Corrosion-resistant high-strength magnesium-based prestressed pipe pile and preparation method thereof
Through the combination of magnesium-based prestressed pipe piles and magnesium-oxygen slurry layer, the problem of strong corrosion in the near-shore tidal flat areas is solved, the structural stability and durability are improved, and it is suitable for photovoltaic power generation equipment. use requirements.
Patent Information
- Application Number
- CN202411127551.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-26
AI Technical Summary
Traditional concrete photovoltaic pipe piles are highly corrosive in the offshore and mudflat areas, and cannot meet the requirements of service life and safety, resulting in insufficient structural stability and durability.
Magnesium-based prestressed pipe piles, including steel bars, magnesium sulfide slurry layer and magnesium oxychloride slurry layer, and an integrated molding structure is formed by casting. The magnesium sulfide slurry layer is compatible with the steel bars, and the magnesium oxychloride slurry layer is suitable for Seawater environment, increasing corrosion resistance and strength.
It has achieved structural stability and durability improvement in high saline and alkali environments, ensuring the long-term safety and reliability of photovoltaic power generation equipment.
Smart Images

Figure CN119019149A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of new energy photovoltaic pipe piles, and in particular relates to a corrosion-resistant and high-strength magnesium-based prestressed pipe pile and a preparation method thereof. Background Art
[0002] Photovoltaic power generation is in line with the national new energy development direction. China's photovoltaic power generation installed capacity ranks among the top in the world and has been expanding in recent years. Photovoltaic power generation uses open space to install photovoltaic panels to convert sunlight into electricity. These photovoltaic panels are mounted on pipe piles and are distributed in the sea, land, tidal flats, mountains, grasslands and other places. Depending on the different sites and geological conditions, the construction methods of pipe piles are also different. In particular, offshore photovoltaics have also become an important field for the development of new energy.
[0003] However, for the offshore and tidal flat photovoltaic industry, the soil salinization in the tidal flat and offshore areas is serious, and Cl - The content is relatively high, which is highly corrosive to metals and the upper and lower structures of traditional prestressed concrete photovoltaic pipe piles and brackets. Traditional concrete pipe piles and brackets cannot meet the requirements of service life and safety in this environment.
[0004] Therefore, how to develop a photovoltaic pipe pile with stable structure and strong durability is an urgent problem to be solved by technical personnel in this field. Summary of the invention
[0005] The object of the present invention is to provide a corrosion-resistant high-strength magnesium-based prestressed pipe pile with a stable structure and strong durability. Another object of the present invention is to provide a method for preparing a corrosion-resistant high-strength magnesium-based prestressed pipe pile, which can produce a pipe pile with a stable structure and strong durability.
[0006] In order to solve the above technical problems, the present invention provides a corrosion-resistant and high-strength magnesium-based prestressed pipe pile, comprising steel bars, a pipe pile inner layer and a pipe pile outer layer, wherein the pipe pile outer layer is arranged on the outside of the pipe pile inner layer, and the steel bars are embedded in the pipe pile inner layer along the length direction, and the steel bars, the pipe pile inner layer and the pipe pile outer layer are cast-in-one structure, the pipe pile inner layer is a magnesium oxysulfide slurry layer, and the pipe pile outer layer is a magnesium oxychloride slurry layer.
[0007] Optionally, in the above-mentioned corrosion-resistant and high-strength magnesium-based prestressed pipe piles, the surface of the steel bar is provided with an anti-corrosion coating and an acid- and alkali-resistant coating in sequence from the inside to the outside.
[0008] Optionally, in the above-mentioned corrosion-resistant and high-strength magnesium-based prestressed pipe pile, the magnesium oxychloride slurry layer includes magnesium oxide, magnesium chloride, a modifier and stone particles, and the modifier includes at least one of a halogen-resistant enhancer, a toughening and desolvating agent, a defoaming agent and a curing agent;
[0009] And / or, the magnesium oxysulfide slurry layer includes magnesium oxide, magnesium sulfate, a modifier, silica fume and stone particles, and the modifier includes at least one of a magnesium oxysulfide modifier, a waterproofing agent, a curing agent and a defoaming agent.
[0010] Optionally, in the above-mentioned corrosion-resistant and high-strength magnesium-based prestressed pipe pile, there are multiple steel bars, and the multiple steel bars are evenly arranged along the circumference of the inner layer of the pipe pile.
