BiOCl product is labeled as G / BOC-15;
[0013] (6) Under the action of a 500W Hg lamp, 0.5g / L of photocatalyst G / BOC-15 was added to the polystyrene microplastics PS-MPs solution, and the photocatalytic degradation of the microplastics PS-MPs was carried out using a photoreaction instrument.
[0014] Preferably, the specific steps are:
[0015] (1) Add 4.8 mmol of Bi(NO3)3·5H2O and 4.8 mmol of potassium chloride to a mixture of 28 mL of ethanol and 12 mL of water;
[0016] (2) dissolving 0.1875 g of α-D-glucose in a mixture of water and ethanol, wherein the volume ratio of water to ethanol is 1:1;
[0017] (3) then dripping the glucose solution prepared in step (2) into the mixed solution in step (1), and continuing stirring for 60 minutes;
[0018] (4) The final solution was transferred to a polytetrafluoroethylene autoclave, and then heated to 100-150° C. for hydrothermal reaction for 10 h;
[0019] (5) collecting the product obtained in step (4), washing it alternately with deionized water and ethanol, and then drying it in a drying oven at 60° C. overnight, wherein the mass ratio of α-D-glucose to BiOCl is 15%, and the obtained BiOCl product is labeled as G / BOC-15;
[0020] (6) Under the action of a 500W Hg lamp, 1 g / L of micron-sized plastic PS-MPs was dispersed in 100 mL of aqueous solution, and then 0.5 g / L of photocatalyst G / BOC-15 was added to the above solution. The photocatalytic degradation of microplastic PS-MPs was carried out using a photoreaction instrument. After 12 hours of reaction, the light source was turned off and the solution was filtered using a water system filter membrane with a pore size of 0.45 μm.
[0021] Preferably, when the mass ratio of α-D-glucose to BiOCl added in step (2) is 15%, the performance of the prepared particle stacked G / BOC-15 material is optimal.
[0022] Preferably, the BiOCl morphology and the content of surface hydroxyl functional groups are regulated by changing the amount of α-D-glucose used in step (2), and the prepared G / BOC-15 photocatalyst has the largest amount of surface hydroxyl modification and the presence of oxygen defects, and has the best photocatalytic degradation performance of polystyrene microplastics.
[0023] Preferably, under direct ultraviolet irradiation, the presence of G / BOC-15 makes the weight loss rate of PS-MPs the highest, and can achieve a degradation weight loss rate of 38% for PS-MPs in 12 hours, and has very good catalytic degradation performance for PS-MPs.
[0024] Beneficial effects:
[0025] (1) During the synthesis process, the mass ratio of α-D-glucose to BiOCl was 7%, 10%, 15%, and 20%, respectively, and the obtained BiOCl products were labeled G / BOC-7, G / BOC-10, G / BOC-15, and G / BOC-20, respectively. As a control experiment, the sample prepared by the same method without adding glucose was labeled as BOC. When the addition amount of α-D-glucose in step (2) was 15%, the obtained particle stacked BiOCl photocatalyst G / BOC-15 had the best performance.
[0026] (2) The present invention adopts a simple and feasible preparation method to prepare a BiOCl photocatalyst that can effectively degrade microplastics. By modifying hydroxyl groups and constructing defects on the surface of the material, it has the characteristics of effectively degrading various microplastics at room temperature; it provides a method for obtaining high-performance photocatalyst materials through a simple and green preparation process. A photocatalytic material that can effectively degrade microplastics and supporting technology provide material and technical support for effectively removing microplastics from wastewater.
[0027] (3) During the photoaging process of microplastics, hydroxyl radicals can trigger the cleavage of polymer carbon chains, which plays a very important role in the aging and degradation of microplastics. Modifying the hydroxyl functional groups on the surface of BiOCl can promote BiOCl to produce more hydroxyl radicals during illumination. The present invention regulates the content of glucose during the synthesis process, that is, regulates the surface hydroxyl content of the catalyst, thereby obtaining the photocatalytic material G / BOC-15 with the best performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 is the XRD pattern of all photocatalysts prepared in Example 1 of the present invention;
[0029] Figure 2 are SEM images of all photocatalysts prepared in Example 1 of the present invention: (a) is BOC, (b) is G / BOC-7, (c) is G / BOC-10, (d) is G / BOC-15 and (e) is G / BOC-20;
[0030] Figure 3 is the infrared spectra of all the photocatalysts prepared in Example 1 of the present invention;
[0031] Figure 4(a) The weight loss rate of all catalysts prepared in Example 1 for degrading microplastics and the catalytic performance of the photocatalysts and (b) the correlation between the weight loss rate and the concentration of surface-modified hydroxyl groups. DETAILED DESCRIPTION
[0032] The above contents of the present invention are further described in detail below through examples, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples, and all technologies implemented based on the above contents of the present invention belong to the scope of the present invention.
[0033] Example 1
[0034] 1) Add 4.8 mmol of Bi(NO3)35H2O and 4.8 mmol of potassium chloride to a mixture of 28 mL of ethanol and 12 mL of water.
