Photocuring additive manufacturing method for converting low-shrinkage polymer into ceramic wave-absorbing material
By adding inorganic solid-phase fillers and coupling agents to the photocuring additive manufacturing technology of polymer-converted ceramics, ultraviolet aging and high-temperature annealing, the problems of low yield and large shrinkage of ceramics are solved, and high-efficiency preparation and low shrinkage are achieved The polymer-converted ceramic wave absorbing material with high yields has improved its dielectric and mechanical properties.
Patent Information
- Application Number
- CN202310584864.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-11-26
AI Technical Summary
The photocuring additive manufacturing technology of polymer-converted ceramics has problems such as low yield, large linear shrinkage and limited wave absorption performance, which limits its application in the field of wave absorption materials.
By mixing the ceramic precursor with a photosensitive resin and a photoinitiator, adding inorganic solid-phase filler and coupling agent, using photocuring additive manufacturing technology to print and prepare polymer-converted ceramic green body, and performing ultraviolet aging, heating aging and high-temperature annealing , a low shrinkage rate polymer-converted ceramic wave absorbing material was obtained.
Achieve high ceramic yield and low shrinkage, improve dielectric performance, especially the minimum reflection loss in the frequency range of 8 to 18GHz can reach -48.61dB, and the effective absorption bandwidth less than -10dB can reach 4.30GHz, which enhances the Mechanical properties of materials.
Smart Images

Figure CN119019174A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of additive manufacturing of polymer-converted ceramics, and in particular relates to a photocuring additive manufacturing method for a low-shrinkage polymer-converted ceramic wave-absorbing material. Background Art
[0002] Polymer-converted ceramic materials have the advantages of excellent high temperature resistance, corrosion resistance, light weight and adjustable dielectric properties, and are emerging microwave absorbing materials in recent years. Polymer-converted ceramics can be prepared in the form of organic liquids. This pure liquid preparation method has great advantages in the photocuring additive manufacturing method (relative to the photosensitive suspension of ceramic powder), such as avoiding the problems of light scattering and powder sedimentation of the ceramic suspension during the printing process, and has high fidelity. Therefore, the photocuring additive manufacturing technology of polymer-converted ceramics is suitable for the preparation of absorbing materials with complex geometric structures.
[0003] At present, the main photocuring additive manufacturing technologies for polymer-converted ceramics include stereolithography additive manufacturing technology and digital light processing additive manufacturing technology. To ensure the photocuring effect, there must generally be enough photosensitive groups in the ceramic precursor. However, the photosensitive groups will decompose and release a large amount of gas during the heat treatment process, which will increase the volume shrinkage and mass loss. Large shrinkage will cause internal stress in the parts, resulting in significant deformation of the ceramic products and macro cracks and defects. In addition, the presence of photosensitive groups also limits the way to adjust the dielectric properties of ceramics by designing the molecular structure of the precursor.
[0004] Therefore, on the whole, the current photocuring additive manufacturing technology of polymer-converted ceramics still has problems such as low ceramic yield, large linear shrinkage and limited absorbing performance, which limits the application of photocuring additive manufacturing technology in the field of polymer-converted ceramic absorbing materials. Summary of the invention
[0005] In view of the above problems existing in the prior art, the present invention aims to provide a photocuring additive manufacturing method for a polymer-converted ceramic absorbing material with low shrinkage and high ceramic yield.
[0006] Specifically, in a first aspect, the present invention provides a method for photocuring additive manufacturing of a low shrinkage polymer-converted ceramic absorbing material, comprising: The ceramic precursor is mixed with a photosensitive resin and a photoinitiator to obtain a photosensitive ceramic precursor, and then an inorganic solid phase filler and a coupling agent are added to the photosensitive ceramic precursor to obtain a photosensitive ceramic precursor slurry; The polymer-converted ceramic green body is prepared by printing with photosensitive ceramic precursor slurry as raw material through photocuring additive manufacturing technology; the polymer-converted ceramic green body is subjected to ultraviolet light aging, heat aging, and then pyrolysis and high-temperature annealing to obtain the low-shrinkage polymer-converted ceramic absorbing material.