[0011] Optionally, in the above-mentioned corrosion-resistant and high-strength magnesium-based prestressed pipe pile, the outer wall of the inner layer of the pipe pile and the inner wall of the outer layer of the pipe pile are matched in a concave-convex manner.
[0012] Optionally, in the above-mentioned corrosion-resistant and high-strength magnesium-based prestressed pipe pile, a plurality of convex portions are provided on the outer wall of the inner layer of the pipe pile, and the plurality of convex portions are evenly arranged along the circumference of the inner layer of the pipe pile.
[0013] The present invention also provides a method for preparing a corrosion-resistant and high-strength magnesium-based prestressed pipe pile, using the corrosion-resistant and high-strength magnesium-based prestressed pipe pile described in the above specific embodiment, the method comprising:
[0014] Mixing ingredients, respectively preparing magnesium oxysulfide slurry and magnesium oxychloride slurry;
[0015] In the first pouring, the steel bars are placed in the first precast mold, and the magnesium oxysulfide slurry is injected into the first precast mold;
[0016] Tensioning and first centrifugation, tensioning the first prefabricated mold after the first pouring, placing the tensioned first prefabricated mold into a centrifugal device for centrifugation and demoulding, thereby obtaining a first prefabricated pipe pile;
[0017] The second pouring is to place the first prefabricated pipe pile into a second prefabricated mold, and inject the magnesium oxychloride slurry into the second prefabricated mold to obtain the second prefabricated pipe pile;
[0018] The second centrifugation is performed, and the second prefabricated pipe piles are placed in a centrifugal device for centrifugation and demoulding to obtain corrosion-resistant and high-strength magnesium-based prestressed pipe piles.
[0019] Optionally, in the above preparation method, in the batching step, the raw materials of the magnesium oxychloride slurry include magnesium oxide, magnesium chloride, a modifier and stone particles, and the modifier includes at least one of a halogen-resistant enhancer, a toughening and desolvating agent, a defoaming agent and a curing agent;
[0020] And / or, the raw materials of the magnesium oxysulfide slurry include at least magnesium oxide, magnesium sulfate, a modifier, silica fume and stone particles, and the modifier includes at least one of a magnesium oxysulfide modifier, a waterproofing agent, a curing agent and a defoaming agent.
[0021] Optionally, in the above preparation method, before the first pouring step, the surface of the steel bar is subjected to anti-corrosion treatment.
[0022] Optionally, in the above preparation method, the anti-corrosion treatment step includes: first electroplating a layer of anti-corrosion coating on the surface of the steel bar as a base layer, and then coating a layer of acid and alkali resistant coating on the base layer.
[0023] The present invention provides a corrosion-resistant and high-strength magnesium-based prestressed pipe pile, which has the following beneficial effects:
[0024] The inner layer of the pipe pile is wrapped around the outside of the steel bar, and the outer layer of the pipe pile is wrapped around the outside of the inner layer of the pipe pile. The inner layer of the pipe pile uses magnesium oxysulfide slurry, and the outer layer of the pipe pile uses magnesium oxychloride slurry. In the field of photovoltaic power generation, especially in offshore and tidal flat areas, the chloride ions contained in the magnesium oxychloride slurry material in this case have good compatibility with seawater, and are suitable as the outer layer of the pipe pile in contact with seawater.
[0025] Since there are steel bars inside the pile, magnesium oxychloride slurry is corrosive to the steel bars, while magnesium oxysulfide slurry does not contain chloride ions and is compatible with the steel bars, making it suitable for the inner layer of the pile to contact the steel bars. The magnesium-based prestressed pile, which is an integrated structure formed by pouring steel bars, the inner layer of the pile and the outer layer of the pile, has the characteristics of stable structure and strong durability.