[0035] 2) A certain amount of 0.0875 g (7%), 0.125 g (10%), 0.1875 g (15%), and 0.25 g (20%) of α-D-glucose was dissolved in 20 mL of a mixture of water and ethanol (the volume ratio of water to ethanol was 1:1).
[0036] 3) Then, the glucose solution in step (2) was dripped into the mixed solution in step (1), and stirring was continued for 60 minutes.
[0037] 4) The final solution was transferred to a polytetrafluoroethylene autoclave, and then heated to 100-150° C. for hydrothermal reaction for 10 h.
[0038] 5) The product was collected, rinsed alternately with deionized water and ethanol, and then dried in a drying oven at 60° C. overnight.
[0039] During the synthesis process, the mass ratios of α-D-glucose to BiOCl were 7%, 10%, 15% and 20%, respectively, and the obtained BiOCl products were labeled as G / BOC-7, G / BOC-10, G / BOC-15 and G / BOC-20, respectively.
[0040] As a control experiment, a sample prepared in the same manner without adding glucose in step (2) was labeled BOC.
[0041] The heterojunction catalyst prepared in Example 1 was subjected to phase analysis by XRD and morphology characterization by SEM. Figure 1 As shown, the XRD characterization results confirm that the material is BiOCl, the card is No. 04-007-4915, and with the increase of glucose amount, the ratio of the peak intensity of the (102) crystal plane to other characteristic peaks such as the (110) plane gradually increases, which also indicates that the (101) crystal plane is gradually exposed in this process.
[0042] from Figure 2 The SEM characterization results show that the morphology of the synthesized catalyst changes greatly with the increase of glucose content during the synthesis process. Under the action of glucose, the initial BOC sheet structure is self-assembled into a flower-like microsphere structure, and the edge of the sheet structure is gradually granulated. When the glucose content increases to 15% by mass, the overall morphology of G / BOC-15 is a spherical structure formed by the aggregation of nanoparticles with a particle size of 30-50nm. As the glucose content further increases to 20%, the excessively high concentration of glucose can serve as a template to reassemble the small particles into a sheet structure and aggregate into a microsphere structure (G / BOC-20).
[0043] Figure 3 Fourier transform infrared spectrum (FT-IR) spectrum, at 1630cm -1 and 3445cm -1 The absorption peaks at correspond to the stretching vibration modes of adsorbed water molecules and surface hydroxyl groups, respectively. G / BOC-15 has the strongest peaks at both locations, indicating that the hydroxyl content is the highest. However, the excessively high concentration of glucose (20%) is sacrificed as a growth template, resulting in a decrease in the content of surface hydroxyl functional groups.
[0044] This also confirms that we can obtain the photocatalytic material G / BOC-15 with the best performance by regulating the content of glucose during the synthesis process, that is, regulating the surface hydroxyl content of the catalyst.
[0045] Example 2
[0046] Under the action of 500W Hg lamp, the photocatalytic degradation experiment of polystyrene microplastics was carried out using a photoreaction instrument.
[0047] First, 1g / L of micron-level plastic was dispersed in 100mL of aqueous solution, and then 0.5g / L of photocatalyst was added to the above solution. After 12 hours of reaction, the light source was turned off, and the solution was filtered through a water system filter membrane with a pore size of 0.45μm (the filter membrane was dried 24 hours in advance). The filtered filter membrane and the mixture of microplastics and photocatalyst on the filter membrane were removed, dried at 60℃ for 24 hours and weighed.
[0048] The results are as follows Figure 4 As shown in (a), under direct ultraviolet irradiation, the weight loss rate of PS-MPs is 12.8%. BOC and G / BOC-X significantly accelerated the photodegradation of PS-MPs (the weight loss range of PS-MPs was 20-38%), among which the presence of G / BOC-15 made the weight loss rate of PS-MPs the highest, and it was able to achieve a 38% degradation weight loss rate for polystyrene microplastics in 12 hours, and had very good catalytic degradation performance for polystyrene microplastics.
[0049] According to the formula The photodegradation efficiency (ξ) of the photocatalyst was calculated, which is an important indicator for evaluating the activity of the photocatalyst and can be used to reflect the degree of acceleration of the photocatalyst, where WL1 and WL0 are the photodegradation rates in the presence and absence of BOC or G / BOC-X, respectively.
[0050] according to Figure 4 (a) It can be seen that after 12h of irradiation, the photodegradation efficiency ξ values of the photocatalysts are 50% (BOC), 100% (G / BOC-7), 120% (G / BOC-10), 160% (G / BOC-15), and 55% (G / BOC-20), respectively.
[0051] The photocatalytic performance of G / BOC-15 is significantly better than that of other compounds. In order to further study the effect of surface hydroxyl groups on MPs degradation, the relationship between the MPs weight loss rate and the content of hydroxyl functional groups on the surface of the photocatalyst was investigated by linear regression analysis. The fitting results are shown in Figure 4 As shown in (b), the two are positively correlated. When the content of hydroxyl functional groups on the surface of the material is about 15%, the photodegradation efficiency of PS-MPs reaches 160%, and the performance reaches the best.