[0007] Preferably, the ceramic precursor is at least one of 3-(methacryloyloxy)propyltrimethoxysilane, polymethylsiloxane, vinylsiloxane, polymethylphenylsiloxane, polycarbosilane, and polysilazane; The photosensitive resin is at least one of 1,6-hexanediol diacrylate, bifunctional aliphatic polyurethane acrylate, acryloyl morpholine, tripropylene glycol diacrylate, and trimethylolpropane triacrylate; The photoinitiator is 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 4-phenylbenzophenone or 1-hydroxy-cyclohexylbenzophenone.
[0008] Preferably, in the photosensitive ceramic precursor, based on the total mass of the ceramic precursor and the photosensitive resin as 100%, the mass fraction of the ceramic precursor is 60-73%, and the mass fraction of the photosensitive resin is 40-27%; the mass of the photoinitiator in the photosensitive ceramic precursor is 1-3% of the mass of the photosensitive resin.
[0009] Preferably, the inorganic solid filler is at least one of silicon dioxide, aluminum oxide, silicon carbide, silicon nitride, and aluminum nitride; The coupling agent is titanium isopropoxide, tetrabutyl titanate or tetraisopropyl di(dioctylphosphite) titanate.
[0010] Preferably, the volume fraction of the inorganic solid filler in the photosensitive ceramic precursor slurry is 35-50 vol%; the mass of the coupling agent is 0.5-3 wt% of the mass of the photosensitive ceramic precursor.
[0011] Preferably, the light source used in the photocuring additive manufacturing technology is ultraviolet light with a wavelength of 320 to 410 nm and a light source power of 4 to 100 mW / cm 2 , single layer exposure power is set to 5~50mW / cm 2 , the exposure time of a single layer is 2 to 15 seconds.
[0012] Preferably, the light source used for the ultraviolet aging is ultraviolet light with a wavelength of 405 to 410 nm, the light source power is 10 to 85 W, and the ultraviolet aging time is 10 to 60 min; The heating aging temperature is 100-200° C., the heating and cooling rates are 0.5-2° C. / min; the heating aging time is 60-150 min; the heating aging environment atmosphere is air, nitrogen, argon or vacuum.
[0013] Preferably, the pyrolysis temperature is 800-1000°C; the pyrolysis heating and cooling rates are 0.5-3°C / min; and the insulation time is 0-2h.
[0014] Preferably, the high temperature annealing temperature is 1100-1500° C.; the heating and cooling rates are 0.5-5° C. / min; and the holding time is 0-3 h.
[0015] In a second aspect, the present invention provides a low shrinkage polymer-converted ceramic absorbing material obtained according to the above manufacturing method.
[0016] Beneficial Effects (1) The inorganic solid phase filler added to the photosensitive ceramic precursor of the present invention can increase the single-layer solidification thickness and improve the printing efficiency; (2) The inorganic solid filler used in the present invention as the skeleton structure inhibits the shrinkage of the ceramic precursor during the pyrolysis process. The smaller shrinkage allows the polymer-converted ceramic to produce microporous channels for gas release, reducing the possibility of macro cracks in the ceramic product and increasing the ceramic yield. The linear shrinkage of the polymer-converted ceramic obtained can reach 5.7%, and the ceramic yield can reach 80.8%; (3) The addition of inorganic solid fillers in the present invention adjusts the dielectric properties of the polymer-converted ceramics, and the minimum reflection loss in the frequency range of 8 to 18 GHz can reach -48.61 dB, and the effective absorption bandwidth less than -10 dB can reach 4.30 GHz; (4) The present invention uses inorganic solid phase fillers as particle reinforcement phases to improve the mechanical properties of polymer-converted ceramic green bodies. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 The process flow chart of the photocuring additive manufacturing method of the polymer-converted ceramic absorbing material exemplified in the present invention; Figure 2 The actual picture of the green body and polymer-converted SiOC ceramic with complex geometric structure prepared in Example 1 of the present invention; Figure 3 This is a reflection loss curve of the polymer-converted SiOC ceramic prepared in Example 2 of the present invention; Figure 4 The real part (ε') and imaginary part (ε") of the complex dielectric constant of the polymer-converted SiOC ceramics prepared in Examples 1-3 of the present invention; Figure 5 The actual picture of the green body and polymer-converted SiOC ceramic with complex geometric structure obtained in Comparative Example 1 of the present invention; Figure 6 This is a physical picture of the polymer-converted ceramic obtained in Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0018] The present invention is further described by way of embodiments. It should be understood that the following embodiments are only used to illustrate the present invention, rather than to limit the present invention.
