Titanium extraction slag-based cementing material for mine full-tailing cemented filling and preparation method of titanium extraction slag-based cementing material

By using titanium slag-based cementitious materials to replace ordinary silicate cement, the problems of high carbon emissions and high costs of cemented backfill materials for mine tailings have been solved, achieving low-carbon, safe, and efficient backfilling results.

CN119019120AActive Publication Date: 2024-11-26UNIV OF SCI & TECH BEIJING +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411024368.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-26
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

In existing technologies, the cemented backfill material for mine tailings mainly uses ordinary silicate cement, which leads to high carbon emissions and high costs. Furthermore, the manufacturing and use of traditional backfill materials are not environmentally friendly.

Method used

A cementitious material based on titanium-extracting slag, including titanium-extracting slag, vanadium-titanium tailings powder, calcium sulfate tailings, carbide slag, inorganic grinding aids, organic grinding aids, and silane coupling modifiers, is prepared through a specific preparation method to create a cementitious material that can replace ordinary silicate cement.

Benefits of technology

It achieves low carbon emissions and low cost of fully cemented tailings backfill material, improves the rheological and mechanical properties of the backfill material, reduces cement consumption, increases the utilization rate of tailings, and achieves a better effect than cement consolidation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019120A_ABST
    Figure CN119019120A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of metal mine underground filling, in particular to a titanium extraction slag-based cementing material for mine full-tailing cemented filling and a preparation method of the titanium extraction slag-based cementing material. The invention discloses a titanium extraction slag-based cementing material for mine full-tailing cemented filling. The titanium extraction slag-based cementing material comprises the following components in parts by mass: 300-400 parts of titanium extraction slag, 450-500 parts of vanadium-titanium tailing powder, 100-120 parts of glauberite tailings, 10-20 parts of carbide slag, 13-15 parts of an inorganic grinding aid, 4-6 parts of an organic grinding aid and 1-3 parts of a silane coupling agent modifier. The rheological property, the mechanical property and the durability of the full-tailing cemented filling material prepared from the titanium extraction slag-based cementing material can meet the requirements of mine filling. The titanium extraction slag-based cementing material is used for full tailing filling, so that the consumption of materials such as cement is greatly reduced, the filling cost is reduced, the carbon emission is reduced, the utilization rate of tailings is increased, and the purposes of low-carbon, safe and efficient production can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of underground filling of metal mines, and in particular to a titanium-extracting slag-based cementitious material used for cementing and filling of full tailings in mines and a preparation method thereof. Background Art

[0002] After smelting in a blast furnace, Panzhihua Iron and Steel's vanadium-titanium magnetite will produce granular or blocky blast furnace waste slag. After using the chlorination method to extract titanium resources, a new type of industrial titanium-extracting slag can be obtained. Panzhihua Iron and Steel produces more than 2 million tons of high-titanium blast furnace slag as a by-product every year, and about 50 million tons have been piled up so far. If the titanium-extracting slag can be used in the cementation filling of the mine's full tailings, it can not only reduce the filling cost, but also reduce the area occupied by its surface storage, which is also of great significance to regional environmental protection.

[0003] At present, one of the main disposal methods for the above-mentioned tailings is to mix these tailings with a certain proportion of cement or cement powder to prepare cementitious filling materials for filling the goaf of mines. In traditional cementitious filling materials, the aggregate of the full tailings cementitious filling body is the full-grade tailings without desludging from the concentrator, and the cementitious material usually uses ordinary silicate cement. The two are evenly mixed with water in a certain proportion to form a filling slurry, which is transported to the goaf underground through pipelines. Although my country's total cement output is relatively high, the cement manufacturing process is a high-carbon emission process. The use of cement not only increases the cost of tailings treatment, but also increases carbon emissions.