[0052] G / BOC-15 also exhibits excellent catalytic performance in the degradation of different types of microplastics. Under the same degradation conditions, the weight loss rates of polylactic acid, polystyrene, polybutylene terephthalate-adipate and polyvinyl chloride are 73%, 38%, 28% and 25%, respectively.
[0053] Example 3
[0054] Different from step (2) in Example 1, D+(-) glucose was used instead of aD-glucose to modify the surface hydroxyl functional groups in the same proportion. By testing the degradation performance of PS microplastics under the same conditions, it was found that the weight loss rate of PS modified with D+(-) glucose was 15%, while the weight loss rate of PS modified with aD-glucose was 38%. The photocatalytic degradation performance of microplastics modified with aD-glucose is 2.53 times that of D+(-) glucose.
[0055] The present invention is not limited to the specific technical solutions described in the above embodiments, and all technical solutions formed by equivalent replacement are within the protection scope required by the present invention.
Claims
1. A method for using a surface hydroxyl-modified defective bismuth oxyhalide photocatalytic material to degrade microplastics. Features: The specific steps are: (1) Bi(NO 3 ) 3 ·5H 2 O and potassium chloride are added to the mixture of ethanol and water; (2) dissolving a certain amount of α-D-glucose in a mixture of water and ethanol, wherein the volume ratio of water to ethanol is 1:1; (3) then dripping the glucose solution prepared in step (2) into the mixed solution in step (1), and continuing stirring for 60 minutes; (4) The final solution was transferred to a polytetrafluoroethylene autoclave, and then heated to 100-150° C. for hydrothermal reaction for 10 h; (5) collecting the product obtained in step (4), washing it alternately with deionized water and ethanol, and then drying it in a drying oven at 60° C. overnight, wherein the mass ratio of α-D-glucose to BiOCl is 15%, and the obtained BiOCl product is labeled as G / BOC-15; (6) Under the action of 5-degree ultraviolet light, 0.5 g / L of photocatalyst G / BOC-15 was added to the polystyrene microplastics PS-MPs solution, and the photocatalytic degradation of the microplastics PS-MPs was carried out using a photoreaction instrument.
2. The method for degrading microplastics using the surface hydroxyl-modified defective bismuth oxyhalide photocatalytic material according to claim 1, Features: The specific steps are: (1) 4.8 mmol of Bi(NO 3 ) 3 ·5H 2 O and 4.8mmol potassium chloride were added to a mixture consisting of 28mL ethanol and 12mL water; (2) dissolving 0.1875 g of α-D-glucose in a mixture of water and ethanol, wherein the volume ratio of water to ethanol is 1:1; (3) then dripping the glucose solution prepared in step (2) into the mixed solution in step (1), and continuing stirring for 60 minutes; (4) The final solution was transferred to a polytetrafluoroethylene autoclave, and then heated to 100-150° C. for hydrothermal reaction for 10 h; (5) collecting the product obtained in step (4), washing it alternately with deionized water and ethanol, and then drying it in a drying oven at 60° C. overnight, wherein the mass ratio of α-D-glucose to BiOCl is 15%, and the obtained BiOCl product is labeled as G / BOC-15; (6) Under the action of a 500W Hg lamp, 1 g / L of micron-sized plastic PS-MPs was dispersed in 100 mL of aqueous solution, and then 0.5 g / L of photocatalyst G / BOC-15 was added to the above solution. The photocatalytic degradation of microplastic PS-MPs was carried out using a photoreaction instrument. After 12 hours of reaction, the light source was turned off and the solution was filtered using a water system filter membrane with a pore size of 0.45 μm.
3. The method for degrading microplastics using the surface hydroxyl-modified defective bismuth oxyhalide photocatalytic material according to claim 1, Features: When the mass ratio of α-D-glucose to BiOCl added in step (2) is 15%, the performance of the prepared particle stacked G / BOC-15 material is optimal.
4. The method for degrading microplastics using the surface hydroxyl-modified defective bismuth oxyhalide photocatalytic material according to claim 1, Features: By changing the amount of α-D-glucose used in step (2), the morphology of BiOCl and the content of surface hydroxyl functional groups can be regulated, and the prepared G / BOC-15 photocatalyst has the largest amount of surface hydroxyl modification and the presence of oxygen defects, and has the best performance in photocatalytic degradation of polystyrene microplastics.
5. The method for degrading microplastics using the surface hydroxyl-modified defective bismuth oxyhalide photocatalytic material according to claim 1, Features: Under direct ultraviolet irradiation, the presence of G / BOC-15 makes the weight loss rate of polystyrene microplastics the highest, and can achieve a degradation weight loss rate of 38% for polystyrene microplastics in 12 hours, and has very good catalytic degradation performance for polystyrene microplastics.
Citation Information
Patent Citations
Preparation method of BiOCl photocatalyst, prepared photocatalyst and application of prepared photocatalyst
CN107159274A
Universal synthesis method of high-activity sugar modified bismuth oxyhalide photocatalytic material
CN111921542A