[0026] The present invention also provides a method for preparing a corrosion-resistant and high-strength magnesium-based prestressed pipe pile, which can produce pipe piles with stable structure and strong durability, which will not be described in detail here. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0028] Figure 1 A front view of a portion of a corrosion-resistant and high-strength magnesium-based prestressed pipe pile after being formed in a first prefabricated mold provided by an embodiment of the present invention;
[0029] Figure 2 A side view of a portion of the corrosion-resistant and high-strength magnesium-based prestressed pipe pile after being formed in a first prefabricated mold provided by an embodiment of the present invention;
[0030] Figure 3 A front view of a portion of the corrosion-resistant and high-strength magnesium-based prestressed pipe pile after being formed in a second prefabricated mold provided by an embodiment of the present invention;
[0031] Figure 4A side view of a portion of the corrosion-resistant and high-strength magnesium-based prestressed pipe pile after being formed in a second precast mold according to an embodiment of the present invention.
[0032] In the above picture:
[0033] 100-reinforcement;
[0034] 200-inner layer of the pile; 210-convex part;
[0035] 300-Outer layer of pipe pile. DETAILED DESCRIPTION
[0036] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.
[0037] The core of the present invention is to provide a corrosion-resistant and high-strength magnesium-based prestressed pipe pile with a stable structure and strong durability. Another core of the present invention is to provide a method for preparing a corrosion-resistant and high-strength magnesium-based prestressed pipe pile, which can produce a pipe pile with a stable structure and strong durability.
[0038] In order to enable those skilled in the art to better understand the technical solution provided by the present invention, the present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.
[0039] Specifically, please refer to Figure 1-Figure 4 The present invention provides a corrosion-resistant and high-strength magnesium-based prestressed pipe pile, which includes a steel bar 100, a pipe pile inner layer 200 and a pipe pile outer layer 300.
[0040] The outer layer 300 of the pipe pile is arranged on the inner layer 200 of the pipe pile, and the steel bar 100 is embedded in the inner layer 200 of the pipe pile along the length direction. The steel bar 100, the inner layer 200 of the pipe pile and the outer layer 300 of the pipe pile are a cast-integrated structure. The inner layer 200 of the pipe pile is a magnesium oxysulfate slurry layer, and the outer layer 300 of the pipe pile is a magnesium oxychloride slurry layer.
[0041] It should be noted that due to the higher requirements for the corrosion resistance of photovoltaic pipe piles in the field of photovoltaic power generation, it has been found through continuous exploration that high-strength, corrosion-resistant, and environmentally controllable magnesium oxysulfide slurry and magnesium oxychloride slurry can be used to replace traditional concrete materials. Magnesium oxysulfide slurry and magnesium oxychloride slurry belong to magnesium cementitious materials. Products made of magnesium cementitious materials have the characteristics of light weight, high strength, corrosion resistance, wear resistance, long life and good thermal insulation.
[0042] The material slurry of the magnesium oxysulfide slurry layer itself does not contain chloride ions, has no corrosive effect on the steel bar 100, and can be used as a slurry layer for wrapping the steel bar 100. In addition, the magnesium oxysulfide slurry is also compatible with the magnesium oxychloride slurry, but its compatibility with seawater is not as good as that of the magnesium oxychloride material. The material slurry of the magnesium oxychloride slurry layer contains chloride ions, which can have good compatibility with seawater, and the strength increases instead of decreasing, so it can be wrapped on the outside of the magnesium oxysulfide slurry layer. The disadvantage of the magnesium oxychloride slurry layer is that chloride ions are corrosive to the steel bar 100, so isolation from the steel bar 100 is achieved through the magnesium oxysulfide slurry layer, which can effectively ensure the strength of the steel bar 100 and prevent the steel bar 100 from being corroded.
[0043] The present invention provides a corrosion-resistant and high-strength magnesium-based prestressed pipe pile, in which a pipe pile inner layer 200 is wrapped around the outside of a steel bar 100, and a pipe pile outer layer 300 is wrapped around the outside of the pipe pile inner layer 200. The pipe pile inner layer 200 uses magnesium oxysulfide slurry, and the pipe pile outer layer 300 uses magnesium oxychloride slurry. In the field of photovoltaic power generation, especially in offshore and tidal flat areas, the chloride ions contained in the magnesium oxychloride slurry material itself in this case have good compatibility with seawater, and are suitable for the outer layer 300 of the pipe pile to contact with seawater.