[0004] Therefore, there is an urgent need to provide a technical solution to the above-mentioned deficiencies in the prior art. Summary of the invention

[0005] In view of the above technical problems, the present invention provides a titanium-extracting slag-based cementitious material for full tailings cementing filling in mines and a preparation method thereof. The titanium-extracting slag-based cementitious material provided by the present invention can completely replace ordinary silicate cement in full tailings filling and can achieve a better effect than cement consolidation, thereby reducing cement consumption, reducing costs and reducing carbon emissions.

[0006] In order to achieve the above-mentioned purpose of the invention, the present invention provides a titanium-extracting slag-based cementitious material for cementing and filling of mine tailings, which adopts the following technical scheme: A titanium-extracting slag-based cementitious material for cementing and filling whole tailings in mines comprises the following components in parts by mass: 300-400 parts of titanium-extracting slag, 450-500 parts of vanadium-titanium tailings powder, 100-120 parts of glauberite tailings, 10-20 parts of carbide slag, 13-15 parts of inorganic grinding aids, 4-6 parts of organic grinding aids and 1-3 parts of silane coupling agent modifier.

[0007] Preferably, the mineral components of the titanium slag include β-C2S, γ-C2S, calcite, calcium titanate and a large amount of glass, wherein the glass is derived from the decomposition and melting of minerals at high temperatures, and is an amorphous substance formed because the atoms cannot reach the degree of order required by the crystal; the titanium slag includes the following components in percentage by mass: 35-40% CaO, 15-20% SiO2, 10-15% Al2O3, 5-8% Fe2O3, 2-3% MgO, 2-3% TiO2, 5-7% Cl, 1-2% SO3, and the remainder is other chemical components. It can be seen from the above chemical composition that the content of calcium oxide in the titanium slag reaches 35-40%, so the titanium slag belongs to high-calcium tailings.

[0008] Preferably, the vanadium-titanium tailings powder comprises the following components in percentage by mass: 20-22% Fe2O3, 11-13% CaO, 30-33% SiO2, 14-16% Al2O3, 8-10% TiO, 10-12% MgO, and 0.5-1% of other chemical components.

[0009] Preferably, in the glauberite tailings, the mass percentage of Na2SO4 is 17-25%, and the mass percentage of CaSO4 is 41-46%. The glauberite tailings used in the present invention are tailings produced after glauberite mines are used to produce sodium sulfate (Na2SO4), which contain a large amount of CaSO4 associated with Na2SO4.

[0010] Preferably, the main components of the carbide slag are Ca(OH)2 and CaCO3, wherein the mass percentage of Ca(OH)2 is greater than or equal to 80%, and the specific surface area is 423m 2 / kg.

[0011] Preferably, the inorganic grinding aid is ultrafine magnesium oxide, and the specific surface area of ​​the ultrafine magnesium oxide is 610-630 m 2 / kg; the organic grinding aid is triethanolamine; the silane coupling agent modifier is a silane coupling agent alcohol solution, and the silane coupling agent is γ-aminopropyltriethoxysilane. The organic grinding aid is industrial grade triethanolamine. (It can improve the early strength of the grouting material) In order to achieve the above-mentioned purpose of the invention, the present invention provides a method for preparing a titanium-extracting slag-based cementitious material for cementing and filling of mine tailings, which adopts the following technical scheme: A method for preparing a titanium-extracting slag-based cementitious material for cementing and filling of mine tailings comprises the following steps: (1) spraying a silane coupling agent modifier uniformly on the surface of an inorganic grinding aid, stirring and then drying to obtain an inorganic grinding aid modified by a silane coupling agent; the mass ratio of the silane coupling agent modifier to the inorganic grinding aid is 1:60-70, the stirring rate is 1300-1400 r / min, the stirring time is 20-30 min, the drying temperature is 90-100° C., and the drying time is 4-5 h; (2) drying the titanium-extracting slag at 100-110°C, spraying the organic grinding aid evenly on the surface of the titanium-extracting slag, and then placing it in a test mill for grinding for 15-20 minutes, adding the inorganic grinding aid modified by the silane coupling agent, and continuing to grind for 20-30 minutes to obtain modified titanium-extracting slag powder; (3) grinding the vanadium-titanium tailings powder to obtain vanadium-titanium tailings fine powder; mixing and grinding the glauberite tailings and carbide slag to obtain a mixture of carbide slag and glauberite tailings; (4) The modified titanium-extracting slag powder, vanadium-titanium tailings powder, carbide slag and glauberite tailings mixture are uniformly mixed to obtain a titanium-extracting slag-based cementitious material with full tailings cementation filling.