[0019] The following combination Figure 1 , exemplarily illustrating the method for photocuring additive manufacturing of low shrinkage polymer-converted ceramic absorbing materials reinforced with inorganic solid phase fillers provided by the present invention. The method for photocuring additive manufacturing of low shrinkage polymer-converted ceramic absorbing materials may include the following steps.
[0020] (1) Preparation of photosensitive ceramic precursor: The ceramic precursor, photosensitive resin and photoinitiator are mechanically stirred and blended to obtain a uniformly mixed photosensitive ceramic precursor.
[0021] In some embodiments, the ceramic precursor may be at least one of 3-(methacryloxy)propyltrimethoxysilane, polymethylsiloxane, vinylsiloxane, polymethylphenylsiloxane, polycarbosilane, and polysilazane.
[0022] The ceramic precursor can be added in the form of a solution. As a preferred example, polymethylphenylsiloxane is stirred and dissolved in a solvent at 30-50° C., and then vinyl siloxane and a solubilizing agent hexafunctional silicone polyurethane acrylate are added thereto to obtain a ceramic precursor solution.
[0023] Preferably, based on the total mass of polymethylphenylsiloxane and vinylsiloxane as 100%, the mass fraction of polymethylphenylsiloxane in the precursor solution can be controlled to be 30-60%, and the mass fraction of vinylsiloxane can be controlled to be 70-40%.
[0024] Preferably, the content of the hexafunctional silicone polyurethane acrylate can be controlled to be 8-9% of the mass of the vinyl siloxane, and it acts as a solubilizer for the vinyl siloxane to improve the solubility of the vinyl siloxane.
[0025] Preferably, the solvent may be tetrahydrofuran, acetone or tripropylene glycol methyl ether. The mass ratio of the solvent to polymethylphenylsiloxane may be controlled to be 1:(2-2.5) to obtain a precursor solution with moderate viscosity and good compatibility with the photosensitive resin.
[0026] In some embodiments, the photosensitive resin may be at least one of 1,6-hexanediol diacrylate, difunctional aliphatic polyurethane acrylate, acryloyl morpholine, tripropylene glycol diacrylate, and trimethylolpropane triacrylate. In a preferred example, the photosensitive resin may be a mixture of 1,6-hexanediol diacrylate, trimethylolpropane triacrylate, and difunctional aliphatic polyurethane acrylate; wherein, based on the total mass of the three being 100%, the mass fraction of 1,6-hexanediol diacrylate may be 50-70%, the mass fraction of trimethylolpropane triacrylate may be 15-25%, and the mass fraction of difunctional aliphatic polyurethane acrylate may be 15-25%, so as to obtain a photosensitive resin with lower viscosity and faster photocuring speed.
[0027] In some embodiments, the photoinitiator may be 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 4-phenylbenzophenone or 1-hydroxy-cyclohexylbenzophenone.