[0044] Since the pipe pile has steel bars 100 inside, the magnesium oxychloride slurry material is corrosive to the steel bars 100, while the magnesium oxysulfide slurry material itself does not contain chloride ions and is compatible with the steel bars 100, and is suitable as the pipe pile inner layer 200 in contact with the steel bars 100. The steel bars 100, the pipe pile inner layer 200 and the pipe pile outer layer 300 are cast to form an integrated magnesium-based prestressed pipe pile, which has the characteristics of stable structure and strong durability.
[0045] In order to further improve the surface performance of the steel bar 100, an anti-corrosion isolation layer may be provided on the surface of the steel bar 100. The anti-corrosion isolation layer may include an anti-corrosion coating and an acid-alkali resistant coating sequentially provided on the surface of the steel bar 100 from the inside to the outside, that is, the surface of the steel bar 100 is sequentially provided with an anti-corrosion coating and an acid-alkali resistant coating from the inside to the outside. Specifically, the two layers of coating on the outside of the steel bar 100 may be applied by electroplating. First, a layer of anti-corrosion coating containing aluminum (or zinc) is electroplated on the surface of the steel bar 100 as a base layer to play an anti-corrosion function; secondly, on the basis of the base layer, a layer of acid-alkali resistant coating with components such as polymer resin, graphene (or lubricating material) is applied by a special process as a secondary coating to further improve the acid and alkali resistance. The coating provided by the above embodiment enables the surface of the steel bar 100 to have excellent adhesion, heavy corrosion resistance, and acid and alkali resistance.
[0046] In a specific embodiment, the magnesium oxychloride slurry layer includes magnesium oxide, magnesium chloride / halogen flakes, a modifier and stone particles. The modifier includes at least one of a halogen-resistant enhancer, a toughening and desolventizing agent, a defoamer and a curing agent. The stone particles, as auxiliary materials, can be in different forms such as stones, gravel or sand.
[0047] The magnesium oxysulfide slurry layer includes magnesium oxide, magnesium sulfate, a modifier, silica fume and stone particles. The modifier includes at least one of a magnesium oxysulfide modifier, a waterproofing agent, a curing agent and a defoaming agent. The stone particles, as auxiliary materials, can be in different forms such as stones, gravel or sand. Silica fume can increase strength.
[0048] In a specific embodiment, there are multiple steel bars 100, and the multiple steel bars 100 are evenly arranged along the circumference of the inner layer 200 of the pipe pile. The multiple steel bars 100 can be connected together by binding to form a cage-shaped steel bar 100 frame, which has the function of consolidating fluid and improving strength.
[0049] In order to improve the stability of the connection between the inner layer 200 of the pipe pile and the outer layer 300 of the pipe pile, the outer wall of the inner layer 200 of the pipe pile and the inner wall of the outer layer 300 of the pipe pile are matched with each other in a concave-convex manner. That is, in one form, a convex portion 210 is provided on the outer wall of the inner layer 200 of the pipe pile, and a concave portion matching with the convex portion 210 is provided on the inner wall of the outer layer 300 of the pipe pile at a relative position. In another form, a concave portion is provided on the outer wall of the inner layer 200 of the pipe pile, and a convex portion 210 matching with the concave portion is provided on the inner wall of the outer layer 300 of the pipe pile at a relative position. The convex portion 210 may be in a semicircular, trapezoidal, rectangular, triangular, etc., and the concave portion matches the convex portion 210, which is not further limited here.
[0050] Furthermore, the number of the protrusions 210 may be one or more. The plurality of protrusions 210 may be evenly arranged along the circumference of the inner layer 200 of the pipe pile.
[0051] In addition, the present invention also provides a method for preparing a corrosion-resistant and high-strength magnesium-based prestressed pipe pile, using the corrosion-resistant and high-strength magnesium-based prestressed pipe pile in the above specific embodiment, the method comprising:
[0052] Ingredients: prepare magnesium oxysulfide slurry and magnesium oxychloride slurry respectively. Magnesium oxysulfide slurry itself does not contain chloride ions, has no corrosive effect on steel bars 100, and is compatible with magnesium oxychloride slurry, but its compatibility with seawater is not as good as that of magnesium oxychloride material. Magnesium oxychloride slurry contains chloride ions, so it has good compatibility with seawater, and its strength increases instead of decreases, but its disadvantage is that chloride ions are corrosive to steel bars 100.
[0053] In the first pouring, the steel bar 100 is placed in the first precast mold, and the stirred magnesium oxysulfide slurry is injected into the first precast mold.