[0012] By modifying the surface of magnesium oxide with a silane coupling modifier, an organic molecular layer can be generated on the surface of the inorganic powder, changing the inorganic powder from hydrophilic to organic, making the filler dispersed evenly, and improving the water repellency of the material.

[0013] Since the titanium-extracting slag is the main volcanic ash active substance in the filling material of the present invention, the fine volcanic ash activity of the titanium-extracting slag directly determines the performance of the filling cementitious material, so the titanium-extracting slag is ground and activated separately from other tailings (vanadium-titanium tailings, carbide slag and glauberite tailings).

[0014] At 100-110°C, the moisture in the titanium extraction slag is dried after 5 hours of drying. If the drying time is too short, the titanium extraction slag will contain residual moisture.

[0015] Inorganic grinding aids (ultrafine magnesium oxide) can enter the cracks generated during the grinding process of titanium slag to improve the grinding efficiency of titanium slag. It can also hydrate in the grouting slurry to generate magnesium hydroxide to expand, thereby offsetting the volume shrinkage caused by hydration, temperature changes and water loss of the grouting cementitious material. It has good temperature stability and low price.

[0016] Preferably, in step (2), the test mill is a 5kg cement test mill with a model of Ø500×500, a ball-to-material ratio of 3:1, a test mill speed of 45-55 r / min, and a specific surface area of ​​the modified titanium slag powder of 485 m 2 / kg,d 50 =18~20μm.

[0017] Preferably, in step (3), the vanadium-titanium tailings powder is ground using a 5kg cement test mill, the ball-to-material ratio is 3:1, and the grinding time is 10 to 15 minutes; the specific surface areas of the vanadium-titanium tailings powder before and after grinding are 420 to 450 m 2 / kg and 650~700m 2 / kg, its d before and after grinding 50 They are 16-18 μm and 7-8 μm respectively; The mixed grinding of the calcium glauberite tailings and the calcium carbide slag adopts a 5kg cement test mill, the ball-to-material ratio is 3:1, the grinding time is 10 to 20 minutes, and the specific surface area of ​​the mixed material of the calcium carbide slag and the calcium glauberite tailings is 350 to 400m 2 / kg,d 50 =25~28μm.

[0018] In order to achieve the above-mentioned purpose of the invention, the present invention provides a titanium-extracting slag-based cementitious material for cementing and filling the whole tailings of a mine, which adopts the following technical scheme: An application of a titanium-extracting slag-based cementitious material for cementing and filling the whole tailings of a mine. The titanium-extracting slag-based cementitious material is used for cementing and filling the whole tailings of a mine. The whole tailings cementing and filling material for a mine comprises the following components in parts by mass: 180 to 200 parts of titanium-extracting slag-based cementitious material, 630 to 660 parts of water, and 1200 to 1300 parts of tailings.

[0019] Beneficial effects: The titanium-extracting slag-based cementitious material provided by the present invention mainly uses solid waste (titanium-extracting slag, vanadium-titanium tailings powder and calcium glauberite tailings) as raw materials, supplemented with inorganic grinding aids, organic grinding aids, carbide slag and silane coupling agent modifiers to prepare titanium-extracting slag-based cementitious materials. Compared with the traditional full tailings cementitious filling body using cement materials as binders, the rheological properties, mechanical properties and durability of the full tailings cementitious filling material prepared using the titanium-extracting slag-based cementitious material of the present invention can meet the requirements of mine filling. The titanium-extracting slag-based cementitious material is used to completely replace ordinary silicate cement in full tailings filling and can achieve an effect better than cement consolidation, greatly reducing the consumption of materials such as cement, reducing filling costs, reducing carbon emissions, and increasing tailings utilization, which can achieve low-carbon, safe and efficient production goals. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] The drawings constituting part of the present application are used to provide a further understanding of the present application. The exemplary embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. Among them: Figure 1 XRD spectrum for phase analysis of titanium slag; Figure 2 This is a curve chart of grinding time and specific surface area of ​​titanium slag. DETAILED DESCRIPTION