[0028] In some embodiments, in the photosensitive ceramic precursor, the mass fraction of the ceramic precursor can be 60-73%, and the mass fraction of the photosensitive resin can be 40-27%, based on the total mass of the ceramic precursor and the photosensitive resin as 100%. Among them, the content of the ceramic precursor affects the final ceramic yield of the photosensitive ceramic precursor, and the content of the photosensitive resin affects the photocuring performance of the photosensitive ceramic precursor. By controlling the mass ratio of the ceramic precursor to the photosensitive resin within the above range, the photocuring effect of the photosensitive ceramic precursor can be achieved while having a higher ceramic yield.
[0029] In some embodiments, the mass of the photoinitiator in the photosensitive ceramic precursor can be controlled to be 1-3% of the mass of the photosensitive resin. The photoinitiator provides sufficient free radicals for the photosensitive ceramic precursor under the action of ultraviolet light, thereby initiating a polymerization reaction.
[0030] (2) Preparation of photosensitive ceramic precursor slurry: Inorganic solid fillers and coupling agents are added to the photosensitive ceramic precursor and mixed thoroughly, and then bubbles are removed under vacuum to obtain a uniformly dispersed photosensitive ceramic precursor slurry.
[0031] In some embodiments, the inorganic solid filler may be at least one of silicon dioxide, aluminum oxide, silicon carbide, silicon nitride, and aluminum nitride; and the particle size of the inorganic solid filler may be 15 to 30 microns.
[0032] In some embodiments, the coupling agent may be titanium isopropoxide, tetrabutyl titanate or tetraisopropyl di(dioctylphosphite) titanate. The addition of the coupling agent may improve the dispersibility of the inorganic solid phase filler in the photosensitive ceramic precursor to reduce the viscosity of the photosensitive ceramic precursor slurry.
[0033] In some embodiments, the volume fraction of the inorganic solid filler in the photosensitive ceramic precursor slurry can be controlled to be 35-50 vol%. If the volume content of the inorganic solid filler is less than 35 vol%, it will result in the inability to form a complete skeleton structure during the subsequent pyrolysis process, causing the ceramic to crack; if the volume content of the inorganic solid filler is greater than 50 vol%, the viscosity of the obtained photosensitive ceramic precursor slurry will be too high, and a polymer-converted ceramic green body with high printing quality cannot be obtained subsequently.
[0034] In some embodiments, the mass of the coupling agent can be controlled to be 0.5-3wt% of the mass of the photosensitive ceramic precursor. An appropriate amount of coupling agent can form molecular bridges on the surface of the solid phase filler to avoid collisions between particles and stabilize the particle suspension, but an excessive amount of coupling agent will bridge the solid phase particles, making the stability and dispersibility of the system worse.
[0035] (3) Preparation of polymer-converted ceramic green bodies. Using photosensitive ceramic precursor slurry as raw material, polymer-converted ceramic green bodies are prepared by printing using photocuring additive manufacturing technology.
[0036] In some embodiments, the light source used in the photocuring additive manufacturing technology can be ultraviolet light with a wavelength of 320 to 410 nm, and the light source power can be 4 to 100 mW / cm 2 , single layer exposure power is set to 5~50mW / cm 2 The exposure time of a single layer can be 2 to 15 seconds. Overexposure will cause the printed shape to be distorted, and underexposure will cause the photosensitive ceramic precursor slurry to fail to solidify effectively, resulting in printing failure.
[0037] The inorganic solid phase filler used in the present invention can increase the thickness of a single layer of solidification and improve printing efficiency, and can also be used as a particle reinforcement phase to improve the mechanical properties of the polymer-converted ceramic green body.
[0038] (4) Aging. The polymer-converted ceramic green body prepared by photo-curing additive manufacturing printing was first subjected to UV aging and then to heat aging.