[0054] Tensioning and first centrifugation, tensioning the first precast mold after the first pouring, placing the tensioned first precast mold into a centrifugal device for centrifugation and demoulding, and obtaining the first precast pipe pile. Specifically, one end of the first precast mold after the first pouring is sent to a specific machine for stretching, and the tensioned first precast mold is placed in a centrifugal tank for centrifugation to ensure the density of magnesium oxysulfate cement, and reach the final setting and removable mold state, and then disassemble the upper and lower steel molds of the first precast mold to obtain the first precast pipe pile with a small outer diameter that has not been fully solidified, that is, the inner layer 200 of the pipe pile. The outer diameter of the first precast mold is smaller than that of the second precast mold.
[0055] For the second pouring, the first prefabricated pipe pile is placed in the second prefabricated mold, and the magnesium oxychloride slurry is injected into the second prefabricated mold, that is, a layer of pipe pile outer layer 300 is wrapped on the outside of the pipe pile inner layer 200 to obtain the second prefabricated pipe pile. Specifically, the first prefabricated pipe pile is placed again in the second prefabricated mold with a larger outer diameter, and the magnesium oxychloride slurry prepared in advance is poured again. After the pouring is completed, the mold is closed.
[0056] The second centrifugation is to place the second prefabricated pipe piles into the centrifugal equipment for centrifugation and demoulding to ensure the density of the magnesium oxychloride cement, and then to cure and solidify the molds to finally obtain corrosion-resistant and high-strength magnesium-based prestressed pipe piles.
[0057] It should be noted that the first prefabricated mold body can be a steel mold that is detachable from top to bottom. The lower half of the steel mold is first placed in place, and the steel bars 100 / steel cage are placed in the prefabricated position (casting cavity) of the lower half of the steel mold. Then the stirred slurry is poured, and the pouring port is not in the left and right direction, but poured from the top. The preparation process of the upper and lower steel molds can refer to the ordinary pipe pile manufacturing process. The outer diameter of the first prefabricated mold is relatively small. The first pouring step is specifically: put the steel bars 100 into the first prefabricated mold, pour the stirred magnesium oxysulfide slurry into the first prefabricated mold, and gradually fill the slurry into the model. After the pouring is completed, the other half of the steel mold is closed.
[0058] Furthermore, the outer wall of the inner layer 200 of the pipe pile and the inner wall of the outer layer 300 of the pipe pile can be matched with each other in a concave-convex manner. The internal structure of the upper mold and the lower mold of the first prefabricated mold after the mold is closed is not only a circular curved surface, but can be set as follows Figure 1 As shown, the outer surface structure formed by curing after pouring the slurry is a first prefabricated pipe pile with 3 to 6 protrusions 210, and its structure can better bond with the magnesium oxychloride slurry poured in the second prefabricated mold, such as Figure 3 As shown, the outer surface of the first preformed mold is prevented from being separated from the inner surface of the second preformed mold.
[0059] The non-metallic magnesium-based photovoltaic pipe piles provided in this solution are new pipe piles that are made by referring to the molding process of prestressed pipe piles by pre-tensioning, adjusting the proportion of inorganic gelling materials, and naturally curing or low-temperature steam curing.
[0060] In a specific embodiment, the main raw materials of the magnesium oxychloride slurry include magnesium oxide, magnesium chloride, a modifier and stone particles, and the modifier includes at least one of an anti-halogen enhancer, a toughening and desolventizing agent, a defoamer and a curing agent. The raw materials of the magnesium oxysulfide slurry include magnesium oxide, magnesium sulfate, a modifier, silica fume and stone particles, and the modifier includes at least one of a magnesium oxysulfide modifier, a waterproofing agent, a curing agent and a defoamer. Among them, the stone particles, as auxiliary materials, can be in different forms such as stones, gravel or sand.
[0061] Among them, the performance indicators of magnesium oxide need to meet the relevant provisions of "Light-burned magnesium oxide for magnesia products" (WB / T 1019-2002), see Table 1.
[0062] Table 1 Performance index of light-burned powder
[0063]
[0064] The performance indicators of magnesium chloride need to meet the relevant provisions of "Industrial Magnesium Chloride for Magnesium Products" (WB / T1018-2002), see Table 2.