[0021] The present application will be described in detail below with reference to the accompanying drawings and in conjunction with embodiments. Each example is provided by way of explanation of the present application and does not limit the present application. In fact, it will be clear to those skilled in the art that modifications and variations may be made in the present application without departing from the scope or spirit of the present application. For example, a feature shown or described as a part of an embodiment may be used in another embodiment to produce yet another embodiment. All other embodiments obtained by those of ordinary skill in the art based on the embodiments in the embodiments of the present invention should belong to the scope of protection of the embodiments of the present invention.

[0022] Example 1 A method for preparing a titanium-extracting slag-based cementitious material for cementing and filling of mine tailings comprises the following steps: (1) Weigh 15 parts of ultrafine magnesium oxide and 3 parts of silane coupling agent modifier respectively, spray the silane modifier alcohol solution evenly on the surface of ultrafine magnesium oxide, stir at a rate of 1400r / min for 30min and then dry for 4h to obtain silane coupling agent modified magnesium oxide. The mass ratio of silane coupling agent modifier to ultrafine magnesium oxide is 1:60. The preparation process of silane coupling agent alcohol solution includes the following steps: ① prepare alcohol solvent, mix water and alcohol (isopropanol or ethanol) in a mass ratio of 1:8, and stir evenly; ② prepare silane coupling agent alcohol solution, mix silane and alcohol solvent in a mass ratio of 1:5, and stir evenly.

[0023] (2) Take 400 parts of titanium slag and put them into an oven at a drying temperature of 110°C for 4 hours. Take 6 parts of triethanolamine and spray them evenly on the surface of the titanium slag, then place it in a test mill and grind it for 15 minutes. Then add the modified magnesium oxide into the test mill and continue grinding for 30 minutes to obtain modified titanium slag powder. The test mill is a 5kg cement test mill with a model of Ø500×500, a ball-to-material ratio of 3:1, a test mill speed of 50±5r / min, and a specific surface area of ​​the modified titanium slag powder of 485m 2 / kg,d 50 =18~20μm.

[0024] (3) Take the specific surface area of ​​420~450m 2 / kg,d 50 = 450 parts of vanadium-titanium tailings powder with a particle size of 16-18 μm were ground to a specific surface area of ​​650 m2 using a 5 kg cement test mill with a ball-to-material ratio of 3:1. 2 / kg,d 50 =8μm, and vanadium-titanium tailings powder was obtained. 20 parts of carbide slag and 100 parts of calcium glauberite tailings were mixed and ground for 20 minutes using a 5kg cement test mill with a ball-to-material ratio of 3:1 to obtain a powder with a specific surface area of ​​400m 2 / kg,d 50 =25μm mixture of carbide slag and glauberite tailings.

[0025] (4) The modified titanium-extracting slag powder, vanadium-titanium tailings powder, carbide slag and calcium glauberite tailings mixture are uniformly mixed to obtain a titanium-extracting slag-based cementitious material A1 with full tailings cementation filling.

[0026] Depend on Figure 1 It can be seen that the XRD spectrum of titanium slag is normal, most of the phase components are glass, containing some β-C2S, γ-C2S, calcite and calcium titanate and other crystalline minerals. After proper grinding, it has high potential activity. From the XRD spectrum, it can be seen that the main mineral components in the tailings are kaolinite, feldspar, calcite, brookite (TiO2) and magnesite (magnesium carbonate), etc. The grinding specific surface area is from 450m 2 / kg increased to 670m 2 / kg, the diffraction intensity of the characteristic peaks of kaolinite and albite in XRD was significantly weakened, indicating that mechanical force activation has a significant effect on these two minerals. No obvious quartz characteristic peaks were detected in the tailings, indicating that the quartz content is low. The SiO2 component in the raw materials mainly exists in the form of feldspar and kaolinite minerals, which is conducive to its activation by mechanical force.