[0039] In some embodiments, the light source used for the ultraviolet aging can be ultraviolet light with a wavelength of 405 to 410 nm, the light source power can be 10 to 85 W, preferably 20 W, and the ultraviolet aging time can be 10 to 60 minutes. The degree of polymerization of the photosensitive resin can be increased by ultraviolet aging, thereby improving the mechanical strength of the polymer-converted ceramic green body.
[0040] In some embodiments, the heating aging temperature may be 100-200°C, the heating and cooling rates may be 0.5-2°C / min, preferably 0.5°C / min; the heating aging time may be 60-150min; the heating aging environment atmosphere may be air, nitrogen, argon or vacuum. The heating aging may promote the crosslinking degree of the ceramic precursor, and a higher crosslinking polymerization degree may reduce the gas release during the pyrolysis process, thereby reducing the formation of cracks and pores.
[0041] (5) Pyrolysis. The aged polymer-converted ceramic green body is pyrolyzed in a vacuum environment. The organic polymer-converted ceramic green body can be converted from an organic polymer to an inorganic ceramic by pyrolysis, and the vacuum atmosphere is conducive to the escape of gas.
[0042] In some embodiments, the pyrolysis temperature can be 800-1000°C, preferably 900°C; the pyrolysis heating and cooling rates can be 0.5-3°C / min, preferably 1°C / min. Faster heating and cooling rates will cause uneven heating of the polymer-converted ceramic green body, resulting in internal stress and causing deformation or cracking of the body; the holding time can be 0-2h, preferably 0.5h, to ensure complete ceramic conversion.
[0043] During the pyrolysis process, the inorganic solid phase filler used in the present invention can reduce the shrinkage of ceramics, so that the final polymer-converted ceramic material has a lower shrinkage rate.
[0044] (6) High temperature annealing. The amorphous polymer-converted ceramic obtained after high temperature pyrolysis is subjected to high temperature annealing in an inert atmosphere or vacuum conditions to obtain a polymer-converted ceramic. The high temperature annealing can form ceramic nanocrystals inside the amorphous ceramic obtained by pyrolysis, and further sinter the inorganic solid phase filler to enhance the dielectric properties of the ceramic.
[0045] In some embodiments, the high temperature annealing temperature can be 1100-1500°C, the heating and cooling rates can be 0.5-5°C / min, and the insulation time can be 0-3h; preferably, the annealing temperature is 1300°C, the heating and cooling rates are 2°C / min, and the insulation time is 1.5h.
[0046] Wherein, the inert atmosphere for the high temperature annealing may be argon or nitrogen.
[0047] The preparation method provided by the present invention realizes the rapid integrated manufacturing of polymer-converted ceramic absorbing materials with low shrinkage, high ceramic yield and adjustable dielectric properties. After the inorganic solid-phase filler is mixed with the liquid ceramic precursor, it is directly photocured and formed in one time. In the subsequent pyrolysis process, the ceramic precursor will release gas and shrink. Among them, the inorganic solid-phase filler acts as a "skeleton" structure to inhibit the shrinkage of the ceramic precursor during the pyrolysis process, and produces microporous channels for gas release, ultimately reducing the possibility of macro cracks in the ceramic product and improving the ceramic yield. At the same time, the addition of the inorganic solid-phase filler can also play a role in adjusting the dielectric constant of the final polymer-converted ceramic. Compared with other methods for preparing polymer-converted ceramic absorbing materials, the present invention has the advantages of short molding time, high molding accuracy and moldless manufacturing, and can realize the integrated molding of parts with complex geometric structures in a relatively short time.
[0048] The linear shrinkage of the polymer-converted ceramics obtained by the preparation method provided by the present invention can reach 5.7%, the ceramic yield can reach 80.8%, the minimum reflection loss in the frequency range of 8 to 18 GHz can reach -48.61 dB, and the effective absorption bandwidth less than -10 dB can reach 4.30 GHz.
[0049] The following examples are further listed to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are only examples in a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values exemplified below.