[0065] Table 2 Performance index of magnesium chloride
[0066]
[0067] In the production of magnesium oxysulfide related products, the magnesium sulfate raw material used generally refers to CMMA / T 1-2015 "Magnesium Sulfate for Magnesium Cementitious Materials Products", and the specific requirements are shown in Table 3.
[0068] Table 3 Specifications of magnesium sulfate heptahydrate
[0069]
[0070] Table 4 Modifiers
[0071] model name Addition amount‰ Appearance GX-4# Halogen resistance enhancer 5-10 Dark reddish brown viscous liquid GX-5# Defoaming and color preserving agent 10 Milky white liquid GX-12# Toughening and solvent reduction 10-20 Orange liquid GX-15# Magnesium oxysulfate modifier 5~10 Green liquid GX-16# Curing agent 5~10 Pink liquid
[0072] The performance indicators of gravel are shown in Table 5.
[0073] Table 5 Performance index of stone
[0074]
[0075] The performance indicators of sand and gravel are shown in Table 6.
[0076] Table 6 Sand and gravel performance indicators
[0077]
[0078] The raw materials used for non-metallic magnesium-based photovoltaic pipe piles are different from those for traditional prestressed concrete pipe piles, so the proportion of ingredients and the order of mixing and feeding are also different.
[0079] Taking the photovoltaic pipe pile with the production specification of PHC-400-AB-11 meters as an example, the reference ratios are shown in Table 7 and Table 8. Magnesium oxide can be replaced by light-burned powder.
[0080] Table 7 Reference ratio
[0081]
[0082] Table 8 Reference Ratio
[0083]
[0084] In order to solve the problem of rust of the steel bars 100 and compatibility with seawater, the surface of the steel bars 100 is treated with anti-corrosion before the first pouring step. When the photovoltaic pipe pile uses multiple steel bars 100, the multiple steel bars 100 are tied to form a steel cage. The steel cage bundling adopts mechanized operation, which is fast and effective. After the steel cage is tied, it is placed in the first prefabricated mold with a truss crane. The specific steel cage has nuts on both ends. After being placed in the first prefabricated mold, it is fixed with a circular steel plate, and there are bolts corresponding to the nuts on the steel plate. The tensioning end looks different from the other end, and the gap in the mold is the tensioning gap. Finally, the tied steel cage is lifted to the pouring area with a truss crane.
[0085] In a specific embodiment, the anti-corrosion treatment step includes: electroplating a layer of anti-corrosion coating as a base layer on the surface of the steel bar 100, and then coating a layer of acid- and alkali-resistant coating on the base layer. First, electroplating a layer of anti-corrosion coating containing aluminum (or zinc) as a base layer on the surface of the steel bar 100 to play an anti-corrosion function; secondly, on the basis of the base layer, a layer of acid- and alkali-resistant coating with components such as polymer resin, graphene (or lubricating material) is coated by a special process as a secondary coating to further improve the acid- and alkali-resistant ability.
[0086] During preparation, the tied steel cage with surface anti-corrosion treatment is placed in the first prefabricated mold.
[0087] As shown in this application and claims, unless the context clearly indicates an exception, the words "a", "an", "a kind" and / or "the" do not refer to the singular, but also include the plural. Generally speaking, the terms "include" and "comprise" only indicate the inclusion of clearly identified steps and elements, and these steps and elements do not constitute an exclusive list. The method or device may also include other steps or elements. The elements defined by the sentence "includes a..." do not exclude the existence of other identical elements in the process, method, commodity or device that includes the elements.
[0088] In the description of the embodiments of the present application, unless otherwise specified, " / " means or, for example, A / B can mean A or B; "and / or" in this article is only a description of the association relationship of associated objects, indicating that there can be three relationships, for example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. In addition, in the description of the embodiments of the present application, "multiple" means two or more than two.
[0089] In the description of this application, unless otherwise clearly defined, terms such as setting, installing, connecting, etc. should be understood in a broad sense, and technicians in the relevant technical field can reasonably determine the specific meanings of the above terms in this application based on the specific content of the technical solution.
[0090] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.