[0027] Figure 2 In order to analyze the relationship between the grinding time and specific surface area of ​​titanium slag, Figure 2 It can be seen that within 15 minutes of grinding, the specific surface area of ​​titanium slag is linearly related to the grinding time, and the first peak of 303m is reached after 15 minutes of grinding. 2 / kg; after that, the specific surface area showed a downward trend with the increase of grinding time, and reached the second peak of 393m at 25min of grinding. 2 / kg, and then it dropped again, indicating that reverse crushing is prone to occur in grinding without adding grinding aids, the materials agglomerate, and the specific surface area is difficult to increase further.

[0028] It was found from the above experiments that the activity of titanium-extracting slag is proportional to the specific surface area of ​​the titanium-extracting slag after grinding. The activity index of the titanium-extracting slag after grinding and activation in the present invention can reach 92.3% at 28 days. The test was carried out according to the "Test Method for Strength of Cement Mortar (ISO Method)" (GB / T 17671-2020) to determine the compressive strength of titanium-extracting slag mortar and cement comparison mortar, and the activity index of titanium-extracting slag micropowder was determined by the ratio of the compressive strengths of the two.

[0029] Example 2 A method for preparing a titanium-extracting slag-based cementitious material for cementing and filling of mine tailings comprises the following steps: (1) Weigh 13 parts of ultrafine magnesium oxide and 1 part of silane coupling agent modifier respectively, spray the silane modifier alcohol solution evenly on the surface of the ultrafine magnesium oxide, stir at a rate of 1300r / min for 20min and dry for 5h to obtain magnesium oxide modified by silane coupling agent. The mass ratio of silane coupling agent modifier to ultrafine magnesium oxide is 1:60.

[0030] (2) Take 300 parts of titanium slag and put them into an oven at a drying temperature of 110°C for 5 hours. Take 4 parts of triethanolamine and spray them evenly on the surface of the titanium slag, then put it into a test mill and grind it for 15 minutes. Then put the modified magnesium oxide into the test mill and continue grinding for 30 minutes to obtain modified titanium slag powder. The test mill is a 5kg cement test mill with a model of Ø500×500, a ball-to-material ratio of 3:1, a test mill speed of 50±5r / min, and a specific surface area of ​​the modified titanium slag powder of 485m 2 / kg,d 50 =18~20μm.

[0031] (3) Take the specific surface area of ​​420~450m 2 / kg,d 50 = 500 parts of vanadium-titanium tailings powder with a particle size of 16-18 μm were ground to a specific surface area of ​​650 m2 using a test mill with a ball-to-material ratio of 3:1. 2 / kg,d 50 =8μm, and vanadium-titanium tailings powder was obtained. 10 parts of carbide slag and 120 parts of calcium glauberite tailings were mixed and ground for 10 minutes using a test mill with a ball-to-material ratio of 3:1 to obtain a specific surface area of ​​350m 2 / kg,d 50 =28μm mixture of carbide slag and glauberite tailings.

[0032] (4) The modified titanium-extracting slag powder, vanadium-titanium tailings powder, carbide slag and calcium glauberite tailings mixture are uniformly mixed to obtain a titanium-extracting slag-based cementitious material A2 with full tailings cementation filling.

[0033] Example 3 A method for preparing a titanium-extracting slag-based cementitious material for cementing and filling of mine tailings comprises the following steps: (1) Weigh 14 parts of ultrafine magnesium oxide and 2 parts of silane coupling agent modifier respectively. Spray the silane modifier alcohol solution evenly on the surface of ultrafine magnesium oxide, stir at a rate of 1300r / min for 15min and dry for 5h to obtain magnesium oxide modified by silane coupling agent. The mass ratio of silane coupling agent modifier to ultrafine magnesium oxide is 1:70.