[0050] Example 1
[0051] (1) 18.9 g of 1,6-hexanediol diacrylate, 6.3 g of trimethylolpropane triacrylate, and 6.3 g of difunctional aliphatic polyurethane acrylate were stirred and mixed to obtain a photosensitive resin; 17.34 g of polymethylphenylsiloxane was stirred and dissolved in 8.67 g of tripropylene glycol methyl ether at 40° C., and then 39 g of vinyl siloxane, 3.5 g of hexafunctional silicone polyurethane acrylate, 31.5 g of the above photosensitive resin and 0.7 g of photoinitiator 2,4,6-trimethylbenzoyl-diphenylphosphine oxide were added thereto, and the mixture was stirred and mixed in a homogenizer for 5 minutes to obtain a uniformly mixed photosensitive ceramic precursor.
[0052] (2) Add 137.4 g of silicon dioxide with a particle size of 25 μm and 1.5 g of tetrabutyl titanate coupling agent to the photosensitive ceramic precursor, then ball mill in a high-energy ball mill for 10 min, and then degas in a vacuum environment for 3 min to obtain a uniformly dispersed photosensitive ceramic precursor slurry. The volume fraction of the inorganic solid filler in the photosensitive ceramic precursor slurry is 35 vol%; the mass of the coupling agent is 1.5 wt% of the mass of the photosensitive ceramic precursor.
[0053] (3) Printing the photosensitive ceramic precursor slurry with a digital light processing 3D printer to prepare a polymer-converted ceramic green body. The light source used in the photocuring additive manufacturing technology is ultraviolet light with a wavelength of 405nm and a light source power of 4 to 100mW / cm 2 , single layer exposure power is set to 20mW / cm 2 , the exposure time for a single layer is 4s.
[0054] (4) The polymer-converted ceramic green body was first aged for 30 min under a UV lamp with a wavelength of 405 nm and a light source power of 20 W, and then transferred to a tubular furnace for heating aging at 170°C (heating and cooling rates of 0.5°C / min) in argon for 150 min.
[0055] (5) The aged polymer-converted ceramic green body is placed in a graphite crucible and put into a high-temperature sintering furnace for pyrolysis in a vacuum. The pyrolysis temperature is 900° C., the heating and cooling rates are 1° C. / min, and the holding time is 0.5 h.
[0056] (6) The amorphous polymer-converted ceramic obtained after high-temperature pyrolysis is subjected to high-temperature annealing in an argon atmosphere to obtain a polymer-converted ceramic. The annealing temperature is 1300°C, the heating and cooling rates are 2°C / min, and the holding time is 1.5h.
[0057] Figure 2 The green body and polymer-converted SiOC ceramics with complex geometric structures prepared in Example 1 of the present invention are real pictures. It can be seen from the figure that the shape of the polymer-converted SiOC ceramics finally prepared remains intact, the geometric structure does not collapse or deform, and the shrinkage rate is also small.
[0058] The shrinkage rate of the polymer-converted SiOC ceramic prepared in this Example 1 is 7.8%, the ceramic yield is 77.2%, the average real part of the dielectric constant in the frequency range of 8 to 18 GHz is 21.4, the average imaginary part of the dielectric constant is 7.7, the minimum reflection loss in the frequency range of 8 to 18 GHz is -46.21 dB, and the effective absorption bandwidth less than -10 dB is 2.31 GHz.
[0059] Example 2
[0060] The preparation process of Example 2 is similar to that of Example 1, with the main difference being that 170 g of silicon dioxide is added in step (2), and the volume fraction of the inorganic solid filler in the photosensitive ceramic precursor slurry is 40 vol%.
[0061] Figure 3 This is a reflection loss curve of the polymer-converted SiOC ceramic prepared in Example 2 of the present invention. It can be seen from the figure that the prepared polymer-converted SiOC ceramic can achieve effective electromagnetic wave absorption in the frequency range of 8 to 18 GHz at a thickness of 1.1 to 1.78 mm.