[0091] The principles and implementation methods of the present invention are described in this article using specific examples. The description of the above embodiments is only used to help understand the method and core ideas of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. A corrosion-resistant and high-strength magnesium-based prestressed pipe pile. It is characterized in that It includes steel bars, an inner layer of a pipe pile and an outer layer of a pipe pile. The outer layer of the pipe pile is arranged on the outside of the inner layer of the pipe pile. The steel bars are embedded in the inner layer of the pipe pile along the length direction. The steel bars, the inner layer of the pipe pile and the outer layer of the pipe pile are a cast-integrated structure. The inner layer of the pipe pile is a magnesium oxysulfate slurry layer, and the outer layer of the pipe pile is a magnesium oxychloride slurry layer.
2. The corrosion-resistant and high-strength magnesium-based prestressed pipe pile according to claim 1, It is characterized in that The surface of the steel bar is provided with an anti-corrosion coating and an acid-alkali resistant coating in sequence from the inside to the outside.
3. The corrosion-resistant and high-strength magnesium-based prestressed pipe pile according to claim 1, It is characterized in that The magnesium oxychloride slurry layer comprises magnesium oxide, magnesium chloride, a modifier and stone particles, wherein the modifier comprises at least one of a halogen resistance enhancer, a toughening and solvent reducing agent, a defoaming agent and a curing agent; And / or, the magnesium oxysulfide slurry layer includes magnesium oxide, magnesium sulfate, a modifier, silica fume and stone particles, and the modifier includes at least one of a magnesium oxysulfide modifier, a waterproofing agent, a curing agent and a defoaming agent.
4. The corrosion-resistant and high-strength magnesium-based prestressed pipe pile according to claim 1, It is characterized in that The number of the steel bars is multiple, and the multiple steel bars are evenly arranged along the circumference of the inner layer of the pipe pile.
5. The corrosion-resistant and high-strength magnesium-based prestressed pipe pile according to any one of claims 1 to 4, It is characterized in that The outer wall of the inner layer of the pipe pile and the inner wall of the outer layer of the pipe pile are matched with each other in a concave-convex manner.
6. The corrosion-resistant and high-strength magnesium-based prestressed pipe pile according to claim 5, It is characterized in that A plurality of convex parts are arranged on the outer wall of the inner layer of the pipe pile, and the plurality of convex parts are evenly arranged along the circumference of the inner layer of the pipe pile.
7. A method for preparing a corrosion-resistant and high-strength magnesium-based prestressed pipe pile. It is characterized in that Using the corrosion-resistant and high-strength magnesium-based prestressed pipe pile according to any one of claims 1 to 6, the method comprises: Mixing ingredients, respectively preparing magnesium oxysulfide slurry and magnesium oxychloride slurry; In the first pouring, the steel bars are placed in the first precast mold, and the magnesium oxysulfide slurry is injected into the first precast mold; Tensioning and first centrifugation, tensioning the first prefabricated mold after the first pouring, placing the tensioned first prefabricated mold into a centrifugal device for centrifugation and demoulding, to obtain a first prefabricated pipe pile; The second pouring is to place the first prefabricated pipe pile into a second prefabricated mold, and inject the magnesium oxychloride slurry into the second prefabricated mold to obtain the second prefabricated pipe pile; The second centrifugation is performed, and the second prefabricated pipe piles are placed in a centrifugal device for centrifugation and demoulding to obtain corrosion-resistant and high-strength magnesium-based prestressed pipe piles.
8. The preparation method according to claim 7, It is characterized in that In the batching step, the raw materials of the magnesium oxychloride slurry include magnesium oxide, magnesium chloride, a modifier and stone particles, and the modifier includes at least one of a halogen-resistant enhancer, a toughening and desolvating agent, a defoaming agent and a curing agent; And / or, the raw materials of the magnesium oxysulfide slurry include magnesium oxide, magnesium sulfate, a modifier, silica fume and stone particles, and the modifier includes at least one of a magnesium oxysulfide modifier, a waterproofing agent, a curing agent and a defoaming agent.
9. The preparation method according to claim 7, It is characterized in that Before the first pouring step, the surface of the steel bar is subjected to anti-corrosion treatment.
10. The preparation method according to claim 9, It is characterized in that The anti-corrosion treatment step includes: first electroplating a layer of anti-corrosion coating as a base layer on the surface of the steel bar, and then coating a layer of acid and alkali resistant coating on the base layer.