[0034] (2) Take 350 parts of titanium slag and put them into an oven at a drying temperature of 110°C for 4 hours. Take 5 parts of triethanolamine and spray it evenly on the surface of the titanium slag, then put it into a test mill and grind it for 20 minutes. Then put the modified magnesium oxide into the test mill and continue grinding for 30 minutes to obtain modified titanium slag powder. The test mill is a 5kg cement test mill with a model of Ø500×500, a ball-to-material ratio of 3:1, a test mill speed of 50±5r / min, and a specific surface area of ​​the modified titanium slag powder of 485m 2 / kg,d 50 =18~20μm.

[0035] (3) Take the specific surface area of ​​420~450m 2 / kg,d 50 = 550 parts of vanadium-titanium tailings powder with a size of 16-18 μm were ground to a specific surface area of ​​700 m2 using a test mill with a ball-to-material ratio of 3:1. 2 / kg,d 50 =7μm, and vanadium-titanium tailings powder was obtained. 10 parts of carbide slag and 120 parts of calcium glauberite tailings were mixed and ground for 15 minutes using a test mill with a ball-to-material ratio of 3:1 to obtain a specific surface area of ​​380m 2 / kg,d 50 =26μm mixture of carbide slag and glauberite tailings.

[0036] (4) The modified titanium-extracting slag powder, vanadium-titanium tailings powder, carbide slag and calcium glauberite tailings mixture are uniformly mixed to obtain a titanium-extracting slag-based cementitious material A3 with full tailings cementation filling.

[0037] Example 4 A method for preparing a full tailings cemented filling material using titanium-extracting slag-based cementitious material comprises the following steps: (1) Prepare the materials: weigh 200 parts of titanium-extracting slag-based cementitious material (A1), 660 parts of water, and 1,200 parts of tailings according to their mass proportions.

[0038] (2) Put the above prepared materials into a concrete mixer and mix them evenly to obtain a mixture of all-tailings cemented filling materials; (3) The above-mentioned full tailings cemented filling material mixture is filled into a mold, demolded after 48 hours, and cured under standard curing conditions (20±2°C, 95±5% relative humidity) to obtain full tailings cemented filling material test block B1.

[0039] Example 5 A method for preparing a full tailings cemented filling material using titanium-extracting slag-based cementitious material comprises the following steps: (1) Prepare the materials: weigh 190 parts of titanium-extracting slag-based cementitious material (A2), 630 parts of water, and 1,300 parts of tailings according to their mass proportions.

[0040] (2) Put the above prepared materials into a concrete mixer and mix them evenly to obtain a mixture of all-tailings cemented filling materials; (3) The above-mentioned full tailings cemented filling material mixture is filled into a mold, demolded after 48 hours, and cured under standard curing conditions (20±2°C, 95±5% relative humidity) to obtain full tailings cemented filling material test block B2.

[0041] Example 6 A method for preparing a full tailings cemented filling material using titanium-extracting slag-based cementitious material comprises the following steps: (1) Prepare the materials. Weigh 180 parts of titanium-extracting slag-based cementitious material (A3), 640 parts of water, and 1,300 parts of tailings according to their mass proportions.

[0042] (2) Put the above-prepared materials into a concrete mixer and mix them evenly to obtain a mixture of tailings cemented filling materials.

[0043] (3) The above-mentioned full tailings cemented filling material mixture was filled into a mold, demolded after 48 hours, and cured under standard curing conditions (20±2°C, 95±5% relative humidity) to obtain full tailings cemented filling material specimen B3.

[0044] Comparative Example 1 A method for preparing a cement-based cementitious filling material comprises the following steps: (1) Prepare the materials: weigh 200 parts of 32.5 composite silicate cement, 660 parts of water, and 1200 parts of metal tailings according to their mass proportions.