[0062] The shrinkage rate of the polymer-converted SiOC ceramic prepared in this Example 2 is 6.5%, the ceramic yield is 79.6%, the average real part of the dielectric constant in the frequency range of 8 to 18 GHz is 18.8, the average imaginary part of the dielectric constant is 6.3, the minimum reflection loss in the frequency range of 8 to 18 GHz is -48.61 dB, and the effective absorption bandwidth less than -10 dB is 3.18 GHz.
[0063] Example 3
[0064] The preparation process of this Example 3 refers to that of Example 1, with the main difference being that 208.7 g of silicon dioxide is added in step (2), and the volume fraction of the inorganic solid filler in the photosensitive ceramic precursor slurry is 45 vol%.
[0065] Figure 4 The real part (ε') and the imaginary part (ε") of the complex dielectric constant of the polymer-converted SiOC ceramics prepared in Examples 1-3 of the present invention are shown in the figure. As can be seen from the figure, from Example 1 to Example 3, with the increase of the content of the inorganic solid phase filler, the real part and the imaginary part of the complex dielectric constant of the polymer-converted SiOC ceramics are reduced, indicating that the inorganic solid phase filler can adjust the dielectric properties of the obtained polymer-converted SiOC ceramics.
[0066] The shrinkage rate of the polymer-converted SiOC ceramic prepared in this Example 3 is 5.7%, the ceramic yield is 80.8%, the average real part of the dielectric constant in the frequency range of 8 to 18 GHz is 16.1, the average imaginary part of the dielectric constant is 4.6, the minimum reflection loss in the frequency range of 8 to 18 GHz is -48.26 dB, and the effective absorption bandwidth less than -10 dB is 4.30 GHz.
[0067] Comparative Example 1
[0068] The preparation process of this comparative example 1 refers to that of Example 1, with the main difference being that no silicon dioxide micron powder is added in step (2).
[0069] Figure 5The green body and polymer-converted SiOC ceramics with complex geometric structures obtained in Comparative Example 1 of the present invention are real pictures. It can be seen from the figure that the polymer-converted SiOC ceramics obtained without adding silica inorganic filler can still maintain an intact structure, but its volume shrinkage is large and the probability of cracks occurring during pyrolysis is high.
[0070] The shrinkage rate of the polymer-converted ceramics prepared in this comparative example is 34.5%, and the ceramic yield is only 53.5%.
[0071] Comparative Example 2
[0072] The preparation process of this comparative example 2 refers to that of example 1, with the main difference being that 109.5 g of silicon dioxide is added in step (2), and the volume fraction of the inorganic solid phase filler in the photosensitive ceramic precursor slurry is 30 vol%.
[0073] Figure 6 This is a photo of the polymer-converted ceramic obtained in comparative example 2 of the present invention. As can be seen from the figure, due to the low content of filler, the polymer-converted ceramic has obvious cracks.
[0074] Comparative Example 3
[0075] The preparation process of this comparative example 3 refers to that of Example 1, with the main difference being that 255 g of silicon dioxide is added in step (2), resulting in the volume fraction of the inorganic solid phase filler in the photosensitive ceramic precursor slurry being greater than 50 vol%.
[0076] Due to the high solid content, the viscosity of the photosensitive ceramic precursor slurry obtained in this comparative example is too high, and it is impossible to print high-quality polymer-converted ceramic green bodies.
[0077] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as a limitation of the present invention. After reading the above content, it will be apparent to those skilled in the art that various modifications and substitutions of the present invention will occur. Therefore, the protection scope of the present invention should be limited by the appended claims.