[0045] (2) Put the above-prepared materials into a concrete mixer and mix them evenly to obtain cement-based bonding filling materials.

[0046] (3) The above-mentioned cement-based cementitious filling material was filled into a mold, demolded after 48 hours, and cured for 28 days under standard curing conditions (20±2°C, 95±5% relative humidity) to obtain a full tailings cementitious filling material specimen S1.

[0047] Comparative Example 2 A method for preparing a cement-based cementitious filling material comprises the following steps: (1) Prepare the materials: weigh 600 parts of 42.5 ordinary Portland cement, 15 parts of water, and 1500 parts of metal tailings powder according to their mass proportions.

[0048] (2) The prepared materials are placed in a concrete mixer and mixed evenly to obtain a cement-based cementitious filling material.

[0049] (3) The cement-based cementitious filling material is filled into a mold, demolded after 48 hours, and cured for 28 days under standard curing conditions (20±2°C, 95±5% relative humidity) to obtain a full tailings cementitious filling material test block S2.

[0050] Characterization and analysis The mechanical properties of the filling materials of Examples 4-6 and Comparative Examples 1-6 were tested according to the GB / T17671-2021 cement mortar strength test method. The results are shown in Table 1. Table 1 Mechanical properties test results The expansion rate of the filling materials of Examples 4-6 and Comparative Examples 1-6 was tested according to the JC / T313-2009 expansion rate test method for expansion cement. The results are shown in Table 2. Table 2 Expansion rate test results From the above results, it can be seen that the full tailings cementing filling material prepared with the titanium slag-based cementing material provided by the present invention has good mechanical properties, and the 7d compressive strength can reach 5.21MPa, which is 54.1% higher than that of cement-based cementing filling materials, and the 28d strength can reach 12.115MPa, which is 95.0% higher than that of cement-based cementing filling materials. In addition, the 7d expansion rate of the full tailings cementing filling material prepared by the embodiment of the present invention is 1.21%~1.56%, and the 28d expansion rate does not change much compared with the 7d expansion rate, which can avoid the influence of late expansion on filling. The above results show that the full tailings cementing filling material provided by the present invention has better expansion performance than cement without adding an expansion agent, which can effectively avoid multiple grouting and greatly save manpower and material resources. The comprehensive experimental results of Examples 4~6 in terms of mechanical properties and expansion rate are better than those of the comparative examples.

[0051] In the present invention, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" mean that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0052] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A titanium-extracting slag-based cementitious material for cementing and filling of mine tailings, characterized in that: The invention comprises the following components in parts by weight: 300-400 parts of titanium extraction slag, 450-500 parts of vanadium-titanium tailings powder, 100-120 parts of calcium glauberite tailings, 10-20 parts of carbide slag, 13-15 parts of inorganic grinding aids, 4-6 parts of organic grinding aids and 1-3 parts of silane coupling agent modifier.

2. The titanium-extracting slag-based cementitious material for cementing and filling of mine tailings according to claim 1, characterized in that: The mineral components of the titanium-extracting slag include β-C2S, γ-C2S, calcium aluminum feldspar, and calcium titanate; the titanium-extracting slag includes the following components in percentage by mass: 35-40% CaO, 15-20% SiO2, 10-15% Al2O3, 5-8% Fe2O3, 2-3% MgO, 2-3% TiO2, 5-7% Cl, and 1-2% SO3.

3. The titanium-extracting slag-based cementitious material for cementing and filling of mine tailings according to claim 1, characterized in that: The vanadium-titanium tailings powder includes the following components in percentage by mass: 20-22% Fe2O3, 11-13% CaO, 30-33% SiO2, 14-16% Al2O3, 8-10% TiO, and 10-12% MgO.

4. The titanium-extracting slag-based cementitious material for cementing and filling of mine tailings according to claim 1, characterized in that: In the glauberite tailings, the mass percentage of Na2SO4 is 17-25%, and the mass percentage of CaSO4 is 41-46%.

5. The titanium-extracting slag-based cementitious material for cementing and filling of mine tailings according to claim 1, characterized in that: The main components of the carbide slag are Ca(OH)2 and CaCO3, wherein the mass percentage of Ca(OH)2 is greater than or equal to 80%, and the specific surface area is 423m 2 / kg.

6. The titanium-extracting slag-based cementitious material for cementing and filling of mine tailings according to claim 1, characterized in that: The inorganic grinding aid is ultrafine magnesium oxide, and the specific surface area of ​​the ultrafine magnesium oxide is 610-630m 2 / kg; the organic grinding aid is triethanolamine; the silane coupling agent modifier is a silane coupling agent alcohol solution, and the silane coupling agent is γ-aminopropyltriethoxysilane.

7. The method for preparing a titanium-extracting slag-based cementitious material for cementing and filling whole tailings in mines according to any one of claims 1 to 6, characterized in that: The following steps are involved: (1) spraying a silane coupling agent modifier uniformly on the surface of an inorganic grinding aid, stirring and then drying to obtain an inorganic grinding aid modified by a silane coupling agent; the mass ratio of the silane coupling agent modifier to the inorganic grinding aid is 1:60-70, the stirring rate is 1300-1400 r / min, the stirring time is 20-30 min, the drying temperature is 90-100° C., and the drying time is 4-5 h; (2) drying the titanium-extracting slag at 100-110°C, spraying the organic grinding aid evenly on the surface of the titanium-extracting slag, and then placing it in a test mill for grinding for 15-20 minutes, adding the inorganic grinding aid modified by the silane coupling agent, and continuing to grind for 20-30 minutes to obtain modified titanium-extracting slag powder; (3) grinding the vanadium-titanium tailings powder to obtain vanadium-titanium tailings fine powder; mixing and grinding the glauberite tailings and carbide slag to obtain a mixture of carbide slag and glauberite tailings; (4) The modified titanium-extracting slag powder, vanadium-titanium tailings powder, carbide slag and calcium glauberite tailings mixture are uniformly mixed to obtain a titanium-extracting slag-based cementitious material with full tailings cementation filling.

8. The method for preparing titanium-extracting slag-based cementitious material for cementing and filling of mine tailings according to claim 7, characterized in that: In step (2), the test mill is a 5kg cement test mill with a model of Ø500×500, a ball-to-material ratio of 3:1, a test mill speed of 45-55 r / min, and a specific surface area of ​​the modified titanium slag powder of 485 m 2 / kg,d 50 =18~20μm.

9. The method for preparing titanium-extracting slag-based cementitious material for cementing and filling of mine tailings according to claim 7, characterized in that: In step (3), the vanadium-titanium tailings powder is ground using a 5kg cement test mill, the ball-to-material ratio is 3:1, and the grinding time is 10 to 15 minutes; the specific surface areas of the vanadium-titanium tailings powder before and after grinding are 420 to 450 m 2 / kg and 650~700m 2 / kg, its d before and after grinding 50 The surface area of ​​the mixed material of glauberite tailings and carbide slag is 350-400m 2 / kg,d 50 =25~28μm.

10. The use of titanium-extracting slag-based cementitious material for cementing and filling of whole tailings in mines as described in any one of claims 1 to 6, wherein the titanium-extracting slag-based cementitious material is used for cementing and filling of whole tailings in mines, and the cementing and filling material for whole tailings in mines comprises the following components in parts by mass: 180 to 200 parts of titanium-extracting slag-based cementitious material, 630 to 660 parts of water, and 1200 to 1300 parts of tailings.

Citation Information

Patent Citations

  • Gel material for filling worked out section by vanadium-titanium-containing slags

    CN103739263A

  • Concrete expanding agent

    CN106277887A

  • Cementing powder special for full-tailing cemented filling and preparation method thereof

    CN113800859A

  • Gold tailing-based auxiliary cementing material as well as preparation method and application thereof

    CN117361907A

  • Vanadium-titanium tailing-based clinker-free cementing material and preparation method thereof