Claims
1. A method for photocuring additive manufacturing of low shrinkage polymer-converted ceramic absorbing materials, characterized in that: include: The ceramic precursor is mixed with a photosensitive resin and a photoinitiator to obtain a photosensitive ceramic precursor, and then an inorganic solid phase filler and a coupling agent are added to the photosensitive ceramic precursor to obtain a photosensitive ceramic precursor slurry; Using photosensitive ceramic precursor slurry as raw material, polymer-converted ceramic green body is prepared by printing through photocuring additive manufacturing technology; The polymer-converted ceramic green body is subjected to ultraviolet aging, heat aging, pyrolysis and high-temperature annealing to obtain the low-shrinkage polymer-converted ceramic absorbing material.
2. The manufacturing method according to claim 1, characterized in that: The ceramic precursor is at least one of 3-(methacryloyloxy)propyltrimethoxysilane, polymethylsiloxane, vinylsiloxane, polymethylphenylsiloxane, polycarbosilane, and polysilazane; The photosensitive resin is at least one of 1,6-hexanediol diacrylate, bifunctional aliphatic polyurethane acrylate, acryloyl morpholine, tripropylene glycol diacrylate, and trimethylolpropane triacrylate; The photoinitiator is 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 4-phenylbenzophenone or 1-hydroxy-cyclohexylbenzophenone.
3. The manufacturing method according to claim 1 or 2, characterized in that: In the photosensitive ceramic precursor, taking the total mass of the ceramic precursor and the photosensitive resin as 100%, the mass fraction of the ceramic precursor is 60-73%, and the mass fraction of the photosensitive resin is 40-27%; the mass of the photoinitiator in the photosensitive ceramic precursor is 1-3% of the mass of the photosensitive resin.
4. The manufacturing method according to any one of claims 1 to 3, characterized in that: The inorganic solid phase filler is at least one of silicon dioxide, aluminum oxide, silicon carbide, silicon nitride, and aluminum nitride; The coupling agent is titanium isopropoxide, tetrabutyl titanate or tetraisopropyl di(dioctylphosphite) titanate.
5. The manufacturing method according to any one of claims 1 to 4, characterized in that: The volume fraction of the inorganic solid filler in the photosensitive ceramic precursor slurry is 35-50 vol%; the mass of the coupling agent is 0.5-3 wt% of the mass of the photosensitive ceramic precursor.
6. The manufacturing method according to any one of claims 1 to 5, characterized in that: The light source used in the photocuring additive manufacturing technology is ultraviolet light with a wavelength of 320 to 410 nm and a light source power of 4 to 100 mW / cm 2 , single layer exposure power is set to 5~50mW / cm 2 , the exposure time of a single layer is 2 to 15 seconds.
7. The manufacturing method according to any one of claims 1 to 6, characterized in that: The light source used for the ultraviolet aging is ultraviolet light with a wavelength of 405 to 410 nm, the light source power is 10 to 85 W, and the ultraviolet aging time is 10 to 60 min; The heating aging temperature is 100-200° C., the heating and cooling rates are 0.5-2° C. / min; the heating aging time is 60-150 min; the heating aging environment atmosphere is air, nitrogen, argon or vacuum.
8. The manufacturing method according to any one of claims 1 to 7, characterized in that: The pyrolysis temperature is 800-1000° C.; the pyrolysis heating and cooling rates are 0.5-3° C. / min; and the heat preservation time is 0-2h.
9. The manufacturing method according to any one of claims 1 to 8, characterized in that: The temperature of the high temperature annealing is 1100-1500° C.; the heating and cooling rates are 0.5-5° C. / min; and the heat preservation time is 0-3h.
10. A low shrinkage polymer-converted ceramic absorbing material obtained by the manufacturing method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method of SiOC radar type wave-absorbing material
CN111362702A
Ceramic precursor slurry and 3D printing reaction forming method of porous ceramic part
CN111548137A
Photocuring 3D printing manufacturing method of aluminum oxide-based ceramic core
CN112537948A
Pre-ceramic 3D printed monomer and polymer formulations
CN115667181A
Photocurable mixture for the manufacture of ceramic products by stereolithography with high-temperature post